A method for non-radical polymerization and oxidation of benzothiophene
By activate sodium persulfate and non-radical polymerization of benzothiophene oxide by using heteroatom doped graphite phase carbon nitride under alkaline conditions, the problems of numerous steps and difficulty in controlling molecular weight in the prior art are solved, and high efficiency and low Cost preparation of S,S-dioxypolybenzothiophene, suitable for semiconductor devices.
Patent Information
- Application Number
- CN202211726894.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-30
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-12-30
AI Technical Summary
The prior art mostly uses acid conditions when polymerizing benzothiophene, with many steps and long reaction time, and it is difficult to prepare S,S-dioxy polybenzothiophene in one step, and the molecular weight control of the polymer is poor, which affects its in semiconductor devices. Application in.
Sodium persulfate is activated using heteroatom-doped graphite phase carbon nitride (SOPCN) under basic conditions, and non-radical polymerization of benzothiophene oxide is achieved by adding 2,6-di-tert-butyl p-methylphenol and hydroquinone. , control the molecular weight of the polymer to form S,S-dioxypolybenzothiophene.
The efficient resource utilization of benzothiophene is achieved, the reaction time is shortened, and the cost is reduced. The generated S,S-dioxypolybenzothiophene is suitable for transistors and other devices, filling the technical gap.
Smart Images

Figure CN115975157B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of organic polymerization, and in particular to a method for non-radical polymerization and oxidation of benzothiophene. Background Art
[0002] Benzothiophene is a white leaf-shaped crystal that is insoluble in water but soluble in most organic solvents. Polycyclic aromatic hydrocarbons such as benzothiophene mainly come from heavy oil products after catalytic cracking technology. After burning, these polycyclic aromatic hydrocarbons produce toxic gases that cause pollution such as acid rain, which will have a negative impact on the environment and human health. In view of this, polymerizing and oxidizing benzothiophene to S,S-dioxypolybenzothiophene is a method of protecting the environment and recycling resources.
[0003] Polymers can be divided into homopolymers and copolymers. Copolymers can be divided into random copolymers, alternating copolymers or block copolymers. Polymers can change the molecular weight of polymers by chemical means such as blocking, grafting, crosslinking and end-capping. Common methods for polymerizing benzothiophene include chemical methods and electrochemical methods. In the chemical method, the patent publication CN102119185A uses a variety of chemical oxidation methods to polymerize benzothiophene or benzothiophene derivatives into polybenzothiophene or polybenzothiophene derivatives. The patent publication CN102757611A uses acid doping (hydrochloric acid) and oxidant doping (ammonium persulfate, ferric chloride) methods to homopolymerize polybenzothiophene. The patent publication CN104395427B prepared polybenzothiophene in a dichloromethane system containing trifluoromethanesulfonic acid. The patent publication JP2003330166A reported that benzothiophene can be polymerized by cation alone under acid catalysis to obtain polybenzothiophene oligomers. In the electrochemical method, there are literature reports that benzothiophene can obtain soluble polybenzothiophene that can emit blue fluorescence in a mixed electrolyte formed by boron trifluoride ether solution and concentrated sulfuric acid (Journal of Polymer Science, 2001(06):807-810). In summary, most chemical methods for preparing polybenzothiophene are homopolymers, and require the use of different types of organic solvents and metal catalysts. In addition, the synthesis steps are numerous and complicated, and the reaction time is long. The organic waste liquid after the reaction also needs to be treated, which pollutes the environment. The electrochemical method requires the use of a variety of equipment such as an electrochemical workstation, which is relatively costly and has a long reaction time, mostly more than 24 hours. Most of the products obtained in these methods are polybenzothiophene, and the molecular weight of the polymer is not controlled. Moreover, it cannot be converted into S,S-dioxy polybenzothiophene in one step. Since S,S-dioxy polybenzothiophene has a strong electron-withdrawing group (-SO2-) that can improve the electron affinity, it has a higher electron mobility and fluorescence quantum efficiency. Compared with polybenzothiophene, it is more suitable for devices such as transistors.
