Method for producing porous alpha-alumina catalyst carrier
By optimizing the pore structure of transitional alumina and depositing silver, the problem of performance degradation of porous α-alumina catalyst carriers under high temperature and high pressure conditions has been solved, and the production efficiency and selectivity of ethylene oxide have been improved.
Patent Information
- Application Number
- CN202180045865.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-06-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-06-25
AI Technical Summary
The performance of existing porous α-alumina catalyst carriers decreases under high temperature and high pressure conditions, and it is difficult to optimize the pore structure to improve catalytic activity and selectivity, resulting in low ethylene oxide production efficiency.
High-purity transitional alumina is used as the precursor material, and its pore structure is optimized through the preparation and calcination process to form a porous α-alumina catalyst carrier with high pore volume and surface area, and silver is deposited on its surface to improve catalytic activity.
The selectivity and activity of the catalyst are significantly improved, the formation of unwanted reaction products is reduced, the production efficiency of ethylene oxide is improved, and high mechanical stability is maintained.
Smart Images

Figure GDA0004991268130000304 
Figure GDA0004991268130000311 
Figure GDA0004991268130000323
Abstract
Description
[0001] The present invention relates to a method for producing a porous α-alumina catalyst support, a catalyst for producing ethylene oxide by gas phase oxidation of ethylene comprising silver deposited on the porous alumina catalyst support, a method for preparing the catalyst and a method for producing ethylene oxide by gas phase oxidation of ethylene.
[0002] Alumina (Al2O3) is commonly found in supports and / or catalysts for many heterogeneous catalytic processes. Some of these catalytic processes occur under conditions of high temperature, high pressure and / or high water vapor pressure. It is well known that alumina has many crystalline phases, such as alpha-alumina (commonly expressed as α-alumina or α-Al2O3), gamma-alumina (commonly expressed as γ-alumina or γ-Al2O3), and many polymorphs of alumina. Alpha-alumina is the most stable at high temperatures, but has the lowest surface area.
[0003] Gamma-alumina has a very high surface area. This is generally thought to be because the alumina molecules are in a crystal structure that is not very densely packed. Gamma-alumina forms part of a series known as activated aluminas or transition aluminas, so called because it is one of a series of aluminas that can transition to different polymorphs. Unfortunately, when gamma-alumina is heated to high temperatures, the atomic structure collapses so that the surface area is significantly reduced. The densest crystalline form of alumina is alpha-alumina.
[0004] Ethylene oxide is produced in large quantities and is primarily used as an intermediate for the production of several industrial chemicals. In the industrial oxidation of ethylene to ethylene oxide, heterogeneous catalysts comprising silver deposited on a porous support are generally used. To carry out the heterogeneously catalyzed gas-phase oxidation, an oxygen-containing gas, such as air or a mixture of pure oxygen and ethylene, is generally passed through a plurality of tubes arranged in a reactor, in which a packing of shaped catalyst bodies is present.
[0005] Catalyst performance is usually characterized by selectivity, activity, lifetime of catalyst selectivity and activity, and mechanical stability. Selectivity is the mole fraction of converted olefin that produces the desired olefin oxide. Even small improvements in selectivity and maintaining selectivity for longer periods of time can result in huge gains in process efficiency.
[0006] In order to effectively utilize the internal surface of a porous supported catalyst, the feed gas must diffuse through the pores to reach the internal surface, and the reaction products must diffuse away from these surfaces and out of the catalyst body. In a process for producing ethylene oxide by gas phase oxidation of ethylene, diffusion of ethylene oxide molecules from the catalyst body may be accompanied by undesirable chain reactions initiated by the catalyst, such as isomerization to acetaldehyde followed by complete combustion to carbon dioxide, which reduces the overall selectivity of the process. The average molecular pore residence time and therefore the extent to which undesirable chain reactions occur are affected by the pore structure of the catalyst.
[0007] Therefore, the catalytic performance is affected by the pore structure of the catalyst, which essentially depends on the pore structure of the catalyst support. The term "pore structure" is understood to refer to the arrangement of the void spaces within the support matrix, including the size, size distribution, shape and interconnectivity of the pores. It can be characterized by various methods, such as mercury porosimetry, nitrogen adsorption or computed tomography. H. Giesche, "Mercury Porosimetry: A General (Practical) Overview, Part. Part. Syst. Charact. 23 (2006), 9-19 provides useful insights into mercury porosimetry.
