A device and method for detecting cold welds in welding components and welding structures

By setting detection grooves or channels on the welded parts to determine their sealing properties, the problem of difficult control of the welding penetration is solved, and the accuracy of the virtual welding detection and the improvement of the welding quality are achieved.

CN115990729BActive Publication Date: 2024-10-11CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111214268.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-19
Publication Date
2024-10-11
Estimated Expiration
2041-10-19

AI Technical Summary

Technical Problem

The welding penetration is difficult to control in the existing welding methods, resulting in possible virtual welding between the welded parts, affecting the conductivity and performance.

Method used

A welding component for virtual welding detection is designed, which includes setting a detection groove or detection channel on the second welding part, and judging whether the penetration depth reaches the predetermined requirement through the sealing of the detection groove or channel, and providing equipment and methods for virtual welding detection. .

Benefits of technology

By testing the sealing of grooves or channels, it can be accurately determined whether there is a virtual welding phenomenon between welded parts, thereby improving welding quality and product yield.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115990729B_ABST
    Figure CN115990729B_ABST
Patent Text Reader

Abstract

The present application provides a welding assembly, welding structure, equipment and method for detecting cold welds, wherein the welding assembly includes a first welding part and a second welding surface, wherein the second welding part is provided with a detection groove and / or a detection channel, wherein the detection groove and / or the detection channel extend from the detection port to the edge of the second welding part, wherein the detection groove is provided on the second welding surface, and the detection channel is provided inside the second welding part and communicated with the detection port. After the welding of the first welding part and the second welding part is completed, a connection can be established between the sealing detection device and the detection port to determine whether the current detection groove and / or the detection channel are completely blocked by the molten pool along the cross-sectional direction, and then the sealing detection result of the detection groove and / or the detection channel after fusion welding is used to determine whether there is a cold weld between the first welding part and the second welding part, thereby improving the product yield.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of welding technology, and in particular to a welding assembly and a welding structure for detecting cold welds, and a device and method for detecting cold welds. Background Art

[0002] Welding, also known as fusion welding, is a manufacturing process and technology that joins metals or other thermoplastic materials such as plastics by heating, high temperature or high pressure. Fusion welding is an important type of welding. It heats the workpieces to be joined to partially melt them to form a molten pool. When the molten pool cools and solidifies, the materials are joined. Fusion welding can be assisted by adding molten fillers when necessary. It is suitable for welding various metals and alloys.

[0003] At present, the existing welding methods often have the problem of difficult to control welding penetration. If the welding penetration is too large, one of the welded parts will be directly burned through. If the welding penetration is too small, there may be a cold weld between the two welded parts, affecting the electrical conductivity between the two, resulting in a decrease in the performance of the welded assembly after welding. Summary of the invention

[0004] To this end, it is necessary to provide a welding assembly, welding structure, equipment and method for detecting cold welds to solve the technical problems of existing welding methods that the depth of penetration is difficult to control and the existence of cold welds between welded parts cannot be detected.

[0005] In a first aspect, the present application provides a welding assembly for detecting cold welds, comprising: a first welding part, having a first welding surface, the first welding surface being provided with a detection through hole penetrating the first welding part; a second welding part, having a second welding surface, the second welding surface being welded and adapted to the first welding surface, a detection port being provided on the second welding surface, the position of the detection port corresponding to the position of the detection through hole; the second welding part is also provided with a detection groove and / or a detection channel, the detection groove and / or the detection channel extending from the detection port to the edge of the second welding part, the detection groove being provided on the second welding surface, the detection channel being arranged inside the second welding part and connected to the detection port.

[0006] The above technical solution is to open a detection groove on the second welding surface of the second welding part or set a detection channel inside the second welding part, and set a detection port on the second welding part. The position of the detection port corresponds to the position of the detection through hole. During the fusion welding process, the molten pool formed by the first welding part will enter the detection groove and / or the detection channel. If the detection groove and / or the detection channel are completely blocked by the molten pool along the cross-sectional direction, it means that the depth of fusion between the first welding part and the second welding part reaches the predetermined requirement, and the welding of the first welding part and the second welding part is qualified; on the contrary, if the detection groove and / or the detection channel are not completely blocked by the molten pool along the cross-sectional direction at this time, it means that the depth of fusion between the first welding part and the second welding part does not reach the predetermined requirement, and there is a cold weld between the first welding part and the second welding part. Since the detection groove and / or detection channel extends from the detection port to the edge of the second welding part, it is possible to establish a connection between the sealing detection equipment and the detection port to determine whether the current detection groove and / or detection channel is completely blocked by the molten pool along the cross-sectional direction, and then determine whether there is a cold weld between the first welding part and the second welding part based on the sealing detection result of the detection groove and / or detection channel after fusion welding, that is, determine whether the current fusion depth reaches the groove depth of the detection groove or the depth requirement of the detection channel from the second welding surface.

[0007] As an embodiment of the present application, the number of detection slots and / or detection channels is more than 2. Usually, the first weldment and the second weldment are welded at multiple points, so it is necessary to cover as many positions in the welding area of ​​the two as possible during the cold weld detection. By setting more than 2 detection slots and / or detection channels, it is possible to perform cold weld detection on multiple positions on the welding area after the first weldment and the second weldment are welded, thereby improving the coverage of the cold weld detection between the first weldment and the second weldment, and further improving the accuracy of the cold weld detection between the first weldment and the second weldment.

[0008] As an embodiment of the present application, the detection grooves and / or detection channels are arranged radially, and the detection port is located at the radial center of the radial shape. Usually, the weld between the first weld part and the second weld part is annular. When detecting the cold weld after the welding is completed, by judging the sealing of each detection groove and / or detection channel, it can be judged whether each detection groove and / or detection channel has been completely blocked by the molten pool. If each detection groove and / or detection channel has been completely blocked by the molten pool, it can be inferred that the welding between the first weld part and the second weld part is qualified, otherwise it means that there is a cold weld phenomenon at least in a certain position on the welding area between the first weld part and the second weld part. By arranging the detection grooves and / or detection channels in a radial shape and setting the detection port at the radial center of the radial shape, the judgment of the cold weld detection can cover all welding areas between the first weld part and the second weld part as much as possible, thereby improving the accuracy of the judgment of the cold weld detection.

[0009] As an implementation mode of the present application, the groove depth of the detection groove is 0.2-2.0mm. In the actual production and processing process, there are often certain requirements for the penetration depth of the first weldment and the second weldment after welding. By setting the groove depth of the detection groove to 0.2-2.0mm, it can be ensured that when the penetration depth reaches 0.2-2.0mm, the molten pool will completely block the detection groove, that is, only when the penetration depth reaches 0.2-2.0mm, the sealing of the detection groove after the welding of the first weldment and the second weldment is good, that is, the welding between the first weldment and the second weldment is qualified, thereby avoiding the first weldment and the second weldment. At the same time, the welding penetration requirements for the first weldment and the second weldment are relatively small, and the welding penetration can be effectively controlled by the depth of the groove depth of the detection groove to meet the needs of the actual production process.

