Polycarbonate and preparation method and application thereof
By controlling the proportion of aromatic hydroxyl end groups in the oligomers in polycarbonate and the polymerization reaction conditions, the problem of insufficient heat resistance and yellowing resistance of polycarbonate in the prior art is solved, and the excellent polycarbonate is achieved Performance and widely used in optical discs, films and other fields.
Patent Information
- Application Number
- CN202310015473.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-04
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-01-04
AI Technical Summary
The prior art reduces the aromatic hydroxyl end group content in the oligomer by controlling the total amount of aromatic hydroxyl end group, limits the heat resistance and yellowing resistance of polycarbonate, and limits its application in optical discs, films and other fields. .
By controlling the proportion of aromatic hydroxy end groups in the oligomer, adjusting the mass content of aromatic hydroxy end groups in the polycarbonate between 150ppm and 240ppm, and the weight average molecular weight is ≤2000. The catalyst ratio in the actinization and polycondensation stages is used and The reaction conditions ensure that the proportion of aromatic hydroxyl end groups in the oligomer is 6% to 13%, so as to obtain excellent quality, good heat resistance and yellowing resistance.
The excellent quality, good heat resistance and yellowing resistance of polycarbonate are achieved, making it suitable for applications in optical discs, films and other fields, and the processing stability is improved through processing additives.
Smart Images

Figure BDA0004036268630000081
Abstract
Description
Technical Field
[0001] The invention relates to the field of polycarbonate preparation, and in particular to polycarbonate and a preparation method and application thereof. Background Art
[0002] As an engineering plastic with excellent performance, polycarbonate (PC) is widely used in automobiles, electronic equipment, construction, office supplies, optical discs, sports equipment, medical care, computers, aerospace and other fields. Generally, when applied to large sheets, it is desirable to use polycarbonate resins with high molecular weight / high intrinsic viscosity and low end-capping levels. For other applications such as optical discs and films, it is desirable to use polycarbonate resins with relatively low molecular weight, low intrinsic viscosity and high end-capping levels.
[0003] Patent TW200415174A obtains a polycarbonate resin with a low aromatic hydroxyl content by controlling the relative concentration and content of hydroxyl groups and chloroformate groups present in oligomer polycarbonate. The polycarbonate has aromatic hydroxyl end groups at an undetectable concentration (<5ppm).
[0004] Patent CN1610715A prepares polycarbonate with increased end-capping levels by adding an end-capping agent to the polycarbonate after the polycarbonate has reached a number average molecular weight of about 2,000-15,000 Daltons.
[0005] Patent CN1483055A produces polycarbonate with increased end-capping level by adding an end-capping agent with a special end structure.
[0006] The prior art only reduces the content of aromatic hydroxyl end groups in oligomers by controlling the total amount of aromatic hydroxyl end groups, so as to reduce the influence of aromatic hydroxyl end groups in oligomers on the heat resistance and yellowing resistance of products, which greatly limits its application. Summary of the invention
[0007] To solve the above problems, the present invention provides a polycarbonate and a preparation method and application thereof. By controlling the parameters of the present invention, the obtained polycarbonate has excellent appearance, good heat resistance and yellowing resistance, and can be applied to polycarbonate products in the fields of optical disks, films, etc.
[0008] To achieve the purpose of the present invention, the present application adopts the following technical solutions:
[0009] A polycarbonate, wherein the mass content of aromatic hydroxyl end groups in the polycarbonate is 150ppm-240ppm, wherein the mass content of aromatic hydroxyl end groups in oligomers with a weight average molecular weight of ≤2000 accounts for 6%-13% of the total amount of aromatic hydroxyl end groups in the polycarbonate product.
[0010] In the process of comprehensive research on the structure and properties of polycarbonate, the inventors surprisingly found that the proportion of aromatic hydroxyl end groups of oligomers with a weight-average molecular weight of not more than 2000 in the copolymer has a great influence on the performance of the material. When the proportion of oligomer hydroxyl end groups is low, even if the total aromatic hydroxyl end group content of the polycarbonate powder is high (150ppm~240ppm), its heat resistance and yellowing resistance are inferior to those of polycarbonate products with a low total hydroxyl end group content of the powder. After a lot of research and experiments by the inventors, it was found that by controlling the aromatic hydroxyl end group content in the oligomer and the total aromatic hydroxyl end group content in the polycarbonate, a polycarbonate product with excellent appearance, good heat resistance and yellowing resistance can be obtained, which can be used in the fields of optical disks, films, etc.
