Coating, slider, guide rail and method for preparing coating material

By using aluminum alloy coating and the first silicon carbide whisker structure on the surface of the guide rail, the problem of corrosion of the guide rail in an acidic environment is solved, the corrosion resistance and strength of the guide rail are improved, and the maintenance cost is reduced.

CN115976435BActive Publication Date: 2024-12-03HUIZHOU SHENKEDA INTELLIGENT EQUIP CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202211652100.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-21
Publication Date
2024-12-03
Estimated Expiration
2042-12-21

AI Technical Summary

Technical Problem

The existing guide rail materials are prone to corrosion in an acidic environment, and the anti-rust layer has poor acid resistance and is easily damaged, resulting in high maintenance costs. The prior art cannot effectively improve the corrosion resistance and strength of the guide rail.

Method used

Aluminum alloy coating is used, magnesium, zinc, tungsten and thallium are added, and a first silicon carbide whisker structure is formed on its surface to enhance the hardness and corrosion resistance of the coating. At the same time, by setting the coating on the surface of the guide rail, it ensures that it is under stress. Not easy to fall off.

Benefits of technology

The corrosion resistance and strength of the guide rails are significantly improved, the service life is extended, the maintenance cost is reduced, and the production cost of the plating is reduced by optimizing the distribution of silicon carbide whiskers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115976435B_ABST
    Figure CN115976435B_ABST
Patent Text Reader

Abstract

The present application provides a coating, a slider, a guide rail and a method for preparing a coating material, wherein the coating comprises an aluminum alloy and a first silicon carbide whisker structure. In terms of mass percentage, the aluminum alloy comprises magnesium: 2-6%, zinc: 0.2-1%, silicon: 0.2-1%, rare earth elements: 0.1-0.5%, thallium: 1-5%, aluminum: 86.5-97.5% and impurity remainder. By adding magnesium, zinc, silicon, rare earth elements and thallium to the aluminum base for making the coating, the strength of the coating can be improved while improving the corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of guide rails, and in particular to a guide rail material and a method for preparing the guide rail material. Background Art

[0002] Guide rails, also known as linear guides and linear slides, are used in linear reciprocating motion situations and can achieve high-precision linear motion under load.

[0003] After the guide rail is installed in the application scenario, it is easily affected by the external environment, such as corrosion by acidic substances. Therefore, in order to ensure the service life of the guide rail, the guide rail must have excellent corrosion resistance.

[0004] In the related art, a rust-proof layer is applied on the surface of the guide rail, but the rust-proof layer is usually a single metal, such as copper or silver, which results in poor acid resistance of the rust-proof layer, and the rust-proof layer is easily rubbed off due to bumps, resulting in a short rust-proof time for the guide rail. In order to prevent foreign substances from directly contacting the guide rail after the rust-proof layer is worn, an organic resin rust-proof oil is applied on the rust-proof layer. However, the organic resin rust-proof oil can only isolate a small amount of acidic substances and cannot improve the strength of the rust-proof layer, resulting in poor protection effect. In addition, the organic resin rust-proof oil needs to be replenished frequently, which increases the maintenance cost of the equipment. Summary of the invention

[0005] In view of this, it is necessary to provide a coating, a slider, a guide rail and a method for preparing the coating material, aiming to provide a coating with good strength and corrosion resistance to protect the guide rail.

[0006] An embodiment of the present application provides a coating layer, which is applied to a slider, and the coating layer includes an aluminum alloy and a first silicon carbide whisker structure. In terms of mass percentage, the aluminum alloy includes magnesium: 2-6%, zinc: 0.2-1%, silicon: 0.2-1%, rare earth elements: 0.1-0.5%, thallium: 1-5%, aluminum: 86.5-97.5% and impurity remainder.

[0007] In the above embodiment, by adding magnesium, zinc, tungsten and thallium to the aluminum base for making the coating, the strength of the coating can be increased while the corrosion resistance can be improved. At the same time, the coating includes a first silicon carbide whisker structure, which can increase the hardness of the coating and make the coating less likely to fall off due to external force.

[0008] In at least one embodiment, magnesium is 4-5%.

[0009] In the above embodiment, adding 4-5% magnesium to aluminum can make the aluminum alloy have better strength, excellent corrosion resistance, and resistance to intergranular corrosion, exfoliation corrosion and stress corrosion.

[0010] In at least one embodiment, zinc is 0.5-0.7%.

[0011] In the above embodiment, adding 0.5-0.7% zinc to aluminum can make the aluminum alloy with aluminum+zinc+magnesium structure have better strength and corrosion resistance.

[0012] In at least one embodiment, silicon is 0.3-0.7%.

[0013] In the above embodiment, by adding 0.3-0.7% silicon to the aluminum alloy containing magnesium, magnesium and silicon form a strengthening phase MgSi in the aluminum alloy, so as to improve the strength of the aluminum alloy.

[0014] In at least one embodiment, the thallium is 1.5-3%.