[0010] As an implementation mode of the present application, the depth of the detection channel from the second welding surface is 3-5mm. In the actual production and processing process, there are often different requirements for the depth of penetration between different first welding parts and second welding parts. By setting the depth of the detection channel from the second welding surface to 3-5mm, it can be ensured that when the depth of penetration reaches 3-5mm, the molten pool will completely block the detection channel, that is, only when the depth of penetration reaches 3-5mm, the sealing of the detection channel is good after the welding of the first welding part and the second welding part, that is, the welding between the first welding part and the second welding part is qualified, so that while avoiding the first welding part and the second welding part from having a cold weld, when the welding depth of the first welding part and the second welding part is relatively large, the depth of the detection channel from the second welding surface can be used to effectively control the welding depth, so as to meet the needs of the actual production process.

[0011] As an implementation mode of the present application, the first welding part is an electrode connecting piece, and the second welding part is a battery cell pole. In the field of battery production and processing, it is necessary to weld the electrode connecting piece to the battery cell pole of the battery cell top cover to achieve a conductive connection between the battery cell and external components. If the welding depth between the electrode connecting piece and the battery cell pole is not enough, it will affect the subsequent performance of the battery cell. The present application provides a detection groove on the second welding surface of the battery cell pole or sets a detection channel inside the second welding part, and sets a detection port on the battery cell pole corresponding to the position of the detection through hole on the electrode connecting piece. After the fusion welding is completed, the sealing of the detection groove and / or the detection channel can be judged to determine whether there is a cold welding phenomenon between the electrode connecting piece and the battery cell pole. If there is a cold welding phenomenon, the electrode connecting piece and the battery cell pole after welding can be further processed to improve the product yield.

[0012] In a second aspect, the present application provides a welding structure, including: a first welding part, having a first welding surface, the first welding surface being provided with a detection through hole penetrating the first welding part; a second welding part, having a second welding surface, the second welding surface being welded to the first welding surface, a detection port being provided on the second welding surface, the position of the detection port corresponding to the position of the detection through hole, the second welding part is also provided with a detection groove and / or a detection channel, the detection groove and / or the detection channel extending from the detection port to the edge of the second welding part, the detection groove being provided on the second welding surface, the detection channel being arranged inside the second welding part and being connected to the detection port; part or all of the detection groove and / or the detection channel is blocked by a molten pool generated by welding.

[0013] In the actual production and processing process, the first welded part and the second welded part are often reprocessed or used after welding is completed, and how to timely detect whether there is a cold weld between the first welded part and the second welded part after welding is completed has always been a difficult problem. The difference between the welding structure in this embodiment and the welding assembly for cold weld detection in the first aspect of the present application is that the welding structure refers to the structure formed after the first welded part and the second welded part are welded, which is manifested as part or all of the detection grooves and / or detection channels on the second welded part being blocked by the molten pool generated by welding. When all the inspection grooves and / or inspection channels on the second welded part are blocked by the molten pool produced by welding, it means that all the inspection grooves and / or inspection channels on the second welded part of the welding structure are well sealed, that is, the welding of the first welded part and the second welded part in the welding structure is qualified; when part of the inspection grooves and / or inspection channels on the second welded part are blocked by the molten pool produced by welding, it means that part of the inspection grooves and / or inspection channels on the second welded part of the welding structure are well sealed, that is, the first welded part and the second welded part in the welding structure are well sealed in the welding area where the part of the inspection grooves and / or inspection channels are located, the welding of the first welded part and the second welded part in this part of the area is qualified, and there is no cold welding phenomenon.

[0014] As an embodiment of the present application, the number of detection grooves and / or detection channels is more than 2. Usually, the first weldment and the second weldment are welded at multiple points, so it is necessary to cover as many positions in the welding area of ​​the two as possible during the cold weld detection. By setting more than 2 detection grooves and / or detection channels, it can be ensured as much as possible that the welding penetration between the first weldment and the second weldment in the welding structure reaches the predetermined requirements at multiple positions in the welding area, that is, there are more than 2 detection grooves and / or detection channels blocked by the molten pool.

[0015] As an embodiment of the present application, the detection grooves and / or detection channels are arranged radially, and the detection port is located at the radial center of the radial shape. Usually, in a welding structure, the weld between the first welding part and the second welding part is annular. By arranging the detection grooves and / or detection channels radially, and arranging the detection port at the radial center of the radial shape, as many detection grooves and / or detection channels as possible on the second welding part in the welding structure can be blocked by the molten pool, thereby effectively reducing the phenomenon of cold welding in the welding structure obtained by welding.

[0016] As an implementation mode of the present application, the groove depth of the detection groove is 0.2-2.0mm. In the actual production and processing process, there are often certain requirements for the penetration depth between the first welding part and the second welding part in the welding structure. By setting the groove depth of the detection groove to 0.2-2.0mm, it can be ensured that when the penetration depth between the first welding part and the second welding part in the welding structure reaches at least 0.2-2.0mm, the molten pool will completely block part or all of the detection groove, that is, only when the penetration depth of the first welding part and the second welding part reaches 0.2-2.0mm, the detection groove on the second welding part in the welding structure is good during the sealing test. When the welding penetration requirements of the first welding part and the second welding part are relatively small, the welding penetration between the first welding part and the second welding part in the welding structure can be effectively controlled by setting the depth of the groove depth of the detection groove. When the welding penetration between the first welding part and the second welding part does not meet the predetermined requirements, that is, the molten pool in the welding process does not completely block the detection groove, it can be judged whether there is a cold weld in the welding structure by testing the sealing of the detection through hole connected to the detection groove.

[0017] As an implementation mode of the present application, the depth of the detection channel from the second welding surface is 3-5mm. In the actual production and processing process, there are often certain requirements for the penetration depth between the first welding part and the second welding part in the welding structure. By setting the groove depth of the detection channel to 3-5mm, it can be ensured that when the penetration depth between the first welding part and the second welding part in the welding structure reaches at least 3-5mm, the molten pool will completely block part or all of the detection channel, that is, only when the penetration depth of the first welding part and the second welding part reaches 3-5mm, the detection channel on the second welding part in the welding structure is good during the sealing test. When the welding penetration requirements of the first welding part and the second welding part are relatively large, the welding penetration between the first welding part and the second welding part in the welding structure can be effectively controlled by setting the depth of the groove depth of the detection channel from the second welding surface. When the welding penetration between the first welding part and the second welding part does not meet the predetermined requirements, that is, the molten pool in the welding process does not completely block the detection channel, it can be determined whether there is a cold weld in the welding structure by testing the sealing of the detection through hole connected to the detection channel.

