A modified phenolic resin for photoresist and its preparation method and application
Increasing the glass transition temperature of phenolic resin through grading and grafting technology solves the problem of insufficient heat resistance and etching resistance, achieving a higher glass transition temperature and improved photoresist performance, avoiding patterning Deformation and etching quality degradation.
Patent Information
- Application Number
- CN202211726912.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The glass transition temperature of the novolac resin is too low, resulting in insufficient heat resistance and etching resistance, which affects the development and etching process of the photoresist. When the molecular weight of the phenolic resin is too high, the solubility is reduced, resulting in insufficient adhesion and affecting pattern transfer. quality.
By classifying the phenolic resin, the high molecular weight part is retained and the poly-para-hydroxystyrene polymer is grafted on the low molecular weight part to form a modified phenolic resin, and atom transfer radical polymerization technology is used to control its glass transition temperature.
It improves the heat resistance and etching resistance of phenolic resin, avoids overexposure and pattern deformation, and improves the resolution and sensitivity of photoresist without affecting its resolution and sensitivity after compounding.
Smart Images

Figure CN115975137B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photoresist microelectronic chemistry, and in particular to a method for controlling the glass transition temperature of phenolic resin used in photoresist. Background Art
[0002] Photoresist is the core consumable material for integrated circuit manufacturing and is also a key factor affecting the performance, yield and reliability of integrated circuits. According to the chemical reaction mechanism and development principle of photoresist, photoresist can be divided into positive photoresist and negative photoresist. The exposed area of positive photoresist will undergo photolysis reaction, causing the photoresist to degrade into substances that can be dissolved in the developer. The exposed area of negative photoresist will undergo cross-linking reaction and cannot be dissolved in the developer, while the non-exposed area can be dissolved in the developer.
[0003] G / I line photoresist uses linear phenolic resin as the main resin and diazonaphthoquinone as the photosensitizer. The pattern of the mask is transferred and copied to the wafer through photolithography procedures such as exposure and development. If the molecular weight of linear phenolic resin is too low, the glass transition temperature of phenolic resin will be low, and the heat resistance and etching resistance will be reduced accordingly. Photoresist with low glass transition temperature is prone to overexposure and rounded corners during the development process. At the same time, in all processes involving heating, the temperature range needs to be strictly controlled. Some processes that require high temperature cannot be carried out. However, if the molecular weight of phenolic resin is too high, the solubility of phenolic resin in solvents and developers will be greatly reduced, and even development will not be possible. Therefore, there is a reasonable molecular weight range for phenolic resin in photoresist. In addition, the adhesion of phenolic resin to the substrate, especially the silicon substrate, is a very important parameter for photoresist. If the substrate adhesion is insufficient, it will be difficult for the photoresist to evenly cover the entire substrate surface during the coating process, and wrinkles will appear in the photoresist during the pre-baking process. During the development process, the photoresist may have insufficient adhesion, which may cause pattern deformation and photoresist peeling.
[0004] The ultimate purpose of photoresist is to transfer patterns, which means it must go through a dry or wet etching process, so the etching resistance of the photoresist must be considered. However, the etching resistance of general linear phenolic resins is insufficient, and they deform or collapse during the etching process, which ultimately affects the quality of the etched pattern.
[0005] In the field of photoresists, researchers have found that poly(p-hydroxystyrene) polymers have a very high glass transition temperature and excellent anti-etching properties. Their glass transition temperature is generally between 150 and 180°C, which is much higher than the linear phenolic resin used in i-line photoresists. Therefore, they are used as mainstream photoresist resins in 248nm photoresists. In addition, the main factor leading to the low glass transition temperature of linear phenolic resins is that they contain a lower molecular weight portion. The phenolic resin that removes the low molecular weight portion through classification has a glass transition temperature between 120 and 150°C. However, the low molecular weight portion of the phenolic resin with a high glass transition temperature obtained through classification is not fully utilized, and the utilization rate of the phenolic resin is low. At the same time, due to the lack of the low molecular weight portion, problems such as long development time may occur. Summary of the invention
[0006] The purpose of the present invention is to provide a modified phenolic resin for photoresist, so as to achieve a controllable glass transition temperature of the phenolic resin and improve the heat resistance and etching resistance of the phenolic resin.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] The modified phenolic resin is a mixed resin, comprising phenolic resins of formula I and formula II. Formula I and formula II are respectively the high molecular weight part and the low molecular weight part after phenolic resin classification, and formula II represents the structure after the polymer of formula III is introduced into the low molecular weight phenolic resin by controlled polymerization. In formula I, R represents H or CH3, R1 has the structure of formula III, m, n, and x are integers, and n>m, 5≤x≤30.