[0015] In the above embodiment, adding 1.5-3% thallium to the aluminum alloy can improve the strength of the aluminum alloy and enhance the corrosion resistance of the aluminum alloy.

[0016] An embodiment of the present application further provides a slider, comprising a slider body and a coating as in any of the above embodiments, wherein the coating is coated on the outer surface of the slider body, and a first silicon carbide whisker structure is disposed on a side of the aluminum alloy away from the slider body.

[0017] In the above embodiment, the coating is coated on the outer surface of the slider body, and the first silicon carbide whisker structure is arranged on the side of the aluminum alloy away from the slider body to enhance the comprehensive mechanical properties of the side of the aluminum alloy away from the slider body, such as high hardness, wear resistance, high temperature resistance and corrosion resistance, so that when the slider is impacted, rubbed or corroded, the part with high comprehensive mechanical properties in the coating hits, rubs against external objects or contacts corrosive substances, so as to prevent external objects or corrosive substances from passing through the coating to damage the slider body, thereby improving the protection ability of the coating to the slider body. In addition, compared with the first silicon carbide whisker structure being arranged on the entire coating, the consumption of the second silicon carbide whisker structure can be reduced, thereby reducing the production cost of the coating.

[0018] In at least one embodiment, the slider body includes a body layer and a hardened layer, the body layer is connected to the hardened layer, the hardened layer includes a second silicon carbide whisker structure, and the hardened layer is provided with a roller channel for assembling a ball.

[0019] In the above embodiment, by separately setting different parts of the slider body, that is, setting the second silicon carbide whisker structure at the part that cooperates with the roller, the slider body can be improved in hardness, wear resistance, high temperature resistance, corrosion resistance, etc. At the same time, compared with setting the second silicon carbide whisker structure on the entire slider body, the consumption of the second silicon carbide whisker structure can be reduced, thereby reducing the manufacturing cost of the slider body.

[0020] An embodiment of the present application further provides a guide rail, comprising a slide rail and a slider as in any of the above embodiments, wherein the slider is slidably disposed on the slide rail.

[0021] In at least one embodiment, the slide rail is provided with a coating, the coating is coated on the outer surface of the slide rail, and the first silicon carbide whisker structure is provided on a side of the aluminum alloy away from the slide rail.

[0022] In the above embodiment, the coating is coated on the outer surface of the slide rail, and the first silicon carbide whisker structure is arranged on the side of the aluminum alloy away from the slide rail to enhance the comprehensive mechanical properties of the aluminum alloy away from the slide rail, such as high hardness, wear resistance, high temperature resistance and corrosion resistance, so that when the slide rail is hit, rubbed or corroded, the part of the coating with high comprehensive mechanical properties hits, rubs against external objects or contacts corrosive substances, so as to prevent external objects or corrosive substances from passing through the coating and damaging the slide rail, thereby improving the coating's ability to protect the slide rail. Moreover, compared with the first silicon carbide whisker structure being arranged on the entire coating, the consumption of the second silicon carbide whisker structure can be reduced, thereby reducing the production cost of the coating.

[0023] One embodiment of the present application also provides a method for preparing a coating material, comprising the following steps: the following steps are all performed under inert gas conditions;

[0024] The aluminum alloy is heated to a molten state to obtain a liquid aluminum alloy;

[0025] treating carbonized rice husk, iron oxide and sodium fluoride through a heating process to obtain a first mixture containing a first silicon carbide whisker structure;

[0026] Soak the first mixture in water to dissolve the sodium fluoride, repeating multiple times;

[0027] Aluminum powder is added to the first mixture after soaking in water and reacted fully to obtain a second mixture; wherein the density of the first silicon carbide whisker structure in the second mixture is less than the density of the liquid aluminum alloy;

[0028] The second mixture is added into the liquid aluminum alloy to obtain a first composite alloy.

[0029] In the above embodiment, carbonized rice husks, iron oxide and sodium fluoride are treated by a heating process to obtain a first mixture containing a first silicon carbide whisker structure, and by dissolving the sodium fluoride in the first silicon carbide whisker structure, a first silicon carbide whisker structure having a density less than that of the liquid aluminum alloy can be obtained, so that when the second mixture is placed in the liquid aluminum alloy, the first silicon carbide whisker structure floats on the upper layer of the liquid aluminum alloy, so that the first silicon carbide whisker structure is gathered on one side of the first composite alloy, so that when the first composite alloy is plated on a slider, an end cover or a slide rail, the side of the first composite alloy having the first silicon carbide whisker structure faces the outside, so that the portion of the first composite alloy with high comprehensive mechanical properties is located on the outside, and when the slider is impacted, rubbed or corroded, the portion of the first composite alloy with high comprehensive mechanical properties impacts, rubs against external objects or contacts corrosive substances, so as to prevent external objects or corrosive substances from penetrating the plating layer and damaging the guide rail, thereby improving the protection capability of the first composite alloy to the slider body. Moreover, compared with uniformly arranging the first silicon carbide whisker structure throughout the entire first composite alloy, the consumption of the second silicon carbide whisker structure can be reduced, thereby reducing the production cost of the first composite alloy.

