A hardening layer coating liquid and an anti-glare film
By using hardened layer coating liquid and ball grinding technology in anti-glare film, combining high-refractive and low-refractive index hardened liquid and organic inorganic particles, the problem of poor wear resistance and transparency of the anti-glare film is solved, and high transparency is achieved And wear-resistant anti-glare film, significantly improving the picture quality of the display.
Patent Information
- Application Number
- CN202111225640.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-10-20
- Filing Date
- 2021-10-21
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2041-10-21
AI Technical Summary
The existing anti-glare film has poor wear resistance and poor transparency, resulting in screen shaking, whitening and poor visual effects.
Using hardened layer coating liquid, which contains high refractive index and low refractive index hardened liquid, organic particles and inorganic particles, the anti-glare film with high light transmittance and high wear resistance is formed by adjusting the refractive index and particle ratio, and the anti-glare film with high light transmittance and high wear resistance is used to utilize dioxide Silicon inorganic particles improve scratch resistance and improve the wear resistance of the film through ball milling and ultraviolet curing technologies.
It realizes an anti-glare film with high transparency, low flash point, good wear resistance and no whitening, which significantly improves the picture quality and service life of the monitor.
Smart Images

Figure CN115991960B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional films, and in particular relates to a hardening layer coating liquid and an anti-glare film. Background Art
[0002] Car displays, laptops, LCDs, etc. need to recognize images through the functional film on the surface. The light emitted by the internal backlight components of these displays can reduce the intake and transmit smoothly. When the external light is taken in, it is diffusely reflected, which not only prevents glare but also reduces the glossiness and reduces light and shadow, thereby improving the image quality. Since the functional film is on the outermost layer of the display, the surface of the display is often wiped during daily use and maintenance, which can easily cause scratches on the surface, affecting the service life and appearance.
[0003] With the development of technology, the resolution of displays is getting higher and higher, and at the same time, the problem of picture jitter will arise. The existing technology is to continuously add particles such as silica to increase the overall haze, resulting in a white screen. Especially against a black screen background, the black depth value is low, which appears to be of low taste and poor visual effect.
[0004] Chinese patent document publication number CN 1540365 A (published on October 27, 2004) discloses an anti-glare film. It includes coating an AG particle layer on a substrate such as TAC and PET, and is composed of an anti-glare layer containing two kinds of particles and resin. The large particles are organic particles with an average particle size of 1 to 4 μm, and the small particles are inorganic particles with an average particle size of 0.5 to 1 μm, forming an anti-glare film with a haze of 9% to 20% and a 60-degree mirror gloss of less than 65°. The above anti-glare film can solve the problems of transparency, flickering and whitening. However, since the protruding large particles of the anti-glare film are organic particles, the composition is acrylic resin, and the inorganic particles with good wear resistance are not as good as those with silica, it does not have good wear resistance. In addition, organic particles have a swelling effect. The large organic particles will absorb a certain proportion of solvents and swell after being placed for a long time, resulting in deterioration of the film surface during coating, thereby affecting the production yield and causing great losses. Summary of the invention
[0005] In order to solve the problems of poor wear resistance and poor transparency of the existing anti-glare film, the present invention provides a hardening layer coating liquid and an anti-glare film. The anti-glare film provided by the present invention has excellent anti-glare performance, high wear resistance and good transparency.
[0006] The anti-glare film provided by the present invention is also called a high-definition anti-glare film.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions.
[0008] The invention provides a hardening layer coating liquid, which comprises a high-refractive index hardening liquid, a low-refractive index hardening liquid, organic particles, inorganic particles, propylene glycol methyl ether and butanone.
[0009] Furthermore, the refractive index of the low-refractive-index hardening liquid is in the range of 1.45 to 1.49, and the refractive index of the high-refractive-index hardening liquid is in the range of 1.60 to 1.65.
[0010] Furthermore, the organic particles in the hardening liquid are acrylic resin organic particles, and the inorganic particles are silicon dioxide inorganic particles.
[0011] Furthermore, in the hardening liquid, the particle size of the acrylic resin organic particles is 0.5 to 3 μm, and the refractive index is 1.45 to 1.51; the particle size of the silica inorganic particles is 1 to 5 μm, and the refractive index is 1.45 to 1.51.
[0012] Furthermore, the particle size of the organic particles is 0.5 to 2.0 μm, and the particle size of the inorganic particles is 2 to 3 μm.