[0004] In the chemical method, persulfate (PS) is used as the oxidant of the reaction to simplify the polymerization, reduce the reaction steps and time, save the reaction raw materials, and synthesize a large number of products in a short time. In addition, PS is cheap, has stable chemical properties, is easy to transport and store, and can be used in aqueous solution systems and emulsion systems. However, the oxidative polymerization of PS studied so far is mostly catalyzed under acidic conditions, and there are few studies on the use of PS for the polymerization and oxidation of benzothiophene in organic solvents under alkaline conditions.
[0005] So far, heteroatom (S, O, P) doped graphite phase carbon nitride (g-C3N4) (i.e., SOPCN) can activate PS and show high reactivity to achieve the oxidation of organic matter in solution. The commonly used methods for preparing heteroatom (S, O, P) doped g-C3N4 are high temperature calcination and solvothermal methods. Publication CN112473713A uses a hydrothermal-freeze drying method to prepare S-doped g-C3N4. Publication CN113101963A uses a high temperature calcination and thermal stripping method to prepare ultrathin P-doped g-C3N4. Publication CN112838197A uses a high temperature calcination method to successfully dope S, O and P into g-C3N4. S, O and P can form SN, ON and PN chemical bonds with g-C3N4, which are active sites for activating PS. Therefore, the use of S, O and P doped g-C3N4 for efficient activation of PS polymerization and oxidation of benzothiophene via a non-radical mechanism still needs to be explored.
[0006] Under alkaline conditions, PS can be efficiently activated by SOPCN in the form of non-radicals on SN, ON and PN, and benzothiophene is polymerized and oxidized to homopolymer S, S-dioxypolybenzothiophene. By adding 2,6-di-tert-butyl-p-methylphenol (BHT) and hydroquinone (HQ), the molecular weight of the polymer is controlled. In this process, the two steps of oxidation and polymerization are realized, and the efficient utilization of PS is realized, which saves resources and protects the environment, filling the technical gap.
[0007] In view of this, it is necessary to provide a technical solution to the above problems. Summary of the invention
[0008] The purpose of the present invention is to provide a non-radical polymerization oxidation method of benzothiophene which is simple, combines polymerization and oxidation, is low in cost and protects the environment. The present invention realizes the resource utilization of benzothiophene, turns waste into treasure, reduces costs and fills the technical gap.
[0009] In order to achieve the above object, the present invention adopts the following technical solutions:
[0010] A method for non-radical polymerization and oxidation of benzothiophene, comprising the following steps:
[0011] S1. Adjust the pH of the sodium persulfate solution to 7.0-8.0 with 0.4-0.6M sodium hydroxide solution, and stir at 400-600r / min for 15-25min; adjust the pH of the sodium persulfate solution to 10-12 with 0.9-1.1M sodium bicarbonate solution, and stir at 300-500r / min for 25-35min;
[0012] S2, dissolving an appropriate amount of benzothiophene in an organic solvent, stirring at 450-550 r / min for 25-35 min; and adding the sodium persulfate solution after pH adjustment in step S1 at a preset volume ratio, stirring at 350-450 r / min for 5-10 min;
[0013] S3. The mixed solution of step S2 is introduced with nitrogen for 5 to 15 minutes. After the nitrogen is introduced, an appropriate amount of heteroatom-doped carbon nitride is added to the solution, wherein the heteroatom includes S, O, and P, and the solution is transferred to a constant temperature stirring water bath; the mixture is stirred at 450 to 550 r / min for 5 to 15 minutes at 18 to 22°C, the temperature is increased to 40°C at 5°C / min, and the reaction is carried out at a constant temperature for 0.5 to 1.5 hours; the temperature is then increased to 50°C at 5°C / min, and the reaction is carried out at a constant temperature for 2 to 5 hours;
[0014] S4: 1.5-2.5M 2,6-di-tert-butyl-p-methylphenol and 0.1-0.5M hydroquinone are added to the reaction solution of step S2 respectively, and the reaction conditions are the same as those of step S3; the timing starts after the heteroatom-doped carbon nitride is added, and the content of benzothiophene in the solution is measured regularly.