[0030] In addition, the iron in the second mixture reacts with the aluminum to form an aluminum-iron alloy phase, so that the first composite alloy maintains its light weight while further improving its hardness, thereby preventing the coating from being rubbed off due to bumps.

[0031] In at least one embodiment, the step of treating carbonized rice husk, iron oxide and sodium fluoride by a heating process to obtain a first mixture containing a first silicon carbide whisker structure includes: reacting the carbonized rice husk, iron oxide and sodium fluoride at 1500-1850°C to obtain a first silicon carbide whisker structure, adding water to the first silicon carbide whisker structure and performing mechanical ball milling in a ball mill for 24 hours to obtain a first mixture.

[0032] By adding water to the first silicon carbide whisker structure and performing mechanical ball milling in a ball mill, part of the sodium fluoride in the first silicon carbide whisker structure is dissolved in water, thereby generating pores in the first silicon carbide whisker structure, so as to achieve lightweight while increasing specific surface area.

[0033] In at least one embodiment, the step of soaking the first mixture in water and dissolving sodium fluoride further comprises: soaking the first mixture in water by ultrasonic vibration.

[0034] In the above embodiment, the first mixture is immersed in water through ultrasonic vibration so that water can more easily penetrate into the interior of the first silicon carbide whisker structure, thereby facilitating the dissolution of sodium fluoride and accelerating the dissolution of sodium fluoride in the first silicon carbide whisker structure in the first mixture into water. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1It is a three-dimensional diagram of a guide rail in one embodiment of the present application.

[0036] Figure 2 for Figure 1 Exploded view of the middle slider.

[0037] Figure 3 A flow chart of a method for preparing a coating material provided in one embodiment of the present application.

[0038] Figure 4 A flow chart of a method for preparing another coating material provided in one embodiment of the present application.

[0039] Figure 5 A flow chart of a method for preparing another coating material provided in one embodiment of the present application.

[0040] Figure 6 A flow chart of a method for preparing a slider body material provided in one embodiment of the present application.

[0041] Main component symbols

[0042] Guide Rail 100

[0043] Slide 10

[0044] Slider 20

[0045] Slider body 21

[0046] Body layer 211

[0047] Hard layer 212

[0048] End cap 22

[0049] Ball 23

[0050] Coating 30 DETAILED DESCRIPTION

[0051] The technical solutions in the embodiments of the present application will be described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments.

[0052] It should be noted that when a component is considered to be "connected" to another component, it may be directly connected to the other component or there may be a central component at the same time. When a component is considered to be "located on" another component, it may be directly located on the other component or there may be a central component at the same time. The terms "top", "bottom", "upper", "lower", "left", "right", "front", "back", and similar expressions used herein are for illustrative purposes only.

[0053] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0054] An embodiment of the present application provides a coating layer, which is applied to a slider, and the coating layer includes an aluminum alloy and a first silicon carbide whisker structure. In terms of mass percentage, the aluminum alloy includes magnesium: 2-6%, zinc: 0.2-1%, silicon: 0.2-1%, rare earth elements: 0.1-0.5%, thallium: 1-5%, aluminum: 86.5-97.5% and impurity remainder.

[0055] In the above embodiment, by adding magnesium, zinc, tungsten and thallium to the aluminum matrix for making the coating, the strength of the coating can be increased while the corrosion resistance can be improved.

[0056] Some embodiments will be described below in conjunction with the accompanying drawings. In the absence of conflict, the following embodiments and features in the embodiments may be combined with each other.

[0057] Please refer to Figure 1 One embodiment of the present application provides a guide rail 100 for supporting, fixing and guiding a mobile device or equipment. The guide rail 100 includes a slide rail 10 and a slider 20. The slider 20 is disposed on the slide rail 10 and can reciprocate along the slide rail 10.

[0058] Please refer to Figure 2 The slider 20 includes a slider body 21 and a coating 30 , and the coating 30 is coated on the outer surface of the slider body 21 .

[0059] In one embodiment, the slider 20 further includes an end cover 22 , and a coating 30 is disposed on an outer surface of the end cover 22 .

[0060] In one embodiment, a coating 30 is disposed on the outer surface of the slide rail 10 .

[0061] In one embodiment, the outer surface of the slider body 21, the outer surface of the end cover 22, and the outer surface of the slide rail 10 may be the surface of the slider body 21, the end cover 22, and the slide rail 10 that does not contact the ball 23. It is understandable that in other embodiments, the outer surface of the slider body 21, the outer surface of the end cover 22, and the outer surface of the slide rail 10 may also be the surface in contact with the air, and even include the surface of the slider body 21, the end cover 22, and the slide rail 10 that contacts the ball 23, as long as it is a surface that needs to be prevented from corrosion.