[0013] Furthermore, the low refractive index hardening liquid contains hexafunctional polyurethane acrylic resin polymer, trifunctional acrylate monomer and difunctional acrylate monomer; the high refractive index hardening liquid contains hexafunctional polyurethane acrylic resin polymer, tetrafunctional acrylic monomer and zirconium oxide nanoparticles with a particle size of 20 to 50 nm.
[0014] The hardened layer coating liquid forms an anti-glare film hardened layer after solidification, and has high light transmittance and high wear resistance. Under the condition of haze of 25±2%, the 60° mirror gloss can be controlled within 50° to 70°.
[0015] The present invention adjusts the refractive index by adding two hardening liquids with different refractive indices in a ratio, preferably adjusting the refractive index between 1.45 and 1.55, and forms internal fog through the refractive index difference of different particles, so the application range is wide and the limitation on particles is small.
[0016] The present invention adds two kinds of particles to a hardening liquid with a good ratio. The small particles are organic particles with an average particle size of 0.5 to 3.0 μm and a refractive index of 1.45 to 1.51. Considering that organic particles are prone to swelling effect, the preferred particle size is 0.5 to 2.0 μm so that the entire particle can be buried in the hardening layer. The large particles are inorganic particles with an average particle size of 1 to 5 μm and a refractive index of 1.45 to 1.51. The preferred particle size is 2 to 3 μm, and the coating thickness of the hardening liquid is 4 μm-8 μm.
[0017] Furthermore, the present invention provides a hardening layer coating liquid, the hardening layer coating liquid comprises 20% to 45% of a low refractive index hardening liquid, 5% to 25% of a high refractive index hardening liquid, 1% to 5% of organic particles, 21% to 54% of an inorganic particle ball milling liquid, and 10% to 17% of butanone. The inorganic particle ball milling liquid contains 15% of silica inorganic particles.
[0018] The inorganic particle ball milling liquid comprises inorganic silicon dioxide particles, propylene glycol methyl ether and butanone; the inorganic silicon dioxide particles are dispersed in the propylene glycol methyl ether and butanone.
[0019] The addition ratio of the high refractive index hardening liquid to the low refractive index hardening liquid is 1:1-1:5.
[0020] Furthermore, the hardening layer coating liquid includes 25% to 45% of a low refractive index hardening liquid, 11% to 25% of a high refractive index hardening liquid, 2% to 5% of organic particles, 21% to 35% of an inorganic particle ball milling liquid, and 10% to 17% of butanone. The addition ratio of the high refractive index hardening liquid to the low refractive index hardening liquid is 1:1-1:3.55. The aforementioned technical solution includes embodiments 1-3 and embodiment 5.
[0021] Furthermore, the anti-glare film provided by the present invention has a reduced flash point phenomenon and does not turn white, thus solving the problem of severe flash point and whitening of the existing anti-glare film.
[0022] Furthermore, from the perspective of refractive index, organic particles are close in size and can be evenly distributed in the hardened layer to form a relatively uniform internal haze, and acrylic resin particles are preferred. From the perspective of wear resistance and external haze, inorganic particles are harder, have good scratch resistance, and can form diffuse reflection to reduce the 60° mirror gloss, and silica inorganic particles are preferred.
[0023] Furthermore, inorganic silicon dioxide particles with a particle size of 5 μm are dispersed in propylene glycol methyl ether and butanone, and ball milled to form a silicon dioxide ball milling solution with a solid content of 15%. The average particle size of the inorganic particles after ball milling is 1 to 5 μm.
[0024] Since the inorganic silica particles are relatively heavy and do not have good suspension properties, they cannot effectively float on the hardened layer. Therefore, the silica is dissolved in propylene glycol methyl ether and butanone and ball-milled to form a silica ball-milling liquid with a solid content of 15%. Different particle sizes can be achieved by adjusting the ball mill speed and ball milling time. At the same time, after the inorganic particles are destroyed after ball milling, their weight becomes lighter and they are easily suspended in the solvent. After high-temperature baking, since butanone is a low-boiling point solvent, under high temperature conditions, butanone will evaporate from the coating liquid first and bring the silica particles to the top layer of the hardened film. Finally, after ultraviolet light curing, an anti-glare film with high wear resistance is formed.
[0025] The solid content of the hardening layer coating liquid is 25% to 40%, and the percentage is the weight percentage.