[0008] EP 2 617 489 A1 describes a catalyst support body in which at least 80% of the pore volume is contained in pores with a diameter in the range from 0.1 to 10 μm and at least 80% of the pore volume in pores with a diameter in the range from 0.1 to 10 μm is contained in pores with a diameter in the range from 0.3 to 10 μm.
[0009] WO 03 / 072244 A1 and WO 03 / 072246 A1 each describe a catalyst support in which at least 70% of the pore volume is contained in pores with a diameter of 0.2 to 10 μm and the pores with a diameter between 0.2 and 10 μm provide a volume of at least 0.27 mL / g of support.
[0010] EP 1 927 398 A1 describes a catalyst support body having a pore size distribution with at least two maxima in the range from 0.01 to 100 μm, at least one of these maxima being in the range from 0.01 to 1.0 μm.
[0011] EP 3 639 923 A1 describes a shaped catalyst body having a multimodal pore size distribution with a maximum in the range of 0.1 to 3.0 μm and a maximum in the range of 8.0 to 100 μm, wherein at least 40% of the total pore volume of the shaped catalyst body is derived from pores with a diameter in the range of 0.1 to 3.0 μm.
[0012] WO 2008 / 054564 A1 describes a method for producing a shaped porous body comprising α-alumina platelets. US 2006 / 0281631 A1 describes the preparation of a support body comprising non-platelet alumina. US 6,165,437 A describes the preparation of α-alumina powder having a specific morphology by calcining transition alumina powder in a chlorine-containing atmosphere.
[0013] There remains a great need to enhance the performance of supported catalysts by optimizing alumina-based support structures, and there is a need for methods of producing optimized porous alpha-alumina catalyst supports. The support structure should have a high total pore volume, thereby allowing impregnation with high amounts of silver, while keeping its surface area large enough to provide optimal dispersion of catalytically active species, particularly metal species. It is also desirable to have a pore structure that results in as high a mass transport rate within the support as possible in order to minimize the average pore residence time of the molecules of reactants and products and to limit the extent to which primary reaction products, such as ethylene oxide, undergo unwanted secondary reactions during their diffusion through the pores of the supported catalyst.
[0014] The pore structure depends on factors including the size, size distribution and shape of the particles making up the support matrix. It has now been discovered that highly porous transition aluminas having low bulk density are useful raw materials for producing alpha-alumina catalyst supports having a beneficial pore structure, particularly transition aluminas having relatively high pore volumes and large pore sizes.
[0015] The present invention relates to a method for producing a porous alpha-alumina catalyst carrier, comprising:
[0016] i) preparing a precursor material comprising, based on inorganic solid content,
[0017] - at least 50 wt.% of a transition alumina having a loose bulk density of at most 600 g / L, a pore volume of at least 0.6 mL / g and a median pore diameter of at least 15 nm; and
[0018] - up to 30% by weight of hydrated aluminum oxide;
[0019] ii) shaping the precursor material into a shaped body; and
[0020] iii) calcining the shaped body to obtain a porous α-alumina support.
[0021] In the resulting porous alpha-alumina catalyst support, as shown in the examples discussed below, the majority of the total pore volume is contained in pores with diameters in the range of 0.1 to 1 μm. The pores that make up the majority of the pore volume of the support are therefore surprisingly an order of magnitude larger than the median pore size of transition aluminas.
[0022] Without wishing to be bound by theory, it is believed that pores with diameters in the range of 0.1 to 1 μm provide a particularly suitable environment for catalytic conversion after the catalytic species is applied, for example, by impregnation. These pores are small enough to provide a large surface area, while being large enough to allow rapid diffusion of the raw materials and the resulting products, thereby achieving high activity and selectivity of catalysts based on such catalyst supports. Pores with larger diameters are believed to have no significant contribution to the total surface area, thus providing less efficient reaction space. Pores with diameters less than 0.1 μm are believed to hinder the diffusion of the resulting products, which prolongs the exposure of the products to the catalytic species and triggers a chain reaction, thereby reducing selectivity.