[0009]
[0010] Preferably, the modified phenolic resin is obtained by blending the phenolic resins of formula I and II. The polymer of formula III is covalently bonded to the phenolic resin of formula II, not simply blended.
[0011] Preferably, the molecular weight range of formula I is 2000-30000 g / mol; the molecular weight is the weight average molecular weight, obtained by GPC test based on polystyrene standards; the molecular weight range of formula II is 500-8000 g / mol, calculated by the homopolymer molecular weight and polymerization time curve under the same reaction conditions and the nuclear magnetic resonance hydrogen spectrum.
[0012] Preferably, the molecular weight range of formula I is 16000-20000 g / mol; the molecular weight range of formula II is 600-3600 g / mol.
[0013] Preferably, 3≤m≤200.
[0014] A method for preparing a modified phenolic resin for photoresist comprises the following steps:
[0015] (1) Add a phenolic compound and a catalyst to a reactor, introduce nitrogen gas under stirring, add formaldehyde after replacing the gas, heat to 100±10° C. and reflux for 3±1h; after the reaction, heat to 150±10° C. and distill at atmospheric pressure for 1±0.5h, then heat to 210±10° C. and distill under vacuum for 30±10min, cool and collect the solid to obtain phenolic resin I;
[0016] (2) dissolving phenolic resin I in methanol to form a 10±5 wt% solution, slowly adding water under stirring until a large amount of solid precipitates, separating the solid to obtain phenolic resin II, i.e., structure of formula I; after the solution is separated, evaporating the solvent, and collecting the residual solid phenolic resin III.
[0017] (3) dissolving phenolic resin III and a catalyst in an appropriate solvent, slowly adding bromoisobutyl bromide dropwise, continuing the reaction after the addition is complete, settling the reaction solution in water, filtering, collecting the solid, dissolving and settling for several times, and drying to obtain phenolic resin IV;
[0018] (4) Mix and dissolve phenolic resin IV, 4-acetoxystyrene and solvent uniformly, add catalyst and ligand, introduce nitrogen to replace air under stirring, seal, react at 90±10° C. for 6±2 h, cool, pass the reaction solution through a neutral alumina column, and settle in water; collect solid after dissolving and settling several times to obtain phenolic resin V, dissolve phenolic resin V in methanol, slowly add strong base, reflux for 6±2 h, and cool, neutralize the reaction solution with acid, and settle in water, dissolve and settle several times, and collect solid to obtain phenolic resin VI, i.e., structure of formula II;
[0019] (5) The phenolic resin II and the phenolic resin VI are mixed evenly, and heated and dried to obtain a modified phenolic resin for photoresist.
[0020] Preferably, the phenolic compound in step (1) includes one or more of m-cresol, p-cresol, o-cresol, hydroquinone, pyrogallol and phenol; and the catalyst is one or more of sodium hydroxide, potassium hydroxide, triethylamine, hydrochloric acid, sulfuric acid and oxalic acid.
[0021] Preferably, the volume ratio of water added in step (2) to methanol is 1.0±0.2; and the catalyst in step (3) is one of triethylamine, pyridine and dimethylaminopyridine.
[0022] Preferably, the catalyst in step (4) is a halogenated low-valent metal such as cuprous bromide, cuprous chloride, ferric dibromide, etc., the solvent is tetrahydrofuran, 1,4-dioxane, acetone, and the ligand is bipyridine or PMDETA.
[0023] The modified phenolic resin for photoresist is applied to G-line photoresist or I-line photoresist.