[0026] Furthermore, the high refractive index hardening liquid is produced by Japan's Arakawa Chemical, and the low refractive index hardening liquid is produced by Taiwan's Kenmet Materials Technology Co., Ltd.
[0027] The present invention further provides an anti-glare film, comprising a substrate and a hardened layer, wherein the hardened layer is formed by curing the hardened layer coating liquid of the present invention.
[0028] The substrate is a transparent base film. The present invention has no particular limitation on the transparent base film used, such as triacetyl cellulose film (TAC), polyethylene terephthalate film (PET), polycarbonate film (PC), and the like.
[0029] Furthermore, the thickness of the substrate is 50 μm to 250 μm, and the thickness of the hardened layer is 4 μm to 8 μm.
[0030] Compared with the existing anti-glare film, the anti-glare film provided by the present invention has the following beneficial effects: high light transmittance, low flash point, good wear resistance and no whitening. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a schematic structural diagram of the anti-glare film provided by the present invention. DETAILED DESCRIPTION
[0032] In order to make it easier to understand the structure of the present invention and the functional features and advantages that can be achieved, the preferred embodiments of the present invention are described in detail with reference to the drawings as follows:
[0033] like Figure 1 As shown, the anti-glare film provided by the present invention includes an anti-glare hardened layer (also called a hard coating film or hard coating layer, or hardened layer) and a substrate 3 from top to bottom, and the hardened layer is attached to the surface of the substrate 3. The hardened layer includes organic particles 2 and inorganic particles 1.
[0034] In the raw materials of the hardening layer coating liquid provided by the embodiment of the present invention, the average particle size of the silicon dioxide inorganic particles is 5.0 μm, and after ball milling, a ball milling liquid with an average particle size of 2.0 μm and a solid content of 15% is obtained, and the average particle size of the acrylic resin organic particles is 0.5 μm. In the raw materials of the hardening layer coating liquid provided by the embodiment of the present invention, the high refractive index hardening liquid is produced by Japan's Arakawa Chemical, and the low refractive index hardening liquid is produced by Taiwan Kenmet Materials Technology Co., Ltd., China.
[0035] Preparation of ball milling liquid: dissolve inorganic silica particles in propylene glycol methyl ether and butanone, pour into a ball mill, set the ball mill speed to 250r / min for ball milling, and ball milling for 2 hours to form a silica ball milling liquid with a solid content of 15%. Different particle sizes can be achieved by adjusting the ball mill speed and ball milling time. At the same time, after ball milling, the inorganic particles are destroyed, the weight becomes lighter, and it is not easy to settle.
[0036] In the anti-glare film provided by the embodiment of the present invention,
[0037] 1. Substrate (base film) material: highly transparent substrate, triacetyl cellulose film (TAC: refractive index 1.48), polyethylene terephthalate film (PET: refractive index 1.66), polycarbonate film (PC: refractive index 1.58), etc. The thickness of the base film is 80 μm. Since the refractive index of the hardening liquid is adjusted in the range of 1.45 to 1.55, TAC film with a relatively close refractive index is preferred.
[0038] 2. Process conditions for curing of the hardened layer and coating thickness of the hardened layer:
[0039] Temperature: 85℃, 5min,
[0040] Light curing energy: 400~600mj / cm 2 ,
[0041] Coating thickness: 4-8μm (within the above thickness range, not only can the coating be uniform, but also has good wear resistance).
[0042] Before applying the hardening layer coating liquid on the surface of the substrate, the hardening layer coating liquid should be prepared and left to stand for 30 minutes.
[0043] The testing instrument and testing method for the anti-glare film provided in the embodiment of the present invention are as follows:
[0044] 1. Transmittance and haze test: Nippon Denshoku NDH-2000N tests the total light transmittance and haze of the anti-glare film according to the JISK-7150 standard. For the internal haze test, a 5cm×5cm film piece is selected and the surface is covered with a silicone protective film before testing.
[0045] 2. Wear resistance test: Kunshan Jingjia Instrument A20-339, according to JISK-5600 standard, using 0000# steel wool, 1000gf / cm 2 The maximum number of times to rub the hardened layer of the anti-glare film back and forth under a load to test whether the film surface is scratched. If the friction resistance is more than 1500 times without scratches, it is said to have high wear resistance.