[0011] Preferably, the polycarbonate is an aromatic polycarbonate, and particularly preferably, the polycarbonate is a bisphenol A polycarbonate.
[0012] Another object of the present invention is to provide a method for preparing polycarbonate, the method comprising:
[0013] (a) Photochemical stage: adding an alkaline solution of a dihydric phenol compound, phosgene, an inert organic solvent, and a catalyst to a polymerization reactor for reaction to obtain an oligomer mixture, and separating the oligomer mixture into oil and water phases to obtain an oil phase oligomer organic solvent and an aqueous phase alkaline solution;
[0014] (b) Condensation polymerization stage: Add the catalyst 2 solution and the end-capping agent solution to the oil phase obtained in the photochemical stage and mix them evenly; add the aqueous solution of alkali metal hydroxide and the aqueous solution of catalyst 1 to the aqueous phase obtained in the photochemical stage, then mix the obtained oil phase and aqueous phase, complete the polymerization reaction under stirring, and obtain a polycarbonate solution.
[0015] Preferably, the dihydric phenolic compound includes 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), hydroquinone, resorcinol, 1,1-bis(4-hydroxyphenyl)phenylethane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(3-methyl-4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)cyclododecane, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfide, 9,9-bis(4-hydroxyphenyl)fluorene, 9,9-bis(3-methyl-4-hydroxyphenyl)fluorene, preferably bisphenol A;
[0016] Preferably, the molar ratio of phosgene to bisphenol compound is 1 to 1.5:1, preferably 1.1 to 1.3:1;
[0017] Preferably, the temperature of the photochemical stage reaction is <55°C, preferably 23-40°C, more preferably 26-40°C;
[0018] Preferably, the pH value in the photochemical stage is 10.5 to 13.5, preferably 11.5 to 12.5.
[0019] Preferably, the catalyst added in the photochemical stage is a quaternary ammonium salt or quaternary phosphonium salt phase transfer catalyst, such as tetra-tert-butylammonium chloride, tetra-tert-butylammonium bromide, trimethylbenzylammonium chloride, trioctylmethylammonium chloride, hexadecyltrimethylammonium bromide, triethylbenzylammonium chloride, trialkylmethylammonium chloride, tetra-tert-butylphosphonium chloride, tetra-tert-butylphosphonium bromide, preferably tetra-tert-butylammonium chloride;
[0020] Preferably, the molar ratio of the amount of the catalyst 1 added to the dihydric phenol compound is 0.01 to 0.08%, preferably 0.035 to 0.055%.
[0021] By adding a quaternary ammonium salt phase transfer catalyst in the photochemical stage, the reaction and hydrolysis ratio of the chloroformate group is changed, and the weight average molecular weight of the oligomer obtained by polymerization in the photochemical stage is controlled, so as to effectively control the proportion of the hydroxyl end groups of the oligomer.
[0022] Preferably, in the photochemical stage, the alkali in the alkaline solution of the dihydric phenol compound is an alkali metal hydroxide, such as sodium hydroxide, potassium hydroxide, and the like.
[0023] Preferably, the inert organic solvent in the photochemical stage includes one or more of dichloromethane, chloroform, dichloroethane and trichloroethane, preferably dichloromethane.
[0024] Preferably, the catalyst 2 in the polycondensation stage is a non-phase transfer catalyst selected from one or more of triethylamine, tributylamine, trioctylamine, N-methylpiperidine, N-ethylpiperidine, N-n-propylpiperidine, N-isopropylpiperidine, tributylbenzylammonium, tetraethylammonium hydroxide, tetraethylammonium chloride, tetraethylammonium bromide, tetraethylammonium hydrogen sulfate, tetraethylammonium tetrafluoroborate, and tetrabutylammonium;
[0025] Preferably, the molar ratio of the amount of the catalyst 2 added to the bisphenol compound is 0.01 to 10%, preferably 0.1 to 1%.