[0018] As an embodiment of the present application, the first welding piece is an electrode connecting piece, and the second welding piece is a battery cell pole. In the field of battery production and processing, it is necessary to weld the electrode connecting piece to the battery cell pole of the battery cell top cover to achieve a conductive connection between the battery cell and external components. If the welding penetration between the electrode connecting piece and the battery cell pole is not enough, it will affect the subsequent performance of the battery cell. The present application provides a detection groove on the second welding surface of the battery cell pole or sets a detection channel inside the second welding piece, and sets a detection port corresponding to the position of the detection through hole on the electrode connecting piece on the battery cell pole. In the welding structure after fusion welding, part or all of the detection groove and / or detection channel are blocked by the molten pool generated by welding. When the welding of the first welding piece and the second welding piece in the welding structure does not meet the predetermined requirements, it can be judged by detecting the sealing of the detection through hole connected to the detection groove and / or detection channel, and then the welding structure with cold welding is screened out for processing, so as to improve the product yield.

[0019] In the third aspect, the present application provides a device for detecting cold welds, the device comprising: a positive pressure generating device or a negative pressure generating device; a detection pipeline, one end of which is connected to the positive pressure generating device or the negative pressure generating device; a detection head, which is connected to the other end of the detection pipeline, and the detection head has a connection structure that is airtightly connected to the detection through hole on the surface of the weld; and an air pressure detector, which is connected to the detection pipeline and is used to detect air pressure.

[0020] When using the equipment for detecting cold welds, the detection head can be tightly connected to the detection through hole first, and then the positive pressure generating device or the negative pressure generating device can be turned on. The positive pressure generating device or the negative pressure generating device provides positive pressure or negative pressure to the detection through hole through the detection pipeline. If the first welding part and the second welding part are welded qualified after the welding is completed, that is, the detection groove and / or the detection channel are completely blocked by the molten pool, during the detection process, the fluid will not flow out of the detection groove and / or the detection channel from the detection port to the outside world, or will not flow into the detection port from the outside world through the detection groove and / or the detection channel. At this time, the air pressure in the detection pipeline detected by the air pressure detector will not change significantly in a short period of time; otherwise If there is a cold weld between the first weld part and the second weld part after welding is completed, that is, the detection groove and / or the detection channel is not completely blocked by the molten pool, during the detection process, the fluid will flow out of the detection groove and / or the detection channel from the detection port to the outside or flow into the detection port from the outside through the detection groove and / or the detection channel. At this time, the air pressure in the detection pipeline detected by the air pressure detector will change significantly in a short period of time. By judging the air pressure change value detected by the air pressure detector, it can be determined whether there is a cold weld between the first weld part and the second weld part after welding is completed, and then the welding structure with cold welds can be screened out for processing to improve the product yield.

[0021] In the fourth aspect, the present application provides a method for detecting a cold weld, comprising the following steps: welding a first welding surface of a first welding part to a second welding surface of a second welding part, a detection through hole penetrating the first welding part is provided on the first welding surface, a detection port is provided on the second welding surface, the position of the detection port corresponds to the position of the detection through hole, the second welding part is also provided with a detection groove and / or a detection channel, the detection groove and / or the detection channel extend from the detection port to the edge of the second welding part, the detection groove is provided on the second welding surface, the detection channel is provided inside the second welding part and is connected to the detection port; the sealing of the detection through hole is detected to determine whether there is a cold weld. Through the above-mentioned method for detecting a cold weld, it is possible to determine whether there is a cold weld phenomenon between the first welding part and the second welding part after welding is completed, and then the welding structure with a cold weld can be screened out for processing to improve the product yield.

[0022] As an implementation mode of the present application, testing the sealing of the detection through hole specifically includes: applying positive pressure or negative pressure to the detection through hole to detect its sealing. When a positive pressure is applied to the detection through hole, if there is a cold weld phenomenon between the first welding part and the second welding part after welding, that is, the detection groove and / or the detection channel are not completely blocked by the molten pool, the fluid will flow out of the detection through hole from the detection groove and / or the detection channel to the edge of the second welding part, and by testing the sealing of the detection through hole, it can be determined whether there is a cold weld phenomenon between the first welding part and the second welding part after welding. When a negative pressure is applied to the detection through hole, if there is a cold weld phenomenon between the first welding part and the second welding part after welding, that is, the detection groove and / or the detection channel are not completely blocked by the molten pool, the fluid will flow from the edge of the second welding part through the detection groove and / or the detection channel into the detection through hole, and by testing the sealing of the detection through hole, it can be determined whether there is a cold weld phenomenon between the first welding part and the second welding part after welding.

[0023] As an implementation mode of the present application, applying positive pressure or negative pressure to the detection through hole to detect its sealing specifically includes: applying positive pressure or negative pressure to the detection through hole through a closed fluid system, stopping the pressure change, and then observing the pressure change of the closed fluid system within a preset time. If the pressure change of the closed fluid system within the preset time is less than the preset value, it is judged that the welding is qualified, otherwise it is judged that there is a cold weld. By comparing the pressure change of the closed fluid system within the preset time with the preset value, the sealing of the detection through hole can be accurately judged to determine whether there is a cold weld phenomenon, and then the welding structure with cold welds can be screened out for processing to improve the product yield.

[0024] As an implementation mode of the present application, the sealing of the detection through hole is tested with gas or liquid as the medium. If the welding is qualified, the molten pool completely blocks the detection groove and / or the detection channel. At this time, the flow path of the gas or liquid is blocked by the molten pool, and the detection groove and / or the detection channel will not change significantly within the predetermined time, indicating that the sealing of the detection through hole is good; if there is a cold weld, the molten pool does not completely block the detection groove and / or the detection channel, and the gas or liquid will flow out of the edge of the second welded part through the detection groove and / or the detection channel, and the detection groove and / or the detection channel will change significantly within the predetermined time, indicating that the sealing of the detection through hole is poor. By introducing gas or dripping liquid, accurate detection of the sealing of the detection through hole can be achieved, and the accuracy of judging whether there is a cold weld can be improved.

[0025] The above description is only an overview of the technical solution of the present application. In order to more clearly understand the technical means of the present application, it can be implemented in accordance with the contents of the specification. In order to make the above and other purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are listed below. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 A cross-sectional view of a welding assembly for detecting a cold weld according to an embodiment of the present application;

[0027] Figure 2 A cross-sectional view of a welding assembly for detecting a cold weld according to another embodiment of the present application;

[0028] Figure 3 This is a schematic structural diagram of a second welding member involved in an embodiment of the present application;

[0029] Figure 4 This is a schematic structural diagram of a second welding member involved in another embodiment of the present application;

[0030] Figure 5 A cross-sectional view of a welding structure with qualified welding according to an embodiment of the present application;

[0031] Figure 6 A cross-sectional view of a welding structure with a cold weld according to an embodiment of the present application;

[0032] Figure 7 A cross-sectional view of a welding structure with qualified welding according to another embodiment of the present application;

[0033] Figure 8 A cross-sectional view of a welding structure with a cold weld according to another embodiment of the present application;

[0034] Fig. 9 A cross-sectional view of a device for detecting cold welds according to an embodiment of the present application detecting a welded structure with qualified welds;

[0035] Fig.10 A cross-sectional view of a device for detecting a cold weld according to an embodiment of the present application detecting a welding structure with a cold weld;

[0036] Fig.11 A cross-sectional view of a device for detecting cold welds according to an embodiment of the present application detecting a welded structure with qualified welds;

[0037] Fig.12 A cross-sectional view of a device for detecting a cold weld according to an embodiment of the present application detecting a welding structure with a cold weld;

[0038] Fig.13 A schematic diagram of the structure of a battery according to an embodiment of the present application;

[0039] Fig.14 This is a schematic structural diagram of a battery cell top cover according to an embodiment of the present application;

[0040] Fig.15 A top view of a battery cell top cover according to an embodiment of the present application;

[0041] Fig.16 This is a schematic structural diagram of a battery cell top cover according to another embodiment of the present application;

[0042] Fig.17 A top view of a battery cell top cover according to another embodiment of the present application;

[0043] Fig.18 The present invention is a flowchart of a method for detecting cold solder joints according to an embodiment of the present application.