[0046] 3. Pencil hardness test: Japanese Elcometer 3086, according to JISK-5600 standard, uses Mitsubishi model 1H~9H pencils, loads 500g, draws 5 lines on the surface of the anti-glare film, and detects whether the film surface is scratched. The higher the pencil model, the higher the hardness of the hardened layer.
[0047] 4. Hardened layer adhesion test: According to JISK-5600 standard, the adhesion of the hardened layer surface is tested, where 100 / 100 means no peeling, and 0 / 100 means complete peeling.
[0048] 5. Thickness test: Cut a 10cm×10cm piece of anti-glare film and test its thickness with a micrometer.
[0049] 6. Flash point test: With the display screen having a pure green picture background, apply the anti-glare film on the screen with OCA stickers, and evaluate the flash point degree of the picture by visual inspection. Samples with no flash points at all will be rated as excellent, samples with some flash points will be rated as qualified, and samples with serious flash points will be rated as unqualified.
[0050] 7. Black and white degree test: Take a 10cm×10cm black acrylic board, apply the anti-glare film on the black acrylic board with OCA glue, and use a color density meter to measure the black density. Items with a density of 2.0 or more are represented as √, which is qualified (not whitish); items with a density of less than 2.0 are represented as ×, which is unqualified. The higher the value of the black density, the clearer it is, the better the taste, and the better the visual effect.
[0051] 8. Gloss test: Use a gloss meter (Sanenchi 3nh, HG60) to measure the 60° gloss according to JIS Z8741. It is best to control the gloss at 50° to 70°. If the gloss is too low, it will easily turn white.
[0052] Example 1
[0053] This embodiment provides a hardening layer coating liquid, comprising 16% high refractive index hardening liquid, 36% low refractive index hardening liquid, 33% inorganic particle ball milling liquid (solid content: 15%), 2% organic particles, and 13% butanone. The average particle size of the inorganic particles is 2 μm, and the particle size of the organic particles is 0.5 μm; the percentage content is weight percentage. The base film adopts TAC base film, with a thickness of 80 μm.
[0054] The process conditions for curing the hardened layer are as follows:
[0055] Temperature: 85℃, time: 5min,
[0056] Light curing energy: 400~600mj / cm 2 ,
[0057] Coating thickness of hardened layer (dry film thickness): 4-8 μm.
[0058] Before coating the hardening layer coating liquid on the surface of the substrate, the hardening layer coating liquid should be prepared according to the method provided by the present invention and allowed to stand for 30 minutes.
[0059] Embodiment 2-6
[0060] The hardening layer coating liquid provided in Example 1 has a formula as shown in Table 1. The preparation method of the hardening layer coating liquid is the method provided by the present invention. The substrate of the anti-glare film and the preparation method of the anti-glare film are the same as those in Example 1.
[0061] Table 1 Part of the raw materials and contents of the hardening layer coating solution provided in Examples 1-6
[0062]
[0063] Comparative Example 1
[0064] Compared with Example 1, the difference of the comparative example is that the particle size of the organic particles is 5 um, and the organic particle component is also acrylic resin particles. The components and their weight parts are shown in Table 2.
[0065] The preparation method and process parameters of the hard coating are the same as those in Example 1.
[0066] The particle size of the organic particles in the hardening solution in Comparative Example 1 is too large.
[0067] Comparative Example 2
[0068] Compared with Example 1, the difference in the comparative example is that the addition amount of the high refractive index hardening liquid is 0, and the components and their weight parts are shown in Table 2.
[0069] The preparation method and process parameters of the hard coating are the same as those in Example 1.
[0070] Comparative Example 3
[0071] Compared with Example 1, the difference in the comparative example is that the amount of organic particles added is 0. The components and their weight parts are shown in Table 2.
[0072] The preparation method and process parameters of the hard coating are the same as those in Example 1.
[0073] Comparative Example 4
[0074] Compared with Example 5, the difference in the comparative example is that the addition amount of the inorganic particle ball milling liquid is 0, and the components and their weight parts are shown in Table 2.
[0075] The preparation method and process parameters of the hard coating are the same as those in Example 1.