[0023] In addition, the method of the present invention enables improved control of the properties of the resulting α-alumina support, such as BET surface area and pore volume, compared to the case where the α-alumina support is obtained by calcination of a precursor material containing α-alumina. In particular, foreign components such as silicon compounds, which are generally understood to stabilize the BET surface area and / or pore volume, are not necessary in the method of the present invention. This enables the manufacture of an α-alumina support having the desired BET surface area and pore volume but having an extremely low or zero impurity content. In addition, it was found that the α-alumina support of the present invention exhibits sufficiently high mechanical stability.
[0024] The precursor material comprises, based on the inorganic solid content, at least 50 wt.-% transition alumina. Preferably, the precursor material comprises, based on the inorganic solid content, at least 60 wt.-%, more preferably at least 70 wt.-% transition alumina, such as at least 80 wt.-% or at least 90 wt.-%, in particular 95 to 100 wt.-%.
[0025] The term "transitional alumina" is understood to mean an alumina comprising a metastable alumina phase, such as a γ-, δ-, η-, θ-, κ- or χ-alumina phase. Preferably, the transitional alumina comprises at least 80 wt.-%, preferably at least 90 wt.-%, most preferably at least 95 wt.-%, such as 95 to 100 wt.-% of a phase selected from γ-alumina, δ-alumina and / or θ-alumina, in particular a phase selected from γ-alumina and / or δ-alumina, based on the total weight of the transitional alumina.
[0026] Transition aluminas are usually in powder form. Transition aluminas are commercially available and can be obtained by thermal dehydration of hydrated aluminum compounds, particularly aluminum hydroxide and aluminum oxy-hydroxides. Suitable hydrated aluminum compounds include naturally occurring and synthetic compounds, such as aluminum trihydroxide (Al(OH)3), such as gibbsite, bayerite and nordstrandite, or aluminum oxy-monohydroxides (AlOOH), such as boehmite, pseudoboehmite and diaspore.
[0027] By gradually dehydrating the hydrated aluminum compound, the crystal lattice rearrangement is affected. For example, boehmite can be converted to gamma-alumina at about 450°C, gamma-alumina can be converted to delta-alumina at about 750°C, and delta-alumina can be converted to theta-alumina at about 1,000°C. When heated above 1,000°C, transition alumina is converted to alpha-alumina.
[0028] It is believed that the morphological properties of the resulting transitional aluminas are primarily dependent on the morphological properties of the hydrated aluminum compounds used to generate them. Accordingly, Busca, “The Surface of Transitional Aluminas: A Critical Review”, Catalysis Today, 226 (2014), 2-13, describes that aluminas derived from various pseudo-boehmite have different pore volumes and pore size distributions, even though the pseudo-boehmite has a similar surface area (160-200 m 2 / g).
[0029] In a preferred embodiment, the transitional alumina comprises non-platelet crystals. The term "non-platelet" refers to any form other than a platelet form, such as an elongated form, such as a rod or needle, or a form having approximately the same size in all three spatial directions. In a preferred embodiment, the transitional alumina comprises non-platelet crystals, for example, rod-shaped crystals as described, for example, in WO 2010 / 068332 A1, or blocky crystals as described, for example, in Busca, "The Surface of Transitional Aluminas: A Critical Review", Catalysis Today, 226 (2014), 2-13, see Figure 2 c, 2d and 2e with Figure 2 Comparison of a, 2b and 2f. Preferably, the average crystal size of the transition alumina as determined from the XRD pattern by the Scherrer equation is at least 5 nm, preferably at least 7 nm, most preferably at least 10 nm.
[0030] Various synthesis methods for obtaining crystalline boehmite-type aluminum oxides having a high pore volume and a large surface area and a high thermal stability are known, for example, from WO 00 / 09445 A2, WO 01 / 02297 A2, WO 2005 / 014482 A2 and WO 2016 / 022709 A1. For example, WO 2016 / 022709 A1 describes a crystalline boehmite-type aluminum oxide having a pore volume of 115 to 120 mm. Average pore size, 250 to 350 kg / m 3 The bulk density and 0.8 to 1.1m 3 / g of pore volume, prepared by precipitation of basic aluminum salts with acidic aluminum salts at controlled pH and temperature. Transition aluminas made by heat treatment of these boehmite aluminas and having the properties as defined in the present claims are particularly suitable transition aluminas for use in the process of the present invention.
[0031] Prior to the heat treatment, the hydrated aluminum compound may be washed, for example, with demineralized water to reduce impurities and allow a high purity transition alumina to be obtained. For example, according to Chen et al., J. Solid State Chem., 265 (2018), 237 to 243, crystalline boehmite obtained from gibbsite by a hydrothermal process is preferably washed prior to the heat treatment.