[0044] Description of reference numerals:

[0045] 100. Battery cell top cover;

[0046] 200. Battery;

[0047] 1. The first welding part;

[0048] 10. First welding surface;

[0049] 101. Detect through holes;

[0050] 2. The second weldment;

[0051] 20. Second welding surface

[0052] 201, inspection port;

[0053] 21. Inspection tank;

[0054] 22. Detection channel;

[0055] 23. Molten pool;

[0056] 3. Testing equipment;

[0057] 31. Inspection pipeline;

[0058] 32. Detection head;

[0059] 33. Positive pressure generating device or negative pressure generating device. DETAILED DESCRIPTION

[0060] The following embodiments of the technical solution of the present application are described in detail in conjunction with the accompanying drawings. The following embodiments are only used to more clearly illustrate the technical solution of the present application, and are therefore only used as examples, and cannot be used to limit the scope of protection of the present application.

[0061] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions.

[0062] In the description of the embodiments of the present application, the technical terms "first", "second", etc. are only used to distinguish different objects, and cannot be understood as indicating or implying relative importance or implicitly indicating the number, specific order or primary and secondary relationship of the indicated technical features. In the description of the embodiments of the present application, the meaning of "multiple" is more than two, unless otherwise clearly and specifically defined.

[0063] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0064] In the description of the embodiments of the present application, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0065] In the description of the embodiments of the present application, the term "multiple" refers to more than two (including two). Similarly, "multiple groups" refers to more than two groups (including two groups), and "multiple pieces" refers to more than two pieces (including two pieces).

[0066] In the description of the embodiments of the present application, the technical terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, which are only for the convenience of describing the embodiments of the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the embodiments of the present application.

[0067] In the description of the embodiments of the present application, unless otherwise clearly specified and limited, technical terms such as "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the embodiments of the present application can be understood according to the specific circumstances.

[0068] In daily production processes, it is often necessary to weld two workpieces together. The inventors have noticed that the current welding method often uses laser welding. Laser welding has the problem of difficult control of welding penetration, which leads to insufficient penetration between welded parts after welding, which can easily lead to poor contact between welded parts during subsequent use, affecting performance. Alternatively, the penetration between welded parts after welding is too great, which may directly burn through the welded parts. In addition, the internal quality of the weld is difficult to detect and trace, affecting the yield of the processed and produced products.

[0069] like Figure 1 As shown, in order to solve the technical problem that it is difficult to control the penetration depth of the weld during the welding process, resulting in the phenomenon of cold welding in the welding structure after welding, which affects the product yield, in the first aspect, the present application provides a welding assembly for cold welding detection, including a first welding part 1 and a second welding part 2, the first welding part 1 having a first welding surface 10, and the first welding surface 10 is provided with a detection through hole 101 that penetrates the first welding part 1; the second welding part 2 has a second welding surface 20, the second welding surface 20 is welded and adapted to the first welding surface 10, and the second welding surface 20 is provided with a detection port 201, and the position of the detection port 201 corresponds to the position of the detection through hole 101; the second welding part 2 is also provided with a detection groove 21, the detection groove 21 is opened on the second welding surface 20, and extends from the detection port 201 to the edge of the second welding part 2.

[0070] During the fusion welding process, the molten pool 23 formed during the welding process will enter the detection groove 21. If the detection groove 21 is completely blocked by the molten pool 23, it means that the fusion depth between the first welding part 1 and the second welding part 2 reaches the predetermined requirement (satisfying at least the groove depth of the detection groove 21), and the welding of the first welding part 1 and the second welding part 2 is qualified; on the contrary, if the fusion depth between the first welding part 1 and the second welding part 2 does not reach the predetermined requirement (that is, the fusion depth does not reach the groove depth of the detection groove 21), it means that there is a cold weld between the first welding part 1 and the second welding part 2. Since the detection groove 21 extends from the detection port 201 to the edge of the second welding part 2, the position of the detection port 201 corresponds to the position of the detection through hole 101 of the first welding part 1, so by establishing a connection between the sealing detection device 3 and the detection through hole 101, it can be judged whether the detection groove 21 has been completely blocked by the molten pool 23 according to the airtightness of the detection through hole 101 after welding, and then it can be judged whether there is a cold weld between the first welding part 1 and the second welding part 2. By providing the detection groove 21 on the second welding surface 20 of the second welding part 2, the penetration depth between the first welding part 1 and the second welding part 2 can be effectively controlled to ensure the product yield.

[0071] like Figure 2 The figure shows a cross-sectional view of a welding assembly for cold welding detection according to another embodiment of the present application. The welding assembly for cold welding detection includes a first welding part 1 and a second welding part 2. The first welding part 1 has a first welding surface 10, and a detection through hole 101 penetrating the first welding part 1 is provided on the first welding surface 10; the second welding part 2 has a second welding surface 20, and the second welding surface 20 is welded and adapted to the first welding surface 10, and a detection port 201 is provided on the second welding surface 20, and the position of the detection port 201 corresponds to the position of the detection through hole 101; the second welding part 2 is also provided with a detection channel 22, and the detection channel 22 extends from the detection port 201 to the edge of the second welding part 2, and the detection channel 22 is arranged inside the second welding part 2 and communicated with the detection port 201.

[0072] The above technical solution is to set a detection channel 22 inside the second welding part 2 and set a detection port 201 on the second welding part 2. The position of the detection port 201 corresponds to the position of the detection through hole 101. During the fusion welding process, the molten pool 23 formed by the first welding part 1 will enter the detection channel 22. If the detection channel 22 is completely blocked by the molten pool 23 along the cross-sectional direction, it means that the depth of fusion between the first welding part 1 and the second welding part 2 reaches the predetermined requirement, and the welding of the first welding part 1 and the second welding part 2 is qualified; on the contrary, if the detection channel 22 is not completely blocked by the molten pool 23 at this time, it means that the depth of fusion between the first welding part 1 and the second welding part 2 does not reach the predetermined requirement, and there is a cold weld between the first welding part 1 and the second welding part 2. Since the detection channel 22 extends from the detection port 201 to the edge of the second welding part 2, it is possible to establish a connection between the sealing detection device 3 and the detection port 201 to determine whether the current detection channel 22 is completely blocked by the molten pool 23 along the cross-sectional direction, and then determine whether there is a cold weld between the first welding part 1 and the second welding part 2 based on the sealing detection result of the detection channel 22 after fusion welding, that is, determine whether the current fusion depth reaches the depth requirement of the detection channel 22 from the second welding surface 20.