[0015] Among them, in step S3, the purpose of introducing nitrogen is to eliminate the influence of oxygen.
[0016] Among them, in step S3, the purpose of setting the reaction temperature in two steps is to reduce the decomposition of the sodium persulfate solution (PS) and control the polymerization temperature. At the same time, setting the stirring speed within a certain range can ensure that various substances are mixed evenly, which is conducive to the uniform reaction; on the other hand, it also helps the entire reaction to be carried out at a constant temperature, avoiding temperature fluctuations from having a great impact on the reaction.
[0017] Among them, in step S4, 2,6-di-tert-butyl-p-methylphenol (BHT) and hydroquinone (HQ) are added to the reaction solution respectively to control the molecular weight of the polymer in the form of non-free radicals. By adding BHT and HQ, it is found that the polymerization oxidation reaction under alkaline conditions is a non-free radical mechanism. At the same time, the molecular weight of the polymer is controlled and the end capping is achieved. During the reaction, benzothiophene achieves polymerization oxidation. As the concentration of benzothiophene increases, the molecular weight of the generated product increases. When the product is treated with a rotary evaporator, insoluble matter is found. Subsequently, it is analyzed by infrared spectroscopy (FTIR) and it is found that the insoluble matter is S, S-dioxy polybenzothiophene.
[0018] Preferably, in step S1, the concentration of the sodium persulfate solution is 16 mM to 448 mM.
[0019] Preferably, in step S1, sodium hydroxide and sodium bicarbonate are used to adjust the pH of the sodium persulfate solution to 11, so as to ensure that the pH of the solution is always kept under alkaline conditions during the reaction. The purpose of stirring during the pH adjustment process is to make the solution evenly dispersed.
[0020] Preferably, in step S2, the organic solvent is a protic solvent, and the protic solvent is at least one of methanol and acetonitrile.
[0021] Preferably, in step S2, the volume ratio of the benzothiophene organic solution to the sodium persulfate solution is 1:1 to 3:1. More preferably, the volume ratio is 1:1.
[0022] Preferably, in step S2, the concentration of the benzothiophene organic solution is 200 to 5000 mg / L, more preferably 500 to 2500 mg / L.
[0023] Preferably, in step S3, the amount of heteroatom-doped carbon nitride added is 2-5 g / L, more preferably 3 g / L.
[0024] Preferably, in step S3, the preparation method of the heteroatom-doped carbon nitride is: stirring and grinding thiourea and phosphorus trichloride in a crucible, then placing them in a muffle furnace for reaction, heating to 550°C at 5°C / min, and maintaining for 1 to 5 hours; after cooling, drying and grinding the obtained solid to obtain the heteroatom-doped carbon nitride. More preferably, the mass ratio of thiourea to phosphorus trichloride is 5:1.
[0025] Preferably, in step S4, the solution after the reaction is centrifuged multiple times (at least 3 times) to separate the heteroatom-doped carbon nitride; the solution after centrifugation is evaporated in a rotary evaporator to dry the solvent; the solid product after rotary evaporation is collected and vacuum dried; the dried solid product is ground; the ground solid product is analyzed by infrared spectroscopy to obtain S,S-dioxypolybenzothiophene.
[0026] Preferably, the solvent is evaporated in a rotary evaporator using a two-step method: first, rotary evaporation is performed at 30° C., and when the solvent flows out, the temperature is increased to 60° C. at 2° C. / min.
[0027] Preferably, the heteroatom-doped carbon nitride after centrifugation is rinsed with acetonitrile for multiple times (at least 4 times), centrifuged, and the solution after centrifugation is collected; the solution after centrifugation is evaporated to dryness of the solvent in an oven, the temperature is raised to 80°C at 5°C / min, and maintained for 20 to 24 hours; there is a small amount of solid after drying, and the solid is subjected to infrared spectroscopy analysis to obtain S,S-dioxypolybenzothiophene.