[0024] The present invention classifies linear phenolic resin, retains the high molecular weight resin obtained by classification, modifies the low molecular weight phenolic resin, grafts a certain amount of poly(p-hydroxystyrene) polymer, and then remixes with the high molecular weight part, thereby improving the heat resistance and etching resistance of the phenolic resin. The present invention adopts atom transfer radical polymerization for modification and molecular weight regulation, so that the glass transition temperature of the phenolic resin can be controlled within a certain range.
[0025] Compared with the prior art, the present invention has the following advantages:
[0026] (1) The present invention improves the glass transition temperature of the phenolic resin, thereby enhancing the heat resistance and etching resistance of the phenolic resin.
[0027] (2) After the phenolic resin of the present invention is compounded to form a photoresist, the main indicators such as resolution and sensitivity are not affected by the modification. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a SEM picture of the modified phenolic resin of Example 2 after exposure to photoresist.
[0029] Figure 2 This is a SEM picture of the modified phenolic resin of Example 4 after exposure to photoresist.
[0030] Figure 3 This is the SEM picture of the unmodified phenolic resin F after compounding to form a photoresist after exposure. DETAILED DESCRIPTION
[0031] The present invention is further described in detail below in conjunction with specific embodiments, but the embodiments of the present invention are not limited thereto. For process parameters not particularly noted, conventional techniques may be used.
[0032] Synthesis and classification of phenolic resin
[0033] 1082g of m-cresol and 10g of oxalic acid were added to the reactor, and nitrogen was introduced under stirring. After replacing the gas, 560g of formalin solution was added, and the temperature was raised to 100°C for reflux reaction for 3 hours. After the reaction was completed, the reactor was changed to a distillation device, the temperature was raised to 150°C, and the distillation was carried out at normal pressure for 1 hour, and then the temperature was raised to 210°C, and the distillation was carried out under vacuum for 30 minutes. The solid was cooled and collected to obtain phenolic resin F.
[0034] The above 800g of phenolic resin F was dissolved in 7200g of methanol, and 7200g of distilled water was slowly added under stirring to separate the precipitated solid, i.e. the higher molecular weight part of phenolic resin, labeled as phenolic resin F1. After drying, it weighed 560g. The remaining turbid liquid was further added with 7200g of water and centrifuged to obtain a solid, which was the lower molecular weight part of phenolic resin, labeled as phenolic resin F2, and weighed 224g after drying.
[0035] The above 90g of phenolic resin F was dissolved in 810g of methanol, and 567g of distilled water was slowly added under stirring to separate the precipitated solid, i.e. the higher molecular weight part of phenolic resin, labeled as phenolic resin F3. After drying, it weighed 76g. 1000g of water was added to the remaining turbid liquid, and centrifuged to obtain a solid, which was the lower molecular weight part of phenolic resin, labeled as phenolic resin F4, which weighed 12g after drying.
[0036] Example 1
[0037] Take 32g of F2 resin and 0.016mol of triethylamine and dissolve them in 120g of tetrahydrofuran, slowly drop 0.015mol of bromoisobutyl bromide, and react at room temperature for 8 hours after the dropwise addition is completed. The reaction solution is precipitated in water, filtered, and the solid is dissolved-precipitated-filtered three times, and the solid is collected and dried. The above solid, 60g of 4-acetoxystyrene and 60g of dioxane are dissolved evenly, 0.04mol of cuprous bromide is added, nitrogen is introduced for 30min under stirring to exclude oxygen, and then 0.12mol of PMDETA is added through a syringe, and the reaction is carried out at 90℃ for 6h. After cooling, the reaction solution is passed through a neutral alumina column to remove the catalyst, and then precipitated in water. Tetrahydrofuran dissolves, water settles, repeats three times, and then the solid is collected and dried. The above solid is dissolved in 120g of methanol, 20g of sodium hydroxide is slowly added under stirring, and the dropwise addition is completed. After reflux reaction for 6h, it is cooled, the reaction solution is neutralized with hydrochloric acid and precipitated in water, and the solid is collected after dissolving and settling three times to obtain solid F2-1.