[0073] Figure 2 The examples in Figure 1 The difference between the embodiments in is that Figure 1 A detection groove 21 extending from the detection port 201 to the edge of the second welding member 2 is provided on the second welding surface 20. Figure 2 An inspection channel 22 is opened inside the second welding surface 20 and extends from the inspection port 201 to the edge of the second welding part 2. Compared with the inspection groove 21, the inspection channel 22 is deeper from the second welding surface 20, and is therefore suitable for welding of welding parts requiring deeper welding penetration.

[0074] like Figure 3 As shown, as an embodiment of the present application, the number of detection slots 21 is more than 2. Usually, the first welding part 1 and the second welding part 2 are welded at multiple points, so it is necessary to cover as many positions in the welding area of ​​the two as possible during the cold welding detection. By setting more than 2 detection slots 21, cold welding detection can be performed on multiple positions on the welding area after the first welding part 1 and the second welding part 2 are welded, thereby improving the coverage of the cold welding detection area between the first welding part 1 and the second welding part 2.

[0075] Preferably, the detection grooves 21 are arranged radially, and the detection port 201 is located at the radial center of the radial shape. Usually, the weld between the first welding part 1 and the second welding part 2 is annular. When detecting the cold weld after welding, by judging the sealing of each detection groove 21, it can be judged whether each detection groove 21 has been completely blocked by the molten pool 23. If each detection groove 21 has been completely blocked by the molten pool 23, it can be inferred that the welding between the first welding part 1 and the second welding part 2 is qualified, otherwise it means that there is a cold weld phenomenon at least in a certain position on the welding area between the first welding part 1 and the second welding part 2. By arranging the detection grooves 21 in a radial shape and arranging the detection port 201 at the radial center of the radial shape, the judgment of the cold weld detection can be made as close as possible to all welding areas between the first welding part 1 and the second welding part 2, thereby improving the accuracy of the judgment of the cold weld detection.

[0076] For example, Figure 3 In the figure, four detection grooves 21 are provided on the second welding surface 20, and the four detection grooves 21 are arranged crosswise, and the angle between adjacent detection grooves 21 is 90°, and the detection port 201 is located in the middle of the second welding surface 20. After the first welding part 1 and the second welding part 2 are welded, if the welding is qualified, the four detection grooves 21 will be completely blocked by the weld (the molten pool 23 is called the weld after condensation) after the first welding part 1 and the second welding part 2 are welded; on the contrary, if there is a cold weld, at least one of the four detection grooves 21 is not completely blocked by the weld. Specifically, the air tightness test of the detection through hole 101 on the detection port 201 can be performed to determine whether the current detection groove 21 has been completely blocked by the weld, thereby realizing the cold weld detection after the welding is completed.

[0077] Preferably, the groove depth of the detection groove 21 is 0.2-2.0mm. In the actual production and processing process, there are often certain requirements for the penetration depth of the first welding part 1 and the second welding part 2 after welding. By setting the groove depth of the detection groove 21 to 0.2-2.0mm, it can be ensured that when the penetration depth reaches 0.2-2.0mm, the molten pool 23 will completely block the detection groove 21, that is, only when the penetration depth reaches 0.2-2.0mm, the sealing of the detection groove 21 after the welding of the first welding part 1 and the second welding part 2 is good, that is, the welding between the first welding part 1 and the second welding part 2 is qualified. When the welding penetration requirement of the first welding part 1 and the second welding part 2 is relatively small, the welding penetration can be effectively controlled by the depth of the groove of the detection groove 21 to meet the needs of the actual production process.

[0078] like Figure 4As shown, as an embodiment of the present application, the number of detection channels 22 is more than 2. Usually, the first welding part 1 and the second welding part 2 are welded at multiple points, so it is necessary to cover as many positions in the welding area of ​​the two as possible during the cold welding detection. By setting more than 2 detection channels 22, cold welding detection can be performed on multiple positions on the welding area after the first welding part 1 and the second welding part 2 are welded, thereby improving the coverage breadth of the cold welding detection area between the first welding part 1 and the second welding part 2.

[0079] Preferably, the detection channel 22 is arranged radially, and the detection port 201 is located at the radial center of the radial shape. Usually, the weld between the first weld 1 and the second weld 2 is annular. When detecting the cold weld after the welding is completed, by judging the sealing of each detection channel 22, it can be judged whether each detection channel 22 has been completely blocked by the molten pool 23. If each detection channel 22 has been completely blocked by the molten pool 23, it can be inferred that the welding between the first weld 1 and the second weld 2 is qualified, otherwise it means that there is a cold weld phenomenon at least in a certain position on the welding area between the first weld 1 and the second weld 2. By arranging the detection channel 22 in a radial shape and setting the detection port 201 at the radial center of the radial shape, the judgment of the cold weld detection can be made as close as possible to all welding areas between the first weld 1 and the second weld 2, thereby improving the accuracy of the judgment of the cold weld detection.

[0080] For example, Figure 4 In the embodiment, four detection channels 22 can be opened inside the second welding surface 20, the angle between adjacent detection channels 22 is 90°, and the detection port 201 is located in the middle of the second welding surface 20. After the first welding part 1 and the second welding part 2 are welded, if the welding is qualified, the four detection channels 22 will be completely blocked by the weld (the molten pool 23 is called the weld after condensation) after the first welding part 1 and the second welding part 2 are welded; on the contrary, if there is a cold weld, at least one of the four detection channels 22 is not completely blocked by the weld. Specifically, the air tightness test of the detection through hole 101 on the detection port 201 can be performed to determine whether the current detection channel 22 has been completely blocked by the weld, thereby realizing the cold weld detection after the welding is completed.

[0081] Preferably, the depth of the detection channel 22 from the second welding surface 20 is 3-5mm. In the actual production and processing process, there are often different requirements for the depth of penetration between different first welding parts 1 and second welding parts 2. By setting the depth of the detection channel 22 from the second welding surface 20 to 3-5mm, it can be ensured that when the depth of penetration reaches 3-5mm, the molten pool 23 will completely block the detection channel 22, that is, only when the depth of penetration reaches 3-5mm, the sealing of the detection channel 22 is good after the welding of the first welding part 1 and the second welding part 2, that is, the welding between the first welding part 1 and the second welding part 2 is qualified. When the welding depth of the first welding part 1 and the second welding part 2 is relatively large, the welding depth can be effectively controlled by the depth of the detection channel 22 from the second welding surface 20 to meet the needs of the actual production process.