[0028] Compared with the prior art, the method for non-radical polymerization and oxidation of benzothiophene of the present invention has the following beneficial effects:
[0029] Compared with the existing acidic catalytic polymerization, the present invention adopts the method of utilizing SN, ON and PN of heteroatom-doped carbon nitride (SOPCN) under alkaline conditions to efficiently activate sodium persulfate (PS) in a non-radical manner, thereby promoting the polymerization and oxidation of benzothiophene, and controlling the molecular weight and achieving end-capping by adding 2,6-di-tert-butyl-p-methylphenol (BHT) and hydroquinone (HQ), thereby finally obtaining S,S-dioxypolybenzothiophene. The polymer can be used in semiconductor devices such as transistors, thereby realizing the resource utilization of benzothiophene, turning waste into treasure, saving resources, and filling the technical gap in this field. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a graph showing the conversion rate of benzothiophene in the SOPCN / PS system of Example 1 of the present invention;
[0031] Figure 2 is a liquid phase diagram of the reaction solution of Example 1 of the present invention;
[0032] Figure 3 The UV-vis graphs of the reaction solutions of Examples 1 and 2 of the present invention;
[0033] Figure 4 This is a non-radical end-capping diagram of the SOPCN / PS system of Example 1 of the present invention;
[0034] Figure 5 This is the infrared spectrum of the insoluble matter after the reaction obtained in Example 2 of the present invention. DETAILED DESCRIPTION
[0035] In order to make the technical solutions and advantages of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] A method for non-radical polymerization and oxidation of benzothiophene, comprising the following steps:
[0038] 1. The steps for preparing SOPCN are as follows:
[0039] 10g of thiourea and 2g of phosphorus trichloride were stirred and ground evenly in a crucible and then placed in a muffle furnace for reaction. The temperature was raised to 550°C at 5°C / min in the muffle furnace and maintained for 3 hours. After cooling, the obtained solid was washed with ethanol and deionized water for 3 times each, dried in an oven at 60°C for 12 hours, and ground into fine powder with an agate mortar to finally obtain the solid SOPCN.
[0040] 2. The experimental steps of SOPCN catalyzing PS polymerization and oxidation of benzothiophene are as follows:
[0041] 1) Adjust the pH of 16 mM PS to 7.0 with 0.5 M sodium hydroxide solution and stir at 500 r / min for 20 min; adjust the pH of PS to 11.0 with 1 M sodium bicarbonate solution and stir at 400 r / min for 30 min.
[0042] 2) Stir 10 mL of 200 mg / L benzothiophene acetonitrile solution at 500 r / min for 30 min. Add 10 mL of 16 mM PS with pH adjusted in step 1 and stir at 400 r / min for 5 min.
[0043] 3) The mixed solution in step 2 was passed through nitrogen for 10 minutes. After the nitrogen was passed through, 3g / L SOPCN was added to the solution and transferred to a constant temperature stirring water bath. Stir at 500r / min for 10 minutes at 20°C, heat to 40°C at 5°C / min, and react at constant temperature for 3 hours. Then heat to 50°C at 5°C / min, and react at constant temperature for 3 hours.
[0044] 4) 2M BHT and 0.2M HQ were added to the reaction solution of step 2. The reaction conditions were the same as step 3.
[0045] 5) Start timing after adding SOPCN and take samples every 1 hour.
[0046] The concentration of benzothiophene was determined using high performance liquid chromatography.
[0047] 1) Determination method:
[0048] Benzothiophene standard stock solution: Dissolve 0.5 g benzothiophene in 100 mL acetonitrile solution and dilute to volume in a 100 mL volumetric flask to prepare a 5 g / L stock solution and store in a refrigerator.
[0049] 2) Drawing of the standard curve: The stock solution was diluted with acetonitrile and deionized water in a volume ratio of 1:1, with a gradient of 200, 100, 50, 25, 5 and 1 mg / L, the peak area in the liquid phase was recorded, and a curve of different concentrations and peak areas was drawn.