[0038] The solid F2-1 and 80 g (ie, 32×560 / 224) F1 were mixed evenly, and heated and dried to obtain the modified phenolic resin 1 of the present invention.
[0039] Example 2
[0040] Take 32g of F2 resin and 0.031mol of triethylamine and dissolve them in 120g of tetrahydrofuran, slowly drop 0.03mol of bromoisobutyl bromide, and react at room temperature for 8 hours after the dropwise addition is completed. The reaction solution is precipitated in water, filtered, and the solid is dissolved-precipitated-filtered three times, and the solid is collected and dried. The above solid, 60g of 4-acetoxystyrene and 60g of dioxane are dissolved evenly, 0.04mol of cuprous bromide is added, nitrogen is introduced for 30min under stirring to exclude oxygen, and then 0.12mol of PMDETA is added through a syringe, and the reaction is carried out at 90℃ for 6h. After cooling, the reaction solution is passed through a neutral alumina column to remove the catalyst, and then precipitated in water. Tetrahydrofuran is dissolved, water is precipitated, and the solid is collected and dried after three times. The above solid is dissolved in 120g of methanol, 20g of sodium hydroxide is slowly added under stirring, and the reflux reaction is completed for 6h and then cooled. The reaction solution is neutralized with hydrochloric acid and precipitated in water. After dissolving and precipitating three times, the solid is collected to obtain solid F2-2.
[0041] The solid F2-2 and 80g F1 were mixed evenly, and heated and dried to obtain the modified phenolic resin 2 of the present invention.
[0042] Example 3
[0043] Take 32g of F2 resin and 0.016mol of triethylamine and dissolve them in 120g of tetrahydrofuran, slowly add 0.015mol of bromoisobutyl bromide, and react at room temperature for 8 hours after the addition is complete. The reaction solution is precipitated in water, filtered, and the solid is dissolved-precipitated-filtered three times, and the solid is collected and dried. The above solid, 60g of 4-acetoxystyrene and 60g of dioxane are dissolved evenly, 0.04mol of cuprous bromide is added, nitrogen is introduced for 30min under stirring to exclude oxygen, and 0.12mol of PMDETA is added through a syringe, and the reaction is carried out at 90℃ for 12h. After cooling, the reaction solution is passed through a neutral alumina column to remove the catalyst, and then precipitated in water. Tetrahydrofuran is dissolved, water is precipitated, and the solid is collected and dried after three times. The above solid was dissolved in 120g of methanol, and 20g of sodium hydroxide was slowly added under stirring. After the addition was completed, reflux reaction was carried out for 6 hours and then cooled. The reaction solution was neutralized with hydrochloric acid and then precipitated in water. After dissolving and precipitating three times, the solid was collected to obtain solid F2-3.
[0044] The solid F2-3 and 80g F1 were mixed evenly, heated and dried to obtain the modified phenolic resin 3 of the present invention.
[0045] Example 4
[0046] Take 32g of F2 resin and 0.031mol of triethylamine and dissolve them in 120g of tetrahydrofuran, slowly drop 0.03mol of bromoisobutyl bromide, and react at room temperature for 8 hours after the dropwise addition is completed. The reaction solution is precipitated in water, filtered, and the solid is dissolved-precipitated-filtered three times, and the solid is collected and dried. The above solid, 60g of 4-acetoxystyrene and 60g of dioxane are dissolved evenly, 0.04mol of cuprous bromide is added, nitrogen is introduced for 30min under stirring to exclude oxygen, and then 0.12mol of PMDETA is added through a syringe, and the reaction is carried out at 90℃ for 12h. After cooling, the reaction solution is passed through a neutral alumina column to remove the catalyst, and then precipitated in water. Tetrahydrofuran is dissolved, water is precipitated, and the solid is collected and dried after three times. The above solid is dissolved in 120g of methanol, 20g of sodium hydroxide is slowly added under stirring, and the reflux reaction is completed for 6h and then cooled. The reaction solution is neutralized with hydrochloric acid and precipitated in water. After dissolving and precipitating three times, the solid is collected to obtain solid F2-4.
[0047] The solid F2-4 and 80g F1 were mixed evenly, heated and dried to obtain the modified phenolic resin 4 of the present invention.