[0032] High purity transition alumina is preferred to limit the content of impurities, such as sodium or silicon, in the catalyst support. High purity transition alumina can be obtained, for example, by the so-called Ziegler process (sometimes referred to as the ALFOL process) and its variants as described in Busca, "The Surface of Transitional Aluminas: A Critical Review", in Catalysis Today, 226 (2014), 2-13. Other processes based on the precipitation of aluminates, such as sodium aluminate, tend to produce transition aluminas with relatively large amounts of impurities, such as sodium.
[0033] The transition alumina used in the present invention preferably has a total content of alkali metals, such as sodium and potassium, of at most 1,500 ppm, more preferably at most 600 ppm, and most preferably from 10 ppm to 200 ppm, relative to the total weight of the transition alumina. Various washing methods are known that can reduce the alkali metal content of the transition alumina and / or the catalyst support obtained therefrom. Washing may include washing with alkali, acid, water or other liquids.
[0034] US2,411,807 A describes that the sodium oxide content in an aluminum oxide precipitate can be reduced by washing with a solution containing hydrofluoric acid and another acid. WO 03 / 086624A1 describes pre-treating a support with an aqueous lithium salt solution to remove sodium ions from the surface of the support. US 3,859,426 A describes the purification of refractory oxides such as aluminum oxide and zirconium oxide by repeated washing with hot deionized water. WO 2019 / 039930 describes a method for purifying aluminum oxide in which metallic impurities are removed by extraction with alcohol.
[0035] In addition to alkali metals, it is also preferred to control the levels of other naturally occurring impurities.
[0036] The transition alumina used in the present invention preferably has a total content of alkaline earth metals such as calcium and magnesium of at most 2,000 ppm, more preferably at most 600 ppm, most preferably at most 400 ppm, relative to the total weight of the transition alumina.
[0037] The transition alumina used in the present invention preferably has a silicon content of at most 10,000 ppm, preferably at most 2,000 ppm, most preferably at most 700 ppm, relative to the total weight of the transition alumina.
[0038] The transition alumina used in the present invention preferably has an iron content of at most 1,000 ppm, more preferably at most 600 ppm, most preferably at most 300 ppm, relative to the total weight of the transition alumina.
[0039] The transition alumina used in the present invention preferably has a content of metals other than those mentioned above, such as titanium, zinc, zirconium and lanthanum, of at most 1,000 ppm, more preferably at most 400 ppm, most preferably at most 100 ppm, relative to the total weight of the transition alumina.
[0040] The transition alumina has a loose bulk density of up to 600 g / L. The term "loose bulk density" is understood to be the "freely settled" or "poured" density. The "loose bulk density" is therefore different from the "tapped density", in which a specified mechanical tapping sequence is applied and generally a higher density is obtained. The loose bulk density can be determined by pouring the transition alumina into a graduated cylinder, suitably through a funnel, taking care not to move or vibrate the cylinder. The volume and weight of the alumina are determined. The loose bulk density is determined by dividing the weight in grams by the volume in litres.
[0041] A low loose bulk density may indicate high porosity and high surface area. Preferably, the transition alumina has a loose bulk density of 50 to 600 g / L, more preferably 100 to 550 g / L, most preferably 150 to 500 g / L, especially 200 to 500 g / L or 200 to 450 g / L.
[0042] The transition alumina has a pore volume of at least 0.6 mL / g. Preferably, the transition alumina has a pore volume of 0.6 to 2.0 mL / g or 0.65 to 2.0 mL / g, more preferably 0.7 to 1.8 mL / g, most preferably 0.8 to 1.6 mL / g.
[0043] The transitional alumina has a median pore size of at least 15 nm. The term "median pore size" is used herein to denote the median pore size by surface area, i.e. the median pore size (area) is the pore size at the 50th percentile of the cumulative surface area plot. Preferably, the transitional alumina has a median pore size of 15 to 500 nm, more preferably 20 to 450 nm, most preferably 20 to 300 nm, such as 20 to 200 nm.
[0044] Mercury porosimetry and nitrogen adsorption are widely used to characterize the pore structure of porous materials, as these methods allow the determination of porosity and pore size distribution in one step. Both techniques are based on different physical interactions and optimally cover a specific range of pore sizes.