[0026] Preferably, in the polycondensation reaction stage, the molar ratio of the catalyst 2 added to the oil phase to the catalyst 1 added to the water phase is 0.9-1.1 times the molar ratio of the chloroformate group (CF) to the hydroxyl end group (-OH) in the photochemical reaction liquid. By adjusting the addition ratio of the two catalysts, the relative speed of the coupling reaction and the hydrolysis reaction can be effectively controlled, so as to effectively control the proportion of the hydroxyl end groups of the oligomers.
[0027] Preferably, the end-capping agent in the polycondensation stage is an aromatic monohydric phenol, preferably a combination of one or more selected from phenol, methylphenol, tert-butylphenol, and p-cumylphenol;
[0028] Preferably, the amount of the end-capping agent added is 1 to 10% of the molar amount of the dihydric phenol compound.
[0029] Preferably, the weight average molecular weight of the oligomer obtained by polymerization in the photochemical stage is 2000-6000 g / mol, preferably 4500-5500 g / mol, more preferably 4800-5200 g / mol.
[0030] Preferably, an aqueous solution of alkaline hydroxide is added during the polycondensation stage to maintain the pH value of the aqueous phase of the reaction system at 11 to 13.5, preferably 12 to 12.5;
[0031] Preferably, the reaction temperature in the polycondensation stage is less than 60°C, preferably 20 to 45°C, more preferably 35 to 40°C;
[0032] A polycarbonate obtained by the preparation method of the present invention has an aromatic hydroxyl end group mass content of 150ppm to 240ppm, wherein the aromatic hydroxyl end group content in the oligomer with a weight average molecular weight of ≤2000 accounts for 6% to 13% of the total aromatic hydroxyl end group content in the polycarbonate product.
[0033] The present invention can effectively control the proportion of aromatic hydroxyl end group content in the oligomer part with a molecular weight of ≤2000 at a low end-capping rate by adjusting the type and proportion of catalyst added in the photochemical stage and the polycondensation stage, thereby making the polycarbonate product have excellent heat resistance and yellowing resistance.
[0034] The present invention also provides the use of the polycarbonate or the polycarbonate prepared by the preparation method. The polycarbonate can be processed to obtain the desired molded product, such as a film, by adding common additives such as stabilizers, release agents, fillers or glass fibers before or during processing.
[0035] The polycarbonate prepared by the method of the invention has better heat resistance, base color and processing stability, and can be used in the fields of optical disks, films, etc. DETAILED DESCRIPTION
[0036] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0037] The pH value of the photochemical reaction liquid and the aqueous phase of the polycondensation reaction liquid was measured by a pH tester.
[0038] The molecular weight of the polymer was tested by gel permeation chromatography (GPC) (equipment model: Agilent Technologies 1260infinity), with dichloromethane as the mobile phase, PS as the standard sample, a flow rate of 1 mL / min, and both the column temperature and the box temperature at 30°C.
[0039] The oil phase of the photochemical reaction liquid was determined by NMR 1 The aromatic hydroxyl end group content in the oil phase of the photochemical reaction liquid was calculated by integrating the peaks from the bisphenol compounds in the H-NMR spectrum. The aromatic hydroxyl end group content in the aqueous phase of the photochemical reaction liquid was calculated by testing the BPA content in the aqueous phase of the photochemical reaction liquid by HPLC. The aromatic hydroxyl end group content in the photochemical reaction liquid was calculated based on the water-to-oil ratio.
[0040] The chloroformate group (CF) concentration was measured by oxidation-reduction titration, silver nitrate titration, based on the chloride ion concentration, with reference to JIS K8203.
[0041] Determination of powder, Soxhlet extraction of oligomers by NMR 1 The aromatic hydroxyl terminal group content in the powder and Soxhlet extracted oligomers was calculated by integrating the peak derived from the bisphenol compound from the H-NMR spectrum.
[0042] The YI value of the 3 mm test piece obtained by injection molding at 300°C was measured by a colorimeter to reflect the yellowing degree of the sample.