[0076] Table 2 Partial raw materials and contents of the hardening layer coating solution provided in Comparative Examples 1-4
[0077]
[0078] Table 3 Performance test results of the hardened layer formed by the hardened layer coating solution provided in Examples 1-6 and Comparative Examples 1-4
[0079]
[0080]
[0081] Table 4 Performance test results of the hardened layer formed by the hardened layer coating solution provided in Examples 1-6 and Comparative Examples 1-4
[0082]
[0083] The analysis of the experimental data in the above table shows that the hard coating films in Examples 1, 2, 3, and 5 of the present invention have good comprehensive performance, good transparency (light transmittance), low flash point, good wear resistance, and no whitening problem. In particular, after the wear resistance test, the anti-glare film did not turn white after being treated with a black acrylic plate. In Example 4, due to the thinning of the coating thickness, the protruding height of the upper inorganic particles was too high, the flash point effect deteriorated, and the wear resistance also weakened. After the wear test, it turned slightly white after being tested with a black acrylic plate. In Example 6, due to the reduction in the added ratio of high-refractive index hardening liquid and organic particles, the refractive index of the neutralized hardening liquid and the organic particles is relatively close, and the refractive index difference cannot be effectively formed, resulting in insufficient internal fog. Since the external light cannot penetrate the anti-glare film, the black test turns white. Due to the large particle size of the inorganic particles, the flash point effect is poor.
[0084] In Comparative Example 1, due to the replacement of organic particles with large particle size, under the same experimental conditions as in Example 1, the particle size is too large and protrudes from the surface of the hardened layer together with the inorganic particles, resulting in a strong sense of graininess, which affects the flash point performance. In Comparative Examples 2 and 3, due to the lack of high refractive index hardening liquid and organic particles, the coating liquid cannot form a refractive index difference and cannot form internal fog. Since the external light cannot penetrate the anti-glare film, diffuse reflection occurs, and the black acrylic plate is tested to be white. Due to the large particle size of the inorganic particles, the flash point effect is poor. In Comparative Example 4, since no inorganic particles are added, the full-line haze formed is basically internal haze. Since all the external light penetrates the anti-glare film, mirror reflection occurs, resulting in the 60° mirror gloss being too high, which is easy to dazzle the eyes (i.e., like looking in a mirror).
[0085] The above is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. All equivalent changes and modifications made according to the content of the present invention are included in the patent scope of the present invention.
Claims
1. A hardening layer coating liquid, characterized in that: The coating solution comprises a high-refractive index hardening solution, a low-refractive index hardening solution, organic particles, inorganic particles and butanone; The refractive index of the low-refractive-index hardening liquid is in the range of 1.45 to 1.49, and the refractive index of the high-refractive-index hardening liquid is in the range of 1.60 to 1.65; During the preparation process, the inorganic particles are prepared into inorganic particle ball-milling liquid; the hardening layer coating liquid includes 25% to 39% of low refractive index hardening liquid, 11% to 25% of high refractive index hardening liquid, 2% to 5% of organic particles, 30% to 35% of inorganic particle ball-milling liquid, and 10% to 17% of butanone; the percentages are weight percentages; the addition ratio of the high refractive index hardening liquid to the low refractive index hardening liquid is 1:1-1:3.55; the inorganic particle ball-milling liquid contains 15% of silica inorganic particles; The low-refractive index curing liquid comprises hexafunctional polyurethane acrylic resin polymer, trifunctional acrylate monomer and difunctional acrylate monomer; the high-refractive index curing liquid comprises hexafunctional polyurethane acrylic resin polymer, tetrafunctional acrylic monomer and zirconium oxide nanoparticles with a particle size of 20-50nm.
2. The hardening layer coating liquid according to claim 1, characterized in that: The inorganic particles are silicon dioxide inorganic particles, and the organic particles are acrylic resin organic particles; the particle size of the organic particles is 0.5-2.0 μm, and the particle size of the inorganic particles is 2-3 μm.
3. The hardening layer coating liquid according to claim 1, characterized in that: The inorganic particle ball milling liquid comprises inorganic silicon dioxide particles, propylene glycol methyl ether and butanone; the inorganic silicon dioxide particles are dispersed in the propylene glycol methyl ether and butanone.
4. An anti-glare film, characterized in that: The anti-glare film comprises a substrate and a hardened layer, wherein the hardened layer is formed by curing the hardened layer coating solution according to any one of claims 1 to 3.
5. The anti-glare film according to claim 4, characterized in that: The substrate is a triacetyl cellulose film, a polyethylene terephthalate film, or a polycarbonate film.
6. The anti-glare film according to claim 4, characterized in that: The thickness of the substrate is 50µm-250µm, and the thickness of the hardened layer is 4µm-8µm.