[0062] In one embodiment, the coating 30 can be made into a thin sheet and attached to the outer surface of the slider body 21, the outer surface of the end cover 22 or the outer surface of the slide rail 10, or the coating 30 can be attached by immersing the slider body 21, the end cover 22 or the slide rail 10 in a molten state, as long as the coating 30 can be set on the outer surface of the slider body 21, the outer surface of the end cover 22 or the outer surface of the slide rail 10.

[0063] The coating 30 includes an aluminum alloy and a first silicon carbide whisker structure. In terms of mass percentage, the aluminum alloy includes magnesium: 2-6%, zinc: 0.2-1%, silicon: 0.2-1%, rare earth elements: 0.1-0.5%, thallium: 1-5%, aluminum: 86.5-97.5% and the remainder of impurities.

[0064] By adding magnesium, zinc, silicon, rare earth elements and thallium to the aluminum matrix of the coating layer 30 , the strength of the coating layer 30 can be increased while the corrosion resistance can be improved.

[0065] In one embodiment, adding 2-6% magnesium to aluminum can make the aluminum alloy have good strength, excellent corrosion resistance, and resistance to intergranular corrosion, exfoliation corrosion and stress corrosion. It can be understood that in other embodiments, the mass percentage of magnesium can be any mass percentage in the range of 2-6%. Moreover, the mass percentage of magnesium can be in the range between any two mass percentages in the range of 2-6%.

[0066] According to the aluminum alloy provided in the present application, the compositions of the comparative examples and experimental examples are shown in Table 1. Corrosion resistance tests and compressive strength tests were performed on the comparative examples and experimental examples in Table 1 to obtain the experimental results shown in Table 2.

[0067] The corrosion resistance test was carried out using the "GB 6459-1986 Acetate Salt Spray Test (ASS Test) Method for Metal Coverings".

[0068] The compressive strength test was carried out using GB / T7314-2017-Metallic Materials Room Temperature Compression Test Method.

[0069] Table 1 Chemical composition

[0070] Serial number magnesium Zinc silicon Rare Earth Elements thallium Comparative Example 1 1.0 0.1 0.15 0.08 0.9 Comparative Example 2 1.5 0.1 0.15 0.08 0.9 Example 1 2.0 0.1 0.15 0.08 0.9 Example 2 3.0 0.1 0.15 0.08 0.9 Example 3 4.0 0.1 0.15 0.08 0.9 Example 4 5.0 0.2 0.15 0.08 0.9 Example 5 6.0 1 0.15 0.08 0.9

[0071] Table 2 Experimental results

[0072]

[0073] As shown in Table 1 and Table 2, by comparing Examples 1-5 with Comparative Examples 1 and 2, it is found that when the mass percentage of magnesium reaches 2-6%, the strength and corrosion resistance of the aluminum alloy are significantly improved.

[0074] In one embodiment, adding 0.2-1% zinc to aluminum can form an aluminum + zinc + magnesium structure aluminum alloy, which has good strength, excellent corrosion resistance, and resistance to intergranular corrosion, exfoliation corrosion and stress corrosion. It can be understood that in other embodiments, the mass percentage of zinc can be any mass percentage in the range of 0.2-1%. Moreover, the mass percentage of zinc can be in the range between any two mass percentages in the range of 0.2-1%.

[0075] According to the aluminum alloy provided by the present application, the design of the comparative examples and experimental examples is shown in Table 3. Corrosion resistance tests and compressive strength tests were performed on the comparative examples and experimental examples in Table 3 to obtain the experimental results shown in Table 4.

[0076] The corrosion resistance test was carried out using the "GB 6459-1986 Acetate Salt Spray Test (ASS Test) Method for Metal Coverings".

[0077] The compressive strength test was carried out using GB / T7314-2017-Metallic Materials Room Temperature Compression Test Method.

[0078] Table 3 Chemical composition

[0079] Serial number magnesium Zinc silicon Rare Earth Elements thallium Comparative Example 1 2.0 0.1 0.15 0.08 0.9 Comparative Example 2 2.0 0.15 0.15 0.08 0.9 Example 1 2.0 0.20 0.15 0.08 0.9 Example 2 2.0 0.60 0.15 0.08 0.9 Example 3 2.0 1.0 0.15 0.08 0.9 Example 4 2.0 1.0 0.20 0.08 0.9 Example 5 2.0 1.0 1.0 0.08 0.9

[0080] Table 4 Experimental results

[0081]

[0082]

[0083] As shown in Table 3 and Table 4, by comparing Examples 1-5 with Comparative Examples 1 and 2, it is found that when the mass percentage of zinc reaches 0.2-1%, the strength and corrosion resistance of the aluminum alloy are significantly improved.

[0084] In one embodiment, 0.2-1% silicon is added to the aluminum alloy containing magnesium, and magnesium and silicon form a strengthening phase MgSi in the aluminum alloy to improve the strength of the aluminum alloy. It is understood that in other embodiments, the mass percentage of silicon can be any mass percentage in the range of 0.2-1%. Moreover, the mass percentage of silicon can be in the range between any two mass percentages in the range of 0.2-1%.