[0043] The heat-resistant color difference was obtained by measuring the base color changes of test pieces A and B using a colorimeter. Test piece A was a 3 mm test piece obtained by injection molding at 320°C, and test piece B was a 3 mm test piece obtained by injection molding the PC powder after the injection molding of test piece A was completed and the PC powder stayed in the injection molding machine at 320°C for 10 minutes.
[0044] Soxhlet extraction of oligomers: Place 25 g of powder in a Soxhlet extractor and weigh it. Add 150 mL of tetrahydrofuran / acetone solvent and place a magnetic bar. Heat in a water bath at 70°C for 24 hours, evaporate the solvent in a rotary evaporator, and weigh to calculate the mass of the oligomer. Repeat this step until the round-bottom flask reaches a constant weight.
[0045] The raw materials used in the following examples are:
[0046] Bisphenol A: industrial grade, purchased from Bluestar Chemical New Materials Co., Ltd. (Wuxi Resin Factory);
[0047] Tetramethyl bisphenol A: industrial grade, purchased from Changzhou Anker Biotechnology Co., Ltd.;
[0048] Dichloromethane: analytical grade, purchased from Tianjin Kemeiou Chemical Reagent Co., Ltd.;
[0049] p-tert-Butylphenol: analytical grade, purchased from Shandong Chemical Research Institute;
[0050] Tetrabutylammonium bromide: analytical grade, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd.;
[0051] Triethylamine: analytical grade, purchased from Tianjin Komiou Chemical Reagent Co., Ltd.
[0052] Tetraethylammonium hydroxide: analytical grade, purchased from Tianjin Komiou Chemical Reagent Co., Ltd.
[0053] Example 1
[0054] Photochemical stage: Ultrapure water and 32wt% NaOH are mixed in a stirred tank at a mass ratio of 3.93:1 to form a NaOH solution. Bisphenol A (BPA) solid and tetrabutylammonium bromide solid are added to the NaOH solution, stirred and dissolved, and the mass concentration of BPA in the aqueous phase is controlled to be 14.5wt%, and the mass concentration of tetrabutylammonium bromide is controlled to be 0.09wt‰. BPA and tetrabutylammonium bromide aqueous solutions, dichloromethane, phosgene, and 32wt% NaOH are respectively introduced into a photochemical reactor composed of a group of static mixers at a flow rate of 62kg / hr, 60kg / hr, 4.7kg / hr, and 2.4kg / hr. The reactor diameter is DN40 and the length is 800mm. The reactor outlet temperature is controlled to be 35℃ and the injection time is 15min.
[0055] Polycondensation stage: The emulsion obtained in the photochemical stage is introduced into an inclined plate separator for water-oil separation. After the chloroformate group (CF) and the aromatic hydroxyl end group (-OH) are tested, 0.5 kg of a 10 wt% dichloromethane solution of p-tert-butylphenol and 0.32 kg of a 3 wt% dichloromethane solution of triethylamine are added to the oil phase. 0.17 kg of a 32 wt% NaOH solution and 0.051 kg of a 5 wt% tetrabutylammonium bromide aqueous solution are added to the water phase. The water-oil phase is passed into two 40 L overflow stirring tanks connected in series, and the temperature in the two reactors is controlled to be 35 ° C. The reaction is continued for 15 minutes, the crude reaction product is separated to remove the water phase, and the organic phase is washed, separated, purified, and the dichloromethane solvent is removed to obtain a colorless polycarbonate powder.
[0056] Embodiments 2 to 6
[0057] The main difference between Examples 2 to 6 and Example 1 is that the amount of BPA and tetrabutylammonium bromide aqueous solution added and the amount of polycondensation sodium hydroxide added thereby changed to change the ratio of chloroformate groups (CF) to aromatic hydroxyl end groups (-OH) in the photochemical reaction solution, or the amount of PTBP added in the polycondensation stage changed to change the end-capping rate and molecular weight of the final product, or the type of bisphenol compound was changed, and the other conditions were the same as in Example 1.