[0048] Example 5
[0049] Take 12g of F4 resin and 0.013mol of triethylamine and dissolve them in 45g of tetrahydrofuran, slowly add 0.012mol of bromoisobutyl bromide, and react at room temperature for 8 hours after the addition is complete. The reaction solution is precipitated in water, filtered, and the solid is dissolved-precipitated-filtered three times, and the solid is collected and dried. The above solid, 22g of 4-acetoxystyrene and 22g of dioxane are dissolved evenly, 0.015mol of cuprous bromide is added, nitrogen is introduced for 30min under stirring to exclude oxygen, and 0.045mol of PMDETA is added through a syringe, and the reaction is carried out at 90℃ for 12h. After cooling, the reaction solution is passed through a neutral alumina column to remove the catalyst, and then precipitated in water. Tetrahydrofuran is dissolved, water is precipitated, and the solid is collected and dried after three times. The above solid was dissolved in 45g of methanol, and 7.5g of sodium hydroxide was slowly added under stirring. After the addition was completed, reflux reaction was carried out for 6 hours and then cooled. The reaction solution was neutralized with hydrochloric acid and precipitated in water. After dissolving and precipitating three times, the solid was collected to obtain solid F4-1.
[0050] The solid F4-1 and 76g F3 were mixed evenly, and heated and dried to obtain the modified phenolic resin 5 of the present invention.
[0051] Table 1
[0052] Glass transition temperature(℃) Modified phenolic resin 1 120.7 Modified phenolic resin 2 129.2 Modified phenolic resin 3 130.4 Modified phenolic resin 4 142.2 Modified phenolic resin 5 112.5 Unmodified phenolic resin F 100.6
[0053] The present invention adopts atom transfer radical polymerization to graft the phenolic hydroxyl group of low molecular weight phenolic resin to form polyparahydroxystyrene polymer. Atom transfer radical polymerization belongs to a kind of controllable / active radical polymerization, which can form a polymer with controllable molecular weight and narrow molecular weight distribution. The present invention realizes different grafting rates and molecular weights on the side groups of phenolic resin through controlled polymerization, thereby realizing the control of the glass transition temperature of phenolic resin. Comparing the unmodified phenolic resin F with Examples 1-5, it can be seen that the modified phenolic resin achieves a large increase in glass transition temperature. At the same time, comparing Examples 1 and 2, the grafting rate of Example 2 is higher than that of Example 1, so the glass transition temperature is higher than that of Example 1; comparing Examples 1 and 3, 2 and 4, the controlled radical polymerization time of Examples 3 and 4 is longer, and the molecular weight of atom transfer radical polymerization is gradually increased, so the molecular weight of Examples 3 and 4 is higher than that of 1 and 2, thereby resulting in an increase in its glass transition temperature. For Example 5, due to the change in the classification method (the ratio of methanol and water increased, that is, the ratio of added poor solvent water decreased), only the lower molecular weight phenolic resin F4 was separated, and a part of the low molecular weight still remained in F3 and could not be removed. There were more low molecular weight phenolic resins in the system, so the glass transition temperature of F3 resin was lower than that of other graded resins, resulting in the glass transition temperature of the modified phenolic resin in the final Example 5 not being greatly increased.
[0054] The formula of the photoresist is: 20wt% of modified phenolic resin, 2wt% of DNQ, 1% of surfactant bisphenol A epoxy resin, 1% of dye methyl red, and the balance is propylene glycol methyl ether acetate.
[0055] The above raw materials were mixed into a photoresist solution, which was spin-coated onto a silicon wafer at 2000 rpm, with a pre-baking temperature of 100°C for 1 min to obtain a thin film. The film was exposed to 365 nm ultraviolet light with an exposure dose of 30 to 60 mJ / cm 2 After exposure, the photoresist pattern is obtained by developing / fixing and post-baking at 120°C for 2 minutes. Figures 1 to 3 The resolution of the photoresists prepared by using the modified phenolic resins in Examples 1-5 does not exceed 0.7 micrometers.