[0085] According to the aluminum alloy provided by the present application, the compositions of the comparative examples and experimental examples are shown in Table 5. Corrosion resistance tests and compressive strength tests were performed on the comparative examples and experimental examples in Table 5 to obtain the experimental results shown in Table 6.

[0086] The corrosion resistance test was carried out using the "GB 6459-1986 Acetate Salt Spray Test (ASS Test) Method for Metal Coverings".

[0087] The compressive strength test was carried out using GB / T7314-2017-Metallic Materials Room Temperature Compression Test Method.

[0088] Table 5 Chemical composition

[0089] Serial number magnesium Zinc silicon Rare Earth Elements thallium Comparative Example 1 2.0 0.20 0.10 0.08 0.9 Comparative Example 2 2.0 0.20 0.15 0.08 0.9 Example 1 2.0 0.20 0.20 0.08 0.9 Example 2 2.0 0.20 0.60 0.08 0.9 Example 3 2.0 0.20 1.0 0.08 0.9 Example 4 2.0 0.20 1.0 0.10 0.9 Example 5 2.0 0.20 1.0 0.50 0.9

[0090] Table 6 Experimental results

[0091]

[0092]

[0093] As shown in Table 5 and Table 6, by comparing Examples 1-5 with Comparative Examples 1 and 2, it is found that when the mass percentage of silicon reaches 0.2-1%, the strength of the aluminum alloy is significantly improved.

[0094] In one embodiment, 0.1-0.5% of rare earth elements are added to the aluminum alloy. Adding an appropriate amount of rare earth elements can improve the comprehensive mechanical properties of the aluminum alloy, such as the strength, hardness and wear resistance of the aluminum alloy. Among them, the rare earth elements include lanthanum, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, cerium, praseodymium, neodymium, erbium, thulium, ytterbium, lutetium, and two elements closely related to the 15 elements of the lanthanide series, scandium and yttrium, a total of 17 elements. Optionally, one or more of the rare earth elements can be added to the aluminum alloy according to specific production needs.

[0095] It is understood that in other embodiments, the mass percentage of one or more rare earth elements may be any mass percentage within the range of 0.1-0.5%. Furthermore, the mass percentage of one or more rare earth elements may be within the range between any two mass percentages within the range of 0.1-0.5%.

[0096] When used in an environment, especially when chloride ions are present, aluminum alloys are extremely susceptible to corrosion, crevice corrosion, stress corrosion, corrosion fatigue and other damage.

[0097] In one embodiment, a rare earth conversion film can be formed on the surface of the aluminum alloy by adding a rare earth multi-component infiltrant (La, Ce, etc.) by using a chemical vapor method, so that the surface electrode potential of the aluminum alloy tends to be uniform, and the resistance to intergranular corrosion and stress corrosion is improved. Adding La to the aluminum alloy can significantly improve the corrosion resistance of the aluminum alloy. Alternatively, adding Nd to the aluminum alloy can improve the high temperature performance and corrosion resistance of the aluminum alloy, so that the aluminum alloy can be used in harsh environments.

[0098] According to the aluminum alloy provided by the present application, the design of the comparative examples and experimental examples is shown in Table 7. Corrosion resistance tests and compressive strength tests were performed on the comparative examples and experimental examples in Table 7 to obtain the experimental results shown in Table 8.

[0099] The corrosion resistance test was carried out using the "GB 6459-1986 Acetate Salt Spray Test (ASS Test) Method for Metal Coverings".

[0100] The compressive strength test was carried out using GB / T7314-2017-Metallic Materials Room Temperature Compression Test Method.

[0101] Table 7 Chemical composition

[0102]

[0103]

[0104] Table 8 Experimental results

[0105]

[0106] As shown in Table 7 and Table 8, by comparing Examples 1-5 with Comparative Examples 1 and 2, it is found that when the mass percentage of the rare earth element reaches 0.1-0.5%, the strength and corrosion resistance of the aluminum alloy are significantly improved.

[0107] In one embodiment, adding 1-5% thallium to the aluminum alloy can improve the strength of the aluminum alloy and enhance the corrosion resistance of the aluminum alloy. It is understood that in other embodiments, the mass percentage of thallium can be any mass percentage within the range of 1-5%. Moreover, the mass percentage of thallium can be a range between any two mass percentages within the range of 1-5%.

[0108] According to the aluminum alloy provided by the present application, the compositions of the comparative examples and experimental examples are shown in Table 9. Corrosion resistance tests and compressive strength tests were performed on the comparative examples and experimental examples in Table 9 to obtain the experimental results shown in Table 10.

[0109] The corrosion resistance test was carried out using the "GB 6459-1986 Acetate Salt Spray Test (ASS Test) Method for Metal Coverings".

[0110] The compressive strength test was carried out using GB / T7314-2017-Metallic Materials Room Temperature Compression Test Method.