[0045] In many cases, nitrogen adsorption constitutes a sufficiently accurate determination method, especially for smaller pores. Thus, the pore volume and median pore size of transition aluminas can be determined by nitrogen adsorption. Nevertheless, nitrogen adsorption may not adequately represent larger pores.
[0046] Nitrogen adsorption measurements can be performed using a Micrometrics ASAP 2420. Unless otherwise indicated, nitrogen porosity is determined herein according to DIN 66134. Barrett-Joyner-Halenda (BJH) pore size and volume analysis is performed to obtain the total pore volume ("BJH desorption cumulative pore volume") and the median pore size ("BJH desorption mean pore diameter").
[0047] Mercury porosimetry can be performed using a Micrometrics AutoPore V 9600 mercury porosimeter (140 degree contact angle, 485 dynes / cm Hg surface tension, 61,000 psia maximum head pressure). Data were acquired for total pore volume and median pore size for transition aluminas in the pore size range of 3 nm to 1 μm.
[0048] For sufficient accuracy, the pore volume and median pore size of the transition alumina reported are from nitrogen adsorption if the median pore size from mercury porosimetry is less than 50 nm; or, if the median pore size from mercury porosimetry is 50 nm or greater, the pore volume and median pore size of the transition alumina reported are from mercury porosimetry.
[0049] In order to avoid distorting the results, nitrogen adsorption measurements and mercury porosimetry should be performed on samples that have been treated to remove physically adsorbed species, such as water, from the sample. Suitable methods are described below.
[0050] Transition aluminas usually have a density between 20 and 500 m 2 The BET surface area is in the range of 1000 Å / g. The BET method is a standard well-known and widely used method for measuring the surface area of solids by physical adsorption of gas molecules in surface science. Unless otherwise specified, the BET surface area is determined here according to DIN ISO 9277 using nitrogen physical adsorption at 77 K. Unless otherwise specified, the terms "BET surface area" and "surface area" are used equivalently herein.
[0051] The BET surface area of the transition alumina can vary within a relatively large range and can be adjusted by varying the thermal dehydration conditions of the hydrated aluminum compound used to obtain the transition alumina. Preferably, the transition alumina has a BET surface area of 20 to 200 m 2 / g, more preferably 50 to 200 m 2 / g or 50 to 150m 2 / g of BET surface area.
[0052] Suitable transition aluminas are commercially available. In some cases, such commercially available transition aluminas are classified as "medium porosity aluminas" or particularly "high porosity aluminas". Suitable transition aluminas include Alumina, Alumina and Alumina, all from Sasol. TH and TM series of products, and Versal VGL series of products from UOP.
[0053] Transition alumina can be used in its commercially available ("unground") form. This commercial form of alumina comprises single particles or agglomerates (secondary particles) of particles (primary particles). For example, the average (secondary) particle size (e.g. D 50 ) of 25 μm may contain submicron primary particles. The average particle size (D) as referred to herein 50 ) is understood to refer to the particle size of the secondary alumina particles (D 50 ).
[0054] Unground transition alumina powders generally have a D of 10 to 100 μm, preferably 20 to 50 μm.50 Particle size. In addition, transition alumina that has been ground to break up the particles into the desired particle size may be used. Suitably, the transition alumina may be ground in the presence of a liquid, and preferably in the form of a suspension. Alternatively, the grinding may be carried out by dry ball milling. The ground transition alumina powder typically has a D of 0.5 to 8 μm, preferably 1 to 5 μm. 50 Particle size. The particle size of transition alumina can be measured by a laser diffraction particle size analyzer, such as the Malvern Mastersizer 2000, using water as the dispersion medium. The method involves dispersing the particles by ultrasonic treatment, thereby breaking the secondary particles into primary particles. This sonication is continued until no D is observed. 50 Further changes in the values, for example after 3 minutes of sonication.
[0055] In a preferred embodiment, the transition alumina comprises at least 50 wt.%, preferably 60 to 90 wt.%, of a transition alumina having an average particle size of 10 to 100 μm, preferably 20 to 50 μm, based on the total weight of the transition alumina. Optionally, the transition alumina may comprise, for example, up to 50 wt.%, preferably 10 to 40 wt.%, of a transition alumina having an average particle size of 0.5 to 8 μm, preferably 1 to 5 μm, based on the total weight of the transition alumina.