[0056] from Figure 1 , 2 Compared with Figure 3, it can be found that the photoresist formed by the unmodified phenolic resin F collapses after exposure and development, while the modified phenolic resin does not. The collapse may be caused by the lower glass transition temperature of the unmodified phenolic resin F.
[0057] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A modified phenolic resin for photoresist, characterized in that: The modified phenolic resin is a mixed resin comprising a phenolic resin having a structure shown in Formula I and a phenolic resin having a structure shown in Formula II. Wherein R represents H or CH3, q+p=m, p>0, q>0, m, n, x are integers, and n>m, 5≤x≤30.
2. The modified phenolic resin for photoresist according to claim 1, characterized in that: The modified phenolic resin is obtained by blending the phenolic resins of formula I and formula II.
3. The modified phenolic resin for photoresist according to claim 1 or 2, characterized in that: The molecular weight range of formula I is 2000-30000 g / mol; the molecular weight range of formula II is 500-8000 g / mol.
4. The modified phenolic resin for photoresist according to claim 3, characterized in that: The molecular weight range of formula I is 16000-20000 g / mol; the molecular weight range of formula II is 600-3600 g / mol.
5. The method for preparing the modified phenolic resin for photoresist according to any one of claims 1 to 4, characterized in that: The steps include: (1) Add a phenolic compound and a catalyst to a reactor, introduce nitrogen gas under stirring, add formaldehyde after replacing the gas, heat to 100±10° C. and reflux for 3±1h; after the reaction, heat to 150±10° C. and distill at atmospheric pressure for 1±0.5h, then heat to 210±10° C. and distill under vacuum for 30±10min, cool and collect the solid to obtain phenolic resin I; (2) dissolving phenolic resin I in methanol to form a 10±5 wt% solution, slowly adding water under stirring until a large amount of solid precipitates, separating the solid to obtain phenolic resin II, i.e., a structure of formula I; after the solution is separated, evaporating the solvent, and collecting the residual solid phenolic resin III; (3) dissolving phenolic resin III and a catalyst in an appropriate solvent, slowly adding bromoisobutyl bromide dropwise, continuing the reaction after the addition is complete, settling the reaction solution in water, filtering, collecting the solid, dissolving and settling for several times, and drying to obtain phenolic resin IV; (4) Mix and dissolve phenolic resin IV, 4-acetoxystyrene and solvent uniformly, add catalyst and ligand, introduce nitrogen to replace air under stirring, seal, react at 90±10° C. for 6±2 h, cool, pass the reaction solution through a neutral alumina column, and settle in water; collect solid after dissolving and settling several times to obtain phenolic resin V, dissolve phenolic resin V in methanol, slowly add strong base, reflux for 6±2 h, and cool, neutralize the reaction solution with acid, and settle in water, dissolve and settle several times, and collect solid to obtain phenolic resin VI, i.e., structure of formula II; (5) The phenolic resin II and the phenolic resin VI are mixed evenly, and heated and dried to obtain a modified phenolic resin for photoresist.
6. The preparation method according to claim 5, characterized in that: The phenolic compound in step (1) includes one or more of m-cresol, p-cresol, o-cresol and phenol; and the catalyst is one or more of sodium hydroxide, potassium hydroxide, triethylamine, hydrochloric acid, sulfuric acid and oxalic acid.
7. The preparation method according to claim 5 or 6, characterized in that: The volume ratio of water added in step (2) to methanol is 1.0±0.2; and the catalyst in step (3) is one of triethylamine, pyridine and dimethylaminopyridine.
8. The preparation method according to claim 7, characterized in that: The catalyst in step (4) is a halogenated low-valent metal such as cuprous bromide, cuprous chloride, or ferric bromide; the solvent is tetrahydrofuran, 1,4-dioxane, or acetone; and the ligand is bipyridine or PMDETA.
9. The modified phenolic resin for photoresist according to any one of claims 1 to 4 is applied to G-line photoresist or I-line photoresist.
Citation Information
Patent Citations
Silicon-contained I-ray ultraviolet positive photoresist and film-forming resin thereof
CN101974202A
Preparing method for polyhydroxystyrene polymer with molecular weight narrowly distributed
CN105924553A