[0111] Table 9 Chemical composition

[0112] Serial number magnesium Zinc silicon Rare Earth Elements thallium Comparative Example 1 2.0 0.20 0.20 0.1 0.5 Comparative Example 2 2.0 0.20 0.20 0.1 0.9 Example 1 2.0 0.20 0.20 0.1 1.0 Example 2 2.0 0.20 0.20 0.1 2.0 Example 3 2.0 0.20 0.20 0.1 3.0 Example 4 2.0 0.20 0.20 0.1 4.0 Example 5 2.0 0.20 0.20 0.1 5.0

[0113] Table 10 Experimental results

[0114]

[0115] As shown in Table 9 and Table 10, by comparing Examples 1-5 with Comparative Examples 1 and 2, it is found that when the mass percentage of thallium reaches 1-5%, the strength and corrosion resistance of the aluminum alloy are significantly improved.

[0116] Please refer to Figure 3 , In one embodiment of the present application, a method for preparing the coating 30 material is also provided, comprising the following steps: The following steps are all performed under inert gas conditions;

[0117] S310, heating the aluminum alloy to a molten state to obtain a liquid aluminum alloy;

[0118] S320, treating carbonized rice husk, iron oxide and sodium fluoride through a heating process to obtain a first mixture containing a first silicon carbide whisker structure;

[0119] S330, soaking the first mixture in water and dissolving sodium fluoride, repeating multiple times;

[0120] S340, adding aluminum powder to the first mixture after soaking in water and reacting them sufficiently to obtain a second mixture; wherein the density of the first silicon carbide whisker structure in the second mixture is less than the density of the liquid aluminum alloy;

[0121] S350, adding the second mixture into the liquid aluminum alloy to obtain a first composite alloy.

[0122] In one embodiment, the aluminum alloy is the aluminum alloy in any of the above embodiments, and thus has all the beneficial effects of the above aluminum alloys, which will not be described in detail herein.

[0123] In one embodiment, the inert gas may be one or more of helium, neon, argon, krypton, xenon, radon and austenite.

[0124] In one embodiment, the preparation process of carbonized rice husk is:

[0125] After soaking the rice husk in water, it is frozen and crushed to obtain rice husk fibers of 100-600nm. Under the protection of inert gas, the rice husk fibers of 100-600nm are heated to 350-400℃ at a heating rate of 0.1-0.5℃ / min, and then carbonized for 3-5h. Then, the temperature is further increased to 550-650℃ at a rate of 0.6-0.8℃ / min, and then carbonized for 3-5h. Then, the temperature is further increased to 1450-1550℃ at a rate of 6-12℃ / min, and then the temperature is kept for 2-4h, and then cooled to obtain carbonized rice husk.

[0126] Please refer to Figure 4 , step S320 includes:

[0127] S321, carbonized rice husk, iron oxide and sodium fluoride are reacted at 1500-1850° C. to obtain a first silicon carbide whisker structure;

[0128] S322, adding water to the first silicon carbide whisker structure, and performing mechanized ball milling in a ball mill for 24 hours to obtain a first mixture.

[0129] In one embodiment, the carbonized rice husk, iron oxide and sodium fluoride are placed at 1500-1850° C., so that the sodium fluoride and iron oxide catalyze the reaction between silicon dioxide and carbon in the carbonized rice husk to generate a first silicon carbide whisker structure.

[0130] After the first silicon carbide whisker structure is cooled, water is added to the first silicon carbide whisker structure and mechanical ball milling is performed in a ball mill for 24 hours to obtain a first mixture with a grain size of 100-600 nm. In this process, part of the sodium fluoride of the first silicon carbide whisker structure in the first mixture is dissolved in water, so that pores are generated in the first silicon carbide whisker structure, thereby achieving lightweight while increasing specific surface area.

[0131] Then, the first mixture is placed in water at 10-100° C. for 1-2 hours, and the process is repeated multiple times to dissolve most of the sodium fluoride of the first silicon carbide whisker structure in the first mixture in the water, further increasing the specific surface area of ​​the first silicon carbide whisker structure, so that the density of the first silicon carbide whisker structure is less than the density of the aluminum alloy in the molten state. At this time, the first mixture contains iron oxide, the first silicon carbide whisker structure with a large specific surface area, and a small amount of sodium fluoride.

[0132] Please refer to Figure 5 , step S330 also includes: S331, soaking the first mixture in water through ultrasonic vibration.

[0133] In one embodiment, when the first mixture is placed in water, ultrasonic waves of 40 to 75 kHz are used to make it easier for water to penetrate into the interior of the first silicon carbide whisker structure, thereby facilitating the dissolution of sodium fluoride and accelerating the dissolution of sodium fluoride in the first silicon carbide whisker structure in the first mixture into water.

[0134] After the first mixture is soaked in water and water is removed, aluminum powder is added and fully reacted, that is, the aluminum powder reacts with iron oxide to generate iron to obtain a second mixture, which contains iron, a first silicon carbide whisker structure with a larger specific surface area and a small amount of sodium fluoride.