[0058] Comparative Example 1
[0059] The main difference between Comparative Example 1 and Example 1 is that the phase transfer catalyst and the organic tertiary amine catalyst are added to the polycondensation liquid in different ratios of chloroformate groups (CF) and aromatic hydroxyl end groups (-OH).
[0060] Comparative Example 2
[0061] The main difference between Comparative Example 2 and Example 1 is that the type and amount of catalyst added in the photochemical stage remain unchanged, only a phase transfer catalyst is added in the polycondensation stage, and no catalyst 1 is added to the aqueous phase.
[0062] Comparative Example 3
[0063] The main difference between Comparative Example 3 and Example 1 is that the type and amount of catalyst added in the photochemical stage remain unchanged, and only an organic tertiary amine catalyst is added to the water phase in the polycondensation stage, and no catalyst 2 is added to the oil phase.
[0064] Table 1 Parameters and reaction results in Examples and Comparative Examples
[0065]
Claims
1. A polycarbonate, characterized in that: The mass content of aromatic hydroxyl end groups in the polycarbonate is 150ppm-240ppm, wherein the mass content of aromatic hydroxyl end groups in the oligomer with a weight average molecular weight of ≤2000 accounts for 6%-13% of the total amount of aromatic hydroxyl end groups in the polycarbonate product.
2. The polycarbonate according to claim 1, characterized in that The polycarbonate is an aromatic polycarbonate.
3. The polycarbonate according to claim 2, characterized in that The polycarbonate is bisphenol A type polycarbonate.
4. A method for preparing the polycarbonate according to any one of claims 1 to 3, characterized in that: The method includes: (a) Photochemical stage: adding an alkaline solution of a dihydric phenol compound, phosgene, an inert organic solvent, and a catalyst to a polymerization reactor for reaction to obtain an oligomer mixture, and separating the oligomer mixture into oil and water phases to obtain an oil phase oligomer organic solvent and an aqueous phase alkaline solution; (b) Condensation polymerization stage: Add the catalyst 2 solution and the end-capping agent solution to the oil phase obtained in the photochemical stage and mix them evenly; add the aqueous solution of alkali metal hydroxide and the aqueous solution of catalyst 1 to the aqueous phase obtained in the photochemical stage, then mix the obtained oil phase and aqueous phase, complete the polymerization reaction under stirring, and obtain a polycarbonate solution.
5. The preparation method according to claim 4, characterized in that: The diphenolic compound includes 2,2-bis(4-hydroxyphenyl)propane (bisphenol A), hydroquinone, resorcinol, 1,1-bis(4-hydroxyphenyl)phenylethane, 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 1,1-bis(3-methyl-4-hydroxyphenyl)cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)cyclododecane, 4,4'-dihydroxybiphenyl, 4,4'-dihydroxydiphenyl ether, 4,4'-dihydroxydiphenyl sulfide, 9,9-bis(4-hydroxyphenyl)fluorene, and 9,9-bis(3-methyl-4-hydroxyphenyl)fluorene.
6. The preparation method according to claim 5, characterized in that: The dihydric phenol compound is bisphenol A.
7. The preparation method according to claim 4, characterized in that: The molar ratio of phosgene to the bisphenol compound is 1 to 1.5:
1.
8. The preparation method according to claim 7, characterized in that: The molar ratio of phosgene to the bisphenol compound is 1.1-1.3:
1.
9. The preparation method according to claim 4, characterized in that: The temperature of the photochemical reaction is <55°C.
10. The preparation method according to claim 9, characterized in that: The temperature of the photochemical stage reaction is 23-40°C.
11. The preparation method according to claim 10, characterized in that: The temperature of the photochemical stage reaction is 26-40°C.
12. The preparation method according to claim 4, characterized in that: The pH value in the photochemical stage is 10.5-13.
5.
13. The preparation method according to claim 12, characterized in that: The pH value in the photochemical stage is 11.5-12.
5.
14. The preparation method according to claim 4, characterized in that: The catalyst added in the photochemical stage is a quaternary ammonium salt or quaternary phosphonium salt phase transfer catalyst.