[0056] The precursor material comprises up to 30 wt% hydrated alumina based on the inorganic solids content. Preferably, the precursor material comprises 1 to 30 wt% hydrated alumina based on the inorganic solids content, more preferably 1 to 25 wt%, most preferably 1 to 20 wt%, such as 3 to 18 wt%.
[0057] The term "hydrated aluminum oxide" is understood to mean hydrated aluminum compounds as described above, in particular aluminum hydroxide and aluminum oxy-hydroxides. A discussion of the nomenclature of aluminum oxides can be found in K. Wefers and C. Misra, "Oxides and Hydroxides of Aluminum", Alcoa Laboratories, 1987. Suitable hydrated aluminum compounds include naturally occurring compounds and synthetic compounds, such as aluminum trihydroxide (Al(OH)3), such as gibbsite, bayerite and nordstrandite, or aluminum oxy-monohydroxides (AlOOH), such as boehmite, pseudoboehmite and diaspore.
[0058] Preferably, the hydrated alumina comprises boehmite and / or pseudo-boehmite. In a preferred embodiment, the total amount of boehmite and pseudo-boehmite constitutes at least 80% by weight of the hydrated alumina, more preferably at least 90% by weight, most preferably at least 95% by weight, such as 95 to 100% by weight. In a particularly preferred embodiment, the amount of boehmite constitutes at least 80% by weight of the hydrated alumina, more preferably at least 90% by weight, most preferably at least 95% by weight, such as 95 to 100% by weight.
[0059] Suitable hydrated aluminas are commercially available and include those from Sasol Series of products, preferred TH and TM series products, and from UOP Series of products.
[0060] Without wishing to be bound by theory, it is believed that the presence of hydrated alumina improves the mechanical stability of the support. It is particularly believed that nano-scale highly dispersed hydrated alumina suitable for colloidal applications, such as Alumina from Sasol or The boehmite series exhibit high binding forces and can enhance the mechanical stability of the support particularly efficiently. Generally speaking, the use of such nanoscale highly dispersed hydrated alumina to improve mechanical stability enables a relatively low BET surface area to be achieved under given calcination conditions.
[0061] The hydrated alumina may be partially or completely replaced by a suitable alternative aluminum compound while substantially maintaining the mechanical stability of the support. Such suitable alternative aluminum compounds include aluminum alkoxides, such as aluminum ethoxide and aluminum isopropoxide, aluminum nitrate, aluminum acetate and aluminum acetylacetonate.
[0062] The precursor material optionally comprises a liquid. The presence, type and amount of the liquid may be selected according to the desired processing properties of the precursor material. For example, the presence of the liquid may be desirable to obtain a ductile precursor material.
[0063] The liquid is typically selected from water, in particular deionized water, and / or an aqueous solution containing a soluble and / or dispersible compound selected from salts such as ammonium acetate and ammonium carbonate; acids such as formic acid, nitric acid, acetic acid and citric acid; bases such as ammonia, triethylamine and methylamine; surfactants such as triethanolamine, poloxamers, fatty acid esters and alkyl polyglucosides; submicron particles including metal oxides such as silicon dioxide, titanium dioxide and zirconium oxide; clays; and / or polymer particles such as polystyrene and polyacrylates. The liquid is preferably water, most preferably deionized water. The typical amount of the liquid varies in the range of 10 to 60% by weight based on the inorganic solid content of the precursor material.
[0064] The precursor material may contain additional components, which may be processing aids or purposely introduced to adjust the physical properties of the final catalyst support. These components include pore-forming materials, lubricants, organic binders and / or inorganic binders.
[0065] The precursor material may contain organic materials such as pore forming materials, lubricants and organic binders in a total amount of 1.0 to 60 wt %, preferably 3 to 50 wt %, based on the total weight of the precursor material.
[0066] The precursor material may contain the lubricant and the organic binder in an amount of 1.0 to 10 wt %, preferably 3 to 8 wt %, based on the total weight of the precursor material.
[0067] The pore-forming material can be used to provide additional and / or wider pores in the support. The additional pore volume of the wider pores can also advantageously allow for more efficient impregnation of the support during production of the catalyst. Preferably, the pore-forming material is substantially completely removed during heat treatment of the shaped body. The pore-forming function can be achieved by different mechanisms, such as combustion (i.e., burning), decomposition, sublimation, or volatilization in the presence of oxygen.