[0082] like Figure 5 As shown, in a second aspect, the present application provides a welding structure, including a first welding part 1 and a second welding part 2, the first welding part 1 having a first welding surface 10, the first welding surface 10 being provided with a detection through hole 101 penetrating the first welding part 1; the second welding part 2 having a second welding surface 20, the second welding surface 20 being welded to the first welding surface 10, a detection port 201 being provided on the second welding surface 20, the position of the detection port 201 corresponding to the position of the detection through hole 101, the second welding part 2 also being provided with a detection groove 21, the detection groove 21 being provided on the second welding surface 20, the detection groove 21 extending from the detection port 201 to the edge of the second welding part 2; part or all of the detection groove 21 being blocked by a molten pool 23 generated by welding.

[0083] Figure 5 The welding structure in the embodiment is similar to that in the present application. Figure 1 The difference between the welding assembly for cold welding detection shown in the figure is that the welding structure refers to the structure formed after the first welding part 1 and the second welding part 2 are welded, which is manifested as part or all of the detection groove 21 on the second welding part 2 being blocked by the weld. Figure 5 It can be seen that the weld extends downward to the depth below the detection groove 21, and at this time the detection groove 21 is completely blocked by the weld. When all the detection grooves 21 on the second weld 2 are blocked by the weld, it means that all the detection grooves 21 on the second weld 2 of the welding structure are well sealed, that is, the first weld 1 and the second weld 2 in the welding structure are welded properly; when part of the detection groove 21 on the second weld 2 is blocked by the weld, it means that part of the detection groove 21 on the second weld 2 of the welding structure is well sealed, that is, the first weld 1 and the second weld 2 in the welding structure have good sealing in the welding area corresponding to the position of the detection groove 21, and the first weld 1 and the second weld 2 are welded properly in this part of the area, and there is no cold welding phenomenon.

[0084] like Figure 6FIG. 1 is a cross-sectional view of a welding structure with a cold weld according to an embodiment of the present application. Figure 6 It can be seen that the weld does not extend downward to the detection groove 21, and the depth of the weld does not reach the groove depth of the detection groove 21, which means that in the welding structure, the detection groove 21 on the second welding part 2 is not blocked by the weld, and the welding structure has a cold weld. Specifically, when judging whether there is a cold weld in the welding structure, it can be achieved by testing the sealing of the detection through hole 101 of the first welding part 1 in the welding structure, and then the selected welding structure with cold welds can be processed to improve the product yield.

[0085] like Figure 7 The figure shows a cross-sectional view of a welding structure with qualified welding according to another embodiment of the present application. In this embodiment, the welding structure includes a first welding part 1 and a second welding part 2. The first welding part 1 has a first welding surface 10, and a detection through hole 101 penetrating the first welding part 1 is provided on the first welding surface 10; the second welding part 2 has a second welding surface 20, and the second welding surface 20 is welded to the first welding surface 10, and a detection port 201 is provided on the second welding surface 20, and the position of the detection port 201 corresponds to the position of the detection through hole 101. The second welding part 2 is provided with an inspection channel inside, and the inspection channel 22 extends from the inspection port 201 to the edge of the second welding part 2; part or all of the inspection channel 22 is blocked by the molten pool 23 generated by welding.

[0086] Figure 7 The welding structure in the embodiment is similar to that in the present application. Figure 2 The difference between the welding components for the cold weld detection shown in the figure is that the welding structure refers to the structure formed after the first welding part 1 and the second welding part 2 are welded, which is manifested as part or all of the detection channel 22 on the second welding part 2 being blocked by the weld. Figure 7 It can be seen that the weld extends downward to the depth below the detection channel 22, and the detection channel 22 is completely blocked by the weld. When all the detection channels 22 on the second weld 2 are blocked by the weld, it means that all the detection channels 22 on the second weld 2 of the welding structure have good sealing properties, that is, the welding of the first weld 1 and the second weld 2 in the welding structure is qualified; when part of the detection channel 22 on the second weld 2 is blocked by the weld, it means that part of the detection channel 22 on the second weld 2 of the welding structure has good sealing properties, that is, the welding area corresponding to the first weld 1 and the second weld 2 in the welding structure where the detection channel 22 is located has good sealing properties, which avoids the phenomenon of cold welding between the first weld 1 and the second weld 2 to a certain extent.

[0087] like Figure 8 FIG. 1 is a cross-sectional view of a welding structure with a cold weld according to another embodiment of the present invention. Figure 8It can be seen that the weld does not extend downward to the bottom of the detection channel 22, that is, the depth of the weld does not reach the groove depth of the detection channel 22, which means that in the welding structure, the detection channel 22 on the second welding part 2 is not blocked by the weld, and there is a cold weld in the welding structure. Specifically, when judging whether there is a cold weld in the welding structure, it can be achieved by testing the sealing of the detection through hole 101 of the first welding part 1 in the welding structure, and then the screened welding structure with cold welds can be processed to improve the product yield.

[0088] Preferably, Figure 5-Figure 8 In the welding structure shown, the number of the detection slots 21 and / or the detection channels 22 is more than 2. The detection slots 21 and / or the detection channels 22 are arranged radially, and the detection port 201 is located at the radial center of the radial. In this way, the relatively reduced number of detection slots 21 and / or detection channels 22 can be used to perform cold welding detection on each welding area between the first welding part 1 and the second welding part 2 in the welding structure as much as possible, thereby improving the yield rate of the product.

[0089] Preferably, the groove depth of the detection groove 21 is 0.2-2.0 mm, and the depth of the detection channel 22 from the second welding surface 20 is 3-5 mm. In this way, when the welding penetration requirement of the first welding part 1 and the second welding part 2 is relatively small, the welding penetration between the first welding part 1 and the second welding part 2 in the welding structure can be effectively controlled by setting the groove depth of the detection groove 21, so as to avoid the phenomenon of cold welding in the welding structure due to the welding penetration between the first welding part 1 and the second welding part 2 not meeting the predetermined requirement. When the welding penetration requirement of the first welding part 1 and the second welding part 2 is relatively large, the welding penetration between the first welding part 1 and the second welding part 2 in the welding structure can be effectively controlled by setting the groove depth of the detection channel 22 from the second welding surface 20, so as to avoid the phenomenon of cold welding in the welding structure due to the welding penetration between the first welding part 1 and the second welding part 2 not meeting the predetermined requirement. By setting the detection groove 21 or the detection channel 22 of different depths, the welding of welding parts with different requirements for penetration can be met.

[0090] like Fig. 9 As shown, in the third aspect, the present application provides a device for detecting cold welds, including a positive pressure generating device or a negative pressure generating device 33, a detection pipe 31, a detection head 32 and an air pressure detector; one end of the detection pipe 31 is connected to the positive pressure generating device or the negative pressure generating device 33; the detection head 32 is connected to the other end of the detection pipe 31, and the detection head 32 has a connection structure that is airtightly connected to the detection through hole 101 on the surface of the weld; the air pressure detector is connected to the detection pipe 31 for detecting air pressure. The air pressure detector can be arranged in the detection pipe 31, or in a buffer tank. Fig. 9In the welding structure, the detection groove 21 of the second welding part 2 is completely blocked by the weld, which means that the welding between the first welding part 1 and the second welding part 2 is qualified and there is no cold welding.