[0050] 3) Determination of water samples: Take an appropriate amount of reaction solution every 1 hour, filter it with a 0.22μm filter membrane, take 10μL of the filtered liquid into the liquid phase for measurement, and record the corresponding peak area.
[0051] At pH 11.0 and benzothiophene 200 mg / L, the conversion rate of benzothiophene in the SOPCN / PS system is shown in the figure below: Figure 1 shown.
[0052] 3. Analysis of oxidation products
[0053] After liquid phase analysis, it was found that many soluble low polymers were generated. The solution after the reaction and the catalyst SOPCN were centrifuged three times, and the solution after centrifugation was fully scanned by ultraviolet light. It was found that new substances were generated and dissolved in the acetonitrile-water mixed solution. The analysis results are as follows: Figure 2 , as shown in 3.
[0054] The non-radical end-capping diagram of SOPCN / PS system at pH 11.0 and benzothiophene 200 mg / L is shown in the figure. Figure 4 shown.
[0055] Example 2
[0056] A method for non-radical polymerization and oxidation of benzothiophene, comprising the following steps:
[0057] 1. The steps for preparing SOPCN are as follows:
[0058] 10g of thiourea and 2g of phosphorus trichloride were stirred and ground evenly in a crucible and then placed in a muffle furnace for reaction. The temperature was raised to 550°C at 5°C / min in the muffle furnace and maintained for 3 hours. After cooling, the obtained solid was washed with ethanol and deionized water for 3 times each, dried in an oven at 60°C for 12 hours, and ground into fine powder with an agate mortar to finally obtain the solid SOPCN.
[0059] 2. The experimental steps of SOPCN catalyzing PS polymerization and oxidation of benzothiophene are as follows:
[0060] 1) Adjust the pH of 16 mM PS to 7.0 with 0.5 M sodium hydroxide solution and stir at 500 r / min for 20 min; adjust the pH of PS to 11.0 with 1 M sodium bicarbonate solution and stir at 400 r / min for 30 min.
[0061] 2) Stir 10 mL of 5000 mg / L benzothiophene acetonitrile solution at 500 r / min for 30 min. Add 10 mL of 448 mM PS with pH adjusted in step 1 and stir at 400 r / min for 5 min.
[0062] 3) The mixed solution in step 2 was introduced with nitrogen for 10 minutes. After the nitrogen was introduced, 3 g / L SOPCN was added to the solution and transferred to a constant temperature stirring water bath. Stir at 500 r / min for 10 minutes at 20°C, heat to 40°C at 5°C / min, and react at constant temperature for 1 hour. Then heat to 50°C at 5°C / min, and react at constant temperature for 1 hour.
[0063] 4) 2M BHT and 0.2M HQ were added to the reaction solution of step 2. The reaction conditions were the same as step 3.
[0064] 3. Analysis of oxidation products
[0065] The solution after the reaction was centrifuged three times to separate the SOPCN. The solvent was evaporated from the centrifuged solution in a rotary evaporator. The rotary evaporation temperature adopted a two-step method. First, rotary evaporation was performed at 30°C, and when the solvent flowed out, the temperature was raised to 60°C at 2°C / min. The solid product after rotary evaporation was collected and vacuum dried at 60°C for 24 hours. The dried solid was ground for no less than 5 minutes. The solid product was analyzed by FTIR, and the analysis showed that it was S,S-dioxypolybenzothiophene. The SOPCN after centrifugation of the reaction solution was rinsed with acetonitrile 4 times, centrifuged, and the solution after centrifugation was collected. The solvent was evaporated from the centrifuged solution in an oven. The temperature was raised to 80°C at 5°C / min and maintained for 24 hours. There was a small amount of solid after drying, and the solid product was analyzed by FTIR, and the analysis showed that it was S,S-dioxypolybenzothiophene. The FTIR graph is as follows Figure 5 shown.
[0066] In Example 2, it can be analyzed that as the initial concentration of benzothiophene increases, the reaction product changes from a low polymer soluble in acetonitrile water to a polymer insoluble in water, and the final product obtained is S,S-dioxypolybenzothiophene.