[0135] The second mixture is placed in a liquid aluminum alloy to obtain a first composite alloy.

[0136] Since the specific surface area of ​​the first silicon carbide whisker structure is relatively large, after the second mixture is placed in the liquid aluminum alloy, the first silicon carbide whisker structure will float on the upper layer of the liquid aluminum alloy, so that after the liquid aluminum alloy is formed, the first silicon carbide whisker structure is concentrated on one side of the aluminum alloy, so that one side of the first composite alloy has the first silicon carbide whisker structure, so that when the first composite alloy is plated on the slider 20, the end cover 22 or the slide rail 10, the side of the first composite alloy having the first silicon carbide whisker structure faces the outside, so that the part with high comprehensive mechanical properties in the first composite alloy is located on the outside, and when the slider 20 is impacted, rubbed or corroded, the part with high comprehensive mechanical properties in the first composite alloy impacts, rubs against external objects or contacts corrosive substances, so as to prevent external objects or corrosive substances from passing through the first composite alloy to damage the slider body 21, thereby improving the protection capability of the first composite alloy to the slider body 21. In addition, compared with uniformly arranging the first silicon carbide whisker structure in the entire first composite alloy, the consumption of the second silicon carbide whisker structure can be reduced, thereby reducing the manufacturing cost of the coating 30.

[0137] In addition, the iron in the second mixture reacts with the aluminum to form an aluminum-iron alloy phase, so that the first composite alloy maintains its light weight while further improving its hardness, thereby preventing the coating 30 from being rubbed off due to bumps.

[0138] It should be noted that specific surface area refers to the total area of ​​a material per unit mass, including the external surface area and the internal surface area. An ideal non-porous material only has an external surface area; a porous and multi-porous material has both an external surface area and an internal surface area.

[0139] In one embodiment, when water is added to the first silicon carbide whisker structure and ground in a ball mill, aluminum powder is added so that the aluminum powder and iron oxide can fully react. The heat generated by the reaction of the aluminum powder and iron oxide can increase the amount of sodium fluoride dissolved in water, so as to quickly remove the sodium fluoride on the first silicon carbide whisker structure in the first mixture.

[0140] In one embodiment, the mass of the carbonized rice husk is 2-15% of the mass of the aluminum alloy matrix. It is understood that in other embodiments, the mass percentage of the carbonized rice husk can be any mass percentage within the range of 2-15%. Moreover, the mass percentage of the carbonized rice husk can be within the range between any two mass percentages within the range of 2-15%.

[0141] In one embodiment, the mass of sodium fluoride is 0.5-5% of the mass of carbonized rice husk. It is understood that in other embodiments, the mass percentage of sodium fluoride can be any mass percentage within the range of 0.5-5%. Moreover, the mass percentage of sodium fluoride can be within the range between any two mass percentages within the range of 0.5-5%.

[0142] In one embodiment, the mass of the iron oxide is 1%-5% of the mass of the carbonized rice husk. It is understood that in other embodiments, the mass percentage of the iron oxide can be any mass percentage within the range of 1%-5%. Moreover, the mass percentage of the iron oxide can be within the range between any two mass percentages within the range of 1%-5%.

[0143] Please refer to Figure 2 The slider body 21 includes a body layer 211 and a hardened layer 212 . The body layer 211 is connected to the hardened layer 212 , and the body layer 211 and the hardened layer 212 are arranged in layers. The hardened layer 212 is provided with a roller channel for assembling the ball 23 .

[0144] In one embodiment, the surfaces of the body layer 211 and the hardened layer 212 in contact with air are coated with the coating 30, even including the surface of the hardened layer 212 in contact with the ball 23. It is understandable that in other embodiments, the surface of the hardened layer 212 in contact with the ball 23 may not be coated with the coating 30.

[0145] In one embodiment, the hardened layer 212 includes a second silicon carbide whisker structure, which is used to enhance the comprehensive mechanical properties of the hardened layer 212, such as high hardness, wear resistance, high temperature resistance and corrosion resistance, so as to reduce the wear of the hardened layer 212 by the ball 23, the corrosion of the hardened layer 212 by the lubricating oil, and the influence of the high temperature generated by the friction of the ball 23 in the hardened layer 212 on the hardened layer 212.

[0146] Please refer to Figure 6 In one embodiment of the present application, a method for preparing the material of the slider body 21 is also provided, comprising the following steps:

[0147] S410, uniformly mixing the prefabricated tungsten steel alloy powder and the prefabricated second silicon carbide whisker structure powder, cold compacting the mixture, and gradually heating and degassing the mixture under the first preset condition to obtain a mixture;

[0148] S420, under the second preset condition, the mixture and the tungsten steel alloy are layered and vacuum sintered for 1-10 hours, and processed by a hot pressing process to obtain a second composite alloy.