[0091] Fig.10 This is a cross-sectional view of a device for detecting a cold weld according to an embodiment of the present application detecting a welding structure with a cold weld. Fig.10 It can be seen that the weld does not extend downward to the bottom of the detection groove 21, that is, the depth of the weld does not reach the groove depth of the detection groove 21. This means that in the welding structure, the detection groove 21 on the second welding part 2 is not blocked by the weld, and there is a cold weld in the welding structure.

[0092] like Figure 11-Figure 12 As shown, the device for detecting cold welds provided by the present application can be used not only for detecting cold welds of the welding structure of the second welding part 2 having the detection groove 21, but also for detecting cold welds of the welding structure of the second welding part 2 having the detection channel 22. Fig.11 In the welding structure, the detection channel 22 of the second welding part 2 is completely blocked by the weld, indicating that the welding between the first welding part 1 and the second welding part 2 is qualified and there is no false welding. Fig.12 In the figure, the weld does not extend downward to the bottom of the detection channel 22, that is, the depth of the weld does not reach the depth of the detection channel 22 from the second welding surface 20, indicating that there is a cold weld between the first welding part 1 and the second welding part 2.

[0093] When using the equipment for detecting cold welds, the detection head 32 can be first tightly connected to the detection through hole 101, and then the positive pressure generating device or the negative pressure generating device 33 can be turned on. The positive pressure generating device or the negative pressure generating device 33 provides positive pressure or negative pressure to the detection through hole 101 through the detection pipe 31. If the first welding part 1 and the second welding part 2 are welded qualified after the welding is completed, that is, the detection groove 21 and / or the detection channel 22 are completely blocked by the molten pool 23, during the detection process, the fluid will not flow out of the detection groove 21 and / or the detection channel 22 from the detection port 201 to the outside world, or will not flow into the detection port 201 from the outside world through the detection groove 21 and / or the detection channel 22. At this time, the air pressure in the detection pipe 31 detected by the air pressure detector will not increase significantly in a short period of time. On the contrary, if there is a cold weld between the first weld 1 and the second weld 2 after welding, that is, the detection groove 21 and / or the detection channel 22 are not completely blocked by the molten pool 23, during the detection process, the fluid will flow out of the detection groove 21 and / or the detection channel 22 from the detection port 201 to the outside or flow into the detection port 201 from the outside through the detection groove 21 and / or the detection channel 22. At this time, the air pressure in the detection pipeline 31 detected by the air pressure detector will change significantly in a short period of time. By judging the air pressure change value detected by the air pressure detector, it can be determined whether there is a cold weld between the first weld 1 and the second weld 2 after welding, and then the welding structure with cold weld can be screened out for processing to improve the product yield.

[0094] As an embodiment of the present application, the first welding part 1 is an electrode connecting piece, and the second welding part 2 is a battery cell pole. The electrode connecting piece can be a copper sheet, an aluminum sheet, etc. Fig.13 As shown, in the field of battery 200 production and processing, it is necessary to weld the electrode connecting piece to the cell pole of the cell top cover 100 to achieve conductive connection between the cell and external components. If the welding depth between the electrode connecting piece and the cell pole is not enough, it will affect the subsequent performance of the cell. In this application, by opening a detection groove 21 on the second welding surface 20 of the cell pole or setting a detection channel 22 inside the second welding part 2, and setting a detection port 201 on the cell pole corresponding to the position of the detection through hole 101 on the electrode connecting piece, after the fusion welding is completed, the sealing of the detection groove 21 and / or the detection channel 22 can be judged to determine whether there is a cold welding phenomenon between the electrode connecting piece and the cell pole. If there is a cold welding phenomenon, the electrode connecting piece and the cell pole after welding can be further processed to improve the product yield.

[0095] like Figure 14-15As shown, a cell pole (i.e., the second welding part 2) is provided on the cell top cover 100, and an electrode connecting piece (i.e., the first welding part 1) needs to be welded on the cell pole. By starting a plurality of detection grooves 21 on the second welding surface 20 of the cell pole, the sealing of the detection through hole 101 on the electrode connecting piece in the welded structure after welding can be detected to determine whether the welding penetration between the cell pole and the electrode connecting piece reaches the depth of the detection groove 21, and further determine whether there is a cold weld in the welded structure.

[0096] like Figure 16-Figure 17 As shown, a cell pole (i.e., the second welding piece 2) is provided on the cell top cover 100, and an electrode connecting piece (i.e., the first welding piece 1) needs to be welded on the cell pole. By providing a plurality of detection channels 22 inside the cell pole, the sealing of the detection through hole 101 on the electrode connecting piece in the welded structure after welding can be detected to determine whether the welding penetration between the cell pole and the electrode connecting piece reaches the depth of the detection groove 21, and further determine whether there is a cold weld in the welded structure.

[0097] like Fig.18 As shown, the present application provides a method for detecting a cold solder joint, comprising the following steps:

[0098] First, enter step S1801 to weld the first welding surface 10 of the first welding part 1 and the second welding surface 20 of the second welding part 2; the first welding surface 10 is provided with a detection through hole 101 penetrating the first welding part 1, and the second welding surface 20 is provided with a detection port 201, the position of the detection port 201 corresponds to the position of the detection through hole 101, and the second welding part 2 is also provided with a detection groove 21 and / or a detection channel 22, the detection groove 21 and / or the detection channel 22 extend from the detection port 201 to the edge of the second welding part 2, the detection groove 21 is provided on the second welding surface 20, and the detection channel 22 is provided inside the second welding part 2 and communicates with the detection port 201;

[0099] Then, the process proceeds to step S1802 to inspect the sealing of the inspection through hole 101 to determine whether there is a cold solder joint.

[0100] Through the above-mentioned method for detecting cold solder joints, it is possible to determine whether the first welding part 1 and the second welding part 2 have cold solder joints after welding, and then the welding structures with cold solder joints can be screened out for processing to improve the product yield.

[0101] As an implementation mode of the present application, the sealing of the detection through hole 101 is detected, specifically including: applying positive pressure or negative pressure to the detection through hole 101 to detect its sealing. When positive pressure is applied to the detection through hole 101, if there is a cold weld phenomenon between the first welding part 1 and the second welding part 2 after welding, that is, the detection groove 21 and / or the detection channel 22 are not completely blocked by the molten pool 23, the fluid will flow out of the edge of the second welding part 2 from the detection groove 21 and / or the detection channel 22 from the detection through hole 101. By detecting the sealing of the detection through hole 101, it can be determined whether there is a cold weld phenomenon between the first welding part 1 and the second welding part 2 after welding. When negative pressure is applied to the detection through hole 101, if a cold weld exists between the first welding part 1 and the second welding part 2 after welding, that is, the detection groove 21 and / or the detection channel 22 are not completely blocked by the molten pool 23, the fluid will flow into the detection through hole 101 from the edge of the second welding part 2 through the detection groove 21 and / or the detection channel 22. By detecting the sealing of the detection through hole 101, it can be determined whether a cold weld exists between the first welding part 1 and the second welding part 2 after welding.