15. The preparation method according to claim 14, characterized in that: The catalyst added in the photochemical stage is tetra-tert-butylammonium chloride, tetra-tert-butylammonium bromide, trimethylbenzylammonium chloride, trioctylmethylammonium chloride, hexadecyltrimethylammonium bromide, triethylbenzylammonium chloride, trialkylmethylammonium chloride, tetra-tert-butylphosphonium chloride, and tetra-tert-butylphosphonium bromide.
16. The preparation method according to claim 15, characterized in that: The first catalyst added in the photochemical stage is tetra-tert-butylammonium chloride.
17. The preparation method according to claim 4, characterized in that: The molar ratio of the added amount of the catalyst 1 to the dihydric phenol compound is 0.01-0.08%.
18. The preparation method according to claim 17, characterized in that: The molar ratio of the added amount of the catalyst 1 to the dihydric phenol compound is 0.035-0.055%.
19. The preparation method according to claim 4, characterized in that: In the photochemical stage, the base in the alkaline solution of the dihydric phenol compound is an alkali metal hydroxide.
20. The preparation method according to claim 4, characterized in that: The inert organic solvent in the photochemical stage includes one or more of dichloromethane, chloroform, dichloroethane and trichloroethane.
21. The preparation method according to claim 20, characterized in that: The inert organic solvent in the photochemical stage is dichloromethane.
22. The preparation method according to claim 4, characterized in that: The catalyst 2 in the polycondensation stage is a non-phase transfer catalyst, selected from one or more of triethylamine, tributylamine, trioctylamine, N-methylpiperidine, N-ethylpiperidine, N-n-propylpiperidine, N-isopropylpiperidine, tributylbenzylammonium, tetraethylammonium hydroxide, tetraethylammonium chloride, tetraethylammonium bromide, tetraethylammonium hydrogen sulfate, tetraethylammonium tetrafluoroborate, and tetrabutylammonium.
23. The preparation method according to claim 4, characterized in that: The molar ratio of the added amount of the catalyst 2 to the bisphenol compound is 0.01-10%.
24. The preparation method according to claim 23, characterized in that: The molar ratio of the added amount of the catalyst 2 to the bisphenol compound is 0.1-1%.
25. The preparation method according to claim 4, characterized in that: In the polycondensation reaction stage, the molar ratio of the catalyst 2 added to the oil phase to the catalyst 1 added to the water phase is 0.9-1.1 times the molar ratio of the chloroformate group (CF) to the hydroxyl end group (-OH) in the photochemical reaction liquid.
26. The preparation method according to claim 4, characterized in that: The end-capping agent in the polycondensation stage is an aromatic monohydric phenol.
27. The preparation method according to claim 26, characterized in that: The end-capping agent in the polycondensation stage is a combination of one or more of phenol, methylphenol, tert-butylphenol and p-cumylphenol.
28. The preparation method according to claim 4, characterized in that: The amount of the end-capping agent added in the polycondensation stage is 1 to 10% of the molar amount of the dihydric phenol compound.
29. The preparation method according to claim 4, characterized in that: The weight average molecular weight of the oligomers obtained by polymerization in the photochemical stage is 2000-6000 g / mol.
30. The preparation method according to claim 29, characterized in that: The end-capping agent in the polycondensation stage is 4500-5500 g / mol.
31. The preparation method according to claim 30, characterized in that: The end-capping agent in the polycondensation stage is 4800-5200 g / mol.
32. The preparation method according to claim 4, characterized in that: During the polycondensation stage, an aqueous solution of alkaline hydroxide is added to maintain the pH value of the aqueous phase of the reaction system at 11-13.
5.
33. The preparation method according to claim 32, characterized in that: During the polycondensation stage, an aqueous solution of alkaline hydroxide is added to maintain the pH value of the aqueous phase of the reaction system at 12 to 12.
5.
34. The preparation method according to claim 4, characterized in that: The reaction temperature in the polycondensation stage is less than 60°C.
35. The preparation method according to claim 34, characterized in that: The reaction temperature in the polycondensation stage is 20-45°C.
36. The preparation method according to claim 35, characterized in that: The reaction temperature in the polycondensation stage is 35-40°C.