[0067] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A method for non-radical polymerization and oxidation of benzothiophene, characterized in that: The following steps are involved: S1. Adjust the pH of the sodium persulfate solution to 7.0-8.0 with 0.4-0.6M sodium hydroxide solution and stir at 400-600 r / min for 15-25 min. Adjust the pH of the sodium persulfate solution to 10-12 with 0.9-1.1 M sodium bicarbonate solution and stir at 300-500 r / min for 25-35 min; S2, dissolving an appropriate amount of benzothiophene in an organic solvent, stirring at 450-550 r / min for 25-35 min; adding the sodium persulfate solution after pH adjustment in step S1 at a preset volume ratio, stirring at 350-450 r / min for 5-10 min; S3, the mixed solution of step S2 is introduced with nitrogen for 5-15 minutes, after the nitrogen is introduced, 2-5 g / L of heteroatom-doped carbon nitride is added to the solution, wherein the heteroatom includes S, O, and P, and the solution is transferred to a constant temperature stirring water bath; the solution is stirred at 450-550 r / min for 5-15 minutes at 18-22°C, the temperature is increased to 40°C at 5°C / min, and the reaction is carried out at a constant temperature for 0.5-1.5 hours; the temperature is then increased to 50°C at 5°C / min, and the reaction is carried out at a constant temperature for 2-5 hours; wherein the preparation method of the heteroatom-doped carbon nitride is as follows: thiourea and phosphorus trichloride are stirred and ground evenly in a crucible, and then placed in a muffle furnace for reaction, and the temperature is increased to 550°C at 5°C / min, and maintained for 1-5 hours; after cooling, the obtained solid is dried and ground to obtain the heteroatom-doped carbon nitride; S4: 1.5-2.5M 2,6-di-tert-butyl-p-methylphenol and 0.1-0.5M hydroquinone are added to the reaction solution of step S2 respectively, and the reaction conditions are the same as those of step S3; the timing starts after the heteroatom-doped carbon nitride is added, and the content of benzothiophene in the solution is measured regularly; wherein, the solution after the reaction is centrifuged multiple times to separate the heteroatom-doped carbon nitride; the solvent is evaporated from the solution after centrifugation in a rotary evaporator; the solid product after rotary evaporation is collected and vacuum dried; the dried solid product is ground; the ground solid product is analyzed by infrared spectroscopy to obtain S,S-dioxypolybenzothiophene.
2. The method for non-radical polymerization and oxidation of benzothiophene according to claim 1, characterized in that: In step S1, the concentration of the sodium persulfate solution is 16 mM to 448 mM.
3. The method for non-radical polymerization and oxidation of benzothiophene according to claim 1, characterized in that: In step S2, the organic solvent is a protic solvent, and the protic solvent is at least one of methanol and acetonitrile.
4. The method for non-radical polymerization and oxidation of benzothiophene according to claim 1, characterized in that: In step S2, the volume ratio of the benzothiophene organic solution to the sodium persulfate solution is 1:1 to 3:
1.
5. The method for non-radical polymerization and oxidation of benzothiophene according to claim 1, characterized in that: In step S2, the concentration of the benzothiophene organic solution is 200-5000 mg / L.
6. The method for non-radical polymerization and oxidation of benzothiophene according to claim 1, characterized in that: In step S4, the solvent is evaporated in a rotary evaporator in two steps: first, rotary evaporation is performed at 30°C, and when the solvent flows out, the temperature is increased to 60°C at a rate of 2°C / min.
7. The method for non-radical polymerization and oxidation of benzothiophene according to claim 1, characterized in that: In step S4, the heteroatom-doped carbon nitride after centrifugation is rinsed with acetonitrile for multiple times, centrifuged, and the solution after centrifugation is collected; the solution after centrifugation is evaporated in an oven to dry the solvent, and the temperature is increased to 80°C at 5°C / min and maintained for 20 to 24 hours; after drying, there is a small amount of solid, and the solid is analyzed by infrared spectroscopy to obtain S,S-dioxypolybenzothiophene.