[0102] As an implementation mode of the present application, applying positive pressure or negative pressure to the detection through hole 101 to detect its sealing specifically includes: applying positive pressure or negative pressure to the detection through hole 101 through a closed fluid system, stopping the pressure change, and then observing the pressure change of the closed fluid system within a preset time. If the pressure change of the closed fluid system within the preset time is less than the preset value, it is judged that the welding is qualified, otherwise it is judged that there is a cold weld. By comparing the pressure change of the closed fluid system within the preset time with the preset value, the sealing of the detection through hole 101 can be accurately judged to determine whether there is a cold weld phenomenon, and then the welding structure with cold welds can be screened out for processing to improve the product yield.

[0103] As an implementation mode of the present application, the sealing of the detection through hole 101 is tested with gas or liquid as the medium. If the welding is qualified, the molten pool 23 completely blocks the detection groove 21 and / or the detection channel 22. At this time, the flow path of the gas or liquid is blocked by the molten pool 23, and the detection groove 21 and / or the detection channel 22 will not change significantly within the predetermined time, indicating that the sealing of the detection through hole 101 is good; if there is a cold weld, the molten pool 23 does not completely block the detection groove 21 and / or the detection channel 22, and the gas or liquid will flow out of the edge of the second welding part 2 through the detection groove 21 and / or the detection channel 22, and the detection groove 21 and / or the detection channel 22 will change significantly within the predetermined time, indicating that the sealing of the detection through hole 101 is poor. By introducing gas or dripping liquid, the accurate detection of the sealing of the detection through hole 101 can be achieved, and the accuracy of judging whether there is a cold weld can be improved.

[0104] It should be noted that, although the above embodiments have been described in this article, this does not limit the scope of patent protection of this application. Therefore, based on the innovative concept of this application, changes and modifications made to the embodiments described herein, or equivalent structures or equivalent process changes made using the contents of the specification and drawings of this application, directly or indirectly applying the above technical solutions to other related technical fields, are all included in the scope of patent protection of this application.

Claims

1. A welding assembly for detecting cold welding, characterized in that: include: A first welding piece having a first welding surface, wherein a detection through hole penetrating through the first welding piece is provided on the first welding surface; The second welding piece has a second welding surface, the second welding surface is welded and adapted to the first welding surface, and a detection port is provided on the second welding surface, and the position of the detection port corresponds to the position of the detection through hole; the second welding piece is also provided with a detection groove and / or a detection channel, the detection groove and / or the detection channel extends from the detection port to the edge of the second welding piece, the detection groove is provided on the second welding surface, and the detection channel is provided inside the second welding piece and communicated with the detection port; Among them, after applying positive pressure or negative pressure to the detection through hole through a closed fluid system, the pressure change is stopped, and then the pressure change of the closed fluid system is observed within a preset time. If the pressure change of the closed fluid system is less than a preset value within the preset time, it is judged that the welding is qualified, otherwise it is judged that there is a cold weld.

2. The welding assembly for detecting cold welding according to claim 1, characterized in that: The number of the detection slots and / or detection channels is more than 2.

3. The welding assembly for detecting cold welding according to claim 2, characterized in that: The detection slots and / or detection channels are arranged radially, and the detection ports are located at the radial center.

4. The welding assembly for detecting cold welding according to claim 1, characterized in that: The depth of the detection groove is 0.2-2.0 mm.

5. The welding assembly for detecting cold welding according to claim 1, characterized in that: The depth of the detection channel from the second welding surface is 3-5 mm.

6. The welding assembly for detecting cold welds according to any one of claims 1 to 5, characterized in that: The first welding part is an electrode connecting piece, and the second welding part is a battery cell pole.

7. A welding structure, characterized in that: The welding structure comprises: A first welding piece having a first welding surface, wherein a detection through hole penetrating through the first welding piece is provided on the first welding surface; A second welding piece, comprising a second welding surface, the second welding surface being welded to the first welding surface, a detection port being provided on the second welding surface, the position of the detection port corresponding to the position of the detection through hole, the second welding piece further comprising a detection groove and / or a detection channel, the detection groove and / or the detection channel extending from the detection port to an edge of the second welding piece, the detection groove being provided on the second welding surface, the detection channel being provided inside the second welding piece and communicating with the detection port; Part or all of the detection groove and / or detection channel is blocked by the molten pool produced by welding; Among them, after applying positive pressure or negative pressure to the detection groove and / or detection channel through a closed fluid system, the pressure change is stopped, and then the pressure change of the closed fluid system is observed within a preset time. If the pressure change of the closed fluid system is less than a preset value within the preset time, it is judged that the welding is qualified, otherwise it is judged that there is a cold weld.

8. The welding structure according to claim 7, characterized in that: The number of the detection slots and / or detection channels is more than 2.

9. The welding structure according to claim 8, characterized in that: The detection slots and / or detection channels are arranged radially, and the detection ports are located at the radial center.

10. The welding structure according to claim 7, characterized in that: The depth of the detection groove is 0.2-2.0 mm.

11. The welding structure according to claim 7, characterized in that: The depth of the detection channel from the second welding surface is 3-5 mm.

12. The welding structure according to any one of claims 7 to 11, characterized in that: The first welding part is an electrode connecting piece, and the second welding part is a battery cell pole.

13. A device for detecting cold solder joints, characterized in that: The device comprises: Positive pressure generating device or negative pressure generating device; A detection pipeline, one end of which is connected to the positive pressure generating device or the negative pressure generating device; A detection head, the detection head is connected to the other end of the detection pipeline, and the detection head has a connection structure that is air-tightly connected to the detection through hole on the surface of the weldment; An air pressure detector is connected to the detection pipeline and is used to stop changing the pressure after the positive pressure generating device or the negative pressure generating device applies positive pressure or negative pressure to the detection pipeline, and then detect the pressure change in the detection pipeline within a preset time. If the pressure change in the detection pipeline is less than a preset value within the preset time, it is judged that the welding is qualified, otherwise it is judged that there is a cold weld.

14. A method for detecting cold solder joints, characterized in that: The following steps are involved: Welding a first welding surface of a first welding part to a second welding surface of a second welding part, wherein the first welding surface is provided with a detection through hole penetrating the first welding part, and the second welding surface is provided with a detection port, the position of the detection port corresponds to the position of the detection through hole, and the second welding part is further provided with a detection groove and / or a detection channel, the detection groove and / or the detection channel extending from the detection port to the edge of the second welding part, the detection groove is provided on the second welding surface, and the detection channel is provided inside the second welding part and communicated with the detection port; After applying positive or negative pressure to the detection through hole through a closed fluid system, stop changing the pressure, and then observe the pressure change of the closed fluid system within a preset time. If the pressure change of the closed fluid system is less than a preset value within the preset time, it is judged that the welding is qualified, otherwise it is judged that there is a cold weld.

15. A method for detecting cold solder joints according to claim 14, characterized in that: The sealing property of the detection through hole is detected by using gas or liquid as the medium.