[0149] A mixture obtained by compacting a prefabricated tungsten steel alloy powder and a prefabricated second silicon carbide whisker structure powder is layered with a tungsten steel alloy and sintered and hot-pressed to obtain a second composite alloy with high local hardness, wear resistance and corrosion resistance, that is, the mixture forms a hardened layer 212 with high hardness, wear resistance and corrosion resistance, the tungsten steel alloy forms the main body layer 211, and the hardened layer 212 and the main body layer 211 are an integrally formed structure, so that the hardened layer 212 does not fail under long-term cooperation with the ball 23, and a part of the hardened layer 212 is replaced by the main layer, thereby reducing the consumption of the second silicon carbide whisker structure, thereby improving the performance of the slider body 21 while reducing the consumption of the second silicon carbide whisker structure, thereby reducing the manufacturing cost of the slider body 21.

[0150] In one embodiment, a prefabricated tungsten steel alloy powder and a prefabricated second silicon carbide whisker structure powder are uniformly mixed by a mechanical mixing method, and the mixed powder is cold compacted and then gradually heated and degassed under a first preset condition.

[0151] In one embodiment, the first preset condition is 10 -5 -10 -8 It is understandable that, in other embodiments, the range of the first preset condition may be 10 -5 -10 -8 Any value in the range. And the range of the first preset condition can be 10 -5 -10 -8 The range between any two mass percentages within the range.

[0152] In one embodiment, vacuum sintering is performed for 1-10 hours under the second preset condition, and the hot pressed ingot is extruded in a mold at 1200-1300° C. to obtain a second composite alloy, so as to manufacture the hardened layer 212 of the slider body 21 through the second composite alloy.

[0153] In one embodiment, the second preset condition is 1450-1500°C and 50-200Mpa. It is understood that in other embodiments, the range of the second preset condition can be any value in the range of 1450-1500°C and any value in the range of 50-200Mpa. In addition, the range of the second preset condition can be a range between any two mass percentages in the range of 1450-1500°C and a range between any two mass percentages in the range of 50-200Mpa.

[0154] In one embodiment, the preparation process of the second silicon carbide whisker structure is:

[0155] Prepare materials (by mass ratio): 46.6-50.8 silicon, 45.5-51.8 carbon, 0.2-0.8 manganese and 0.9-7.1 sodium carbide. The above materials are uniformly mixed by mechanical mixing to obtain composite powder, and then anhydrous ethanol is added to the composite powder and mechanically ball-milled in a ball mill for 24 hours to obtain a composite powder with a grain size of 100-600nm. Finally, the ultrafine composite powder is loaded into a graphite container and synthesized under inert gas conditions and 1500℃-1550℃ for 2-4h.

[0156] In other embodiments, when preparing the second silicon carbide whisker structure, titanium dioxide may be added to increase the toughness of the second silicon carbide whisker structure.

[0157] In one embodiment, adding niobium powder to the second silicon carbide whisker structure powder can improve the stability of the second composite alloy at high temperatures, thereby improving the stability of the hardened layer 212 .

[0158] In addition, those skilled in the art should recognize that the above embodiments are only used to illustrate the present application, and are not intended to limit the present application. As long as they are within the spirit of the present application, appropriate changes and modifications to the above embodiments are within the scope of the present application.

Claims

1. A method for preparing a coating material, It is characterized in that The following steps are involved: The following steps are all carried out under inert gas conditions; The aluminum alloy is heated to a molten state to obtain the liquid aluminum alloy, wherein the aluminum alloy comprises, by mass percentage, 2-6% magnesium, 0.2-1% zinc, 0.2-1% silicon, 0.1-0.5% rare earth elements, 1-5% thallium, 86.5-97.5% aluminum and the remainder of impurities; treating carbonized rice husk, iron oxide and sodium fluoride through a heating process to obtain a first mixture containing a first silicon carbide whisker structure; Soaking the first mixture in water to dissolve the sodium fluoride, repeating the process multiple times; Adding aluminum powder to the first mixture after soaking in water and reacting them sufficiently to obtain a second mixture; wherein the density of the first silicon carbide whisker structure in the second mixture is less than the density of the liquid aluminum alloy; The second mixture is added to the liquid aluminum alloy to obtain a coating, wherein the coating includes the aluminum alloy and a first silicon carbide whisker structure bonded to one side of the aluminum alloy.

2. The preparation method as claimed in claim 1, It is characterized in that The step of treating carbonized rice husk, iron oxide and sodium fluoride by a heating process to obtain a first mixture containing a first silicon carbide whisker structure comprises: The carbonized rice husk, iron oxide and sodium fluoride are reacted at 1500-1850° C. to obtain a first silicon carbide whisker structure; Water is added to the first silicon carbide whisker structure and the mixture is mechanically ball-milled in a ball mill for 24 hours to obtain a first mixture.

3. The preparation method as claimed in claim 1, It is characterized in that The step of soaking the first mixture in water and dissolving the sodium fluoride further includes: soaking the first mixture in water through ultrasonic vibration.