[0068] Suitable pore-forming materials include
[0069] - thermally decomposable materials, such as oxalic acid, malonic acid, ammonium carbonate or ammonium bicarbonate;
[0070] - burnout materials, for example thermally combustible biomaterials, such as gum arabic, sawdust and flour, in particular groundnut shell flour, such as pecan shell flour, cashew shell flour, walnut shell flour or hazelnut shell flour; and / or
[0071] -Organic polymers, such as
[0072] - polysaccharides, such as starches, gums, cellulose and cellulose derivatives, including substituted celluloses, such as methyl cellulose, ethyl cellulose and carboxyethyl cellulose, and cellulose ethers;
[0073] - polyolefins, such as polyethylene and polypropylene;
[0074] - aromatic polymers, such as polystyrene;
[0075] - polycarbonates, such as poly(propylene carbonate); and
[0076] - lignin;
[0077] -Carbonaceous materials, such as
[0078] -graphite;
[0079] - powdered carbonaceous compounds, such as coke, or activated carbon powder; and
[0080] - Milled or unmilled carbon fibers.
[0081] Thermally decomposable materials, such as oxalic acid, malonic acid, ammonium bicarbonate or ammonium carbonate, decompose upon thermal treatment and break down into volatile smaller molecules that may be combustible or non-combustible. For example, malonic acid decomposes upon thermal treatment to produce primarily acetic acid and carbon dioxide. Such thermally decomposable materials can provide certain advantages in industrial processes because these materials can generally be obtained from industrial sources at a purity that will not introduce contaminants into the carrier.
[0082] In order to avoid the formation of a potentially explosive atmosphere, when using a thermally decomposable material, the calcination of the shaped body is preferably carried out in an atmosphere with a reduced oxygen content, such as up to 10% by volume or up to 5% by volume of oxygen. If the thermal decomposition takes place at a relatively low temperature, the process can be safely controlled to be well below the ignition temperature of the potentially combustible molecules formed when the decomposable material decomposes. This allows safe operation of the heat treatment even in the case of a relatively high oxygen concentration in the atmosphere within the heat treatment device. In this case, an air atmosphere can be used.
[0083] Suitable lubricants include
[0084] -graphite;
[0085] - petrolatum, mineral oil or grease;
[0086] fatty acids, such as stearic acid or palmitic acid; fatty acid salts, such as stearates, such as potassium stearate, magnesium stearate and aluminium stearate, or palmitates, such as potassium palmitate, magnesium palmitate and aluminium palmitate; fatty acid derivatives, such as esters of fatty acids, in particular esters of saturated fatty acids, such as stearic acid esters, such as methyl stearate and ethyl stearate; and / or
[0087] - malleable organic solids, for example waxes, for example paraffin, cetyl palmitate.
[0088] It is preferred that the lubricant does not introduce inorganic contaminants into the catalyst support. Among the above lubricants, graphite, stearic acid, aluminum stearate and combinations thereof are preferred.
[0089] Organic binders, sometimes also referred to as "temporary binders", can be used to improve the ductility of the precursor material and maintain the integrity of the "green" phase, i.e., the unfired phase, wherein the mixture is formed into a shaped body. Preferably, the organic binder is substantially completely removed during heat treatment of the shaped body.
[0090] Suitable organic binders include
[0091] - polyvinyl lactam polymers, such as polyvinyl pyrrolidone, or vinyl pyrrolidone copolymers, such as vinyl pyrrolidone-vinyl acetate copolymers;
[0092] - alcohols, in particular polyols such as glycols or glycerol; and / or
[0093] - Polyalkylene glycols, such as polyethylene glycol.
[0094] Advantageously, pore formers and processing aids, such as organic binders and lubricants, exhibit a low ash content. The term "ash content" is understood to relate to the non-combustible components remaining after the combustion of the organic material in air at high temperature, i.e. after the heat treatment of the shaped body. The ash content is preferably below 0.1% by weight, relative to the total weight of the organic material.
[0095] Furthermore, pore formers and processing aids, such as organic binders and lubricants, preferably do not form significant amounts of volatile additional combustible components, such as carbon monoxide, ammonia or combustible organic compounds, during the thermal treatment of the shaped body, i.e. during thermal decomposition or combustion. Excessive volatile organic components can lead to explosive atmospheres. It is preferred to apply an appropriate safety concept to the combustion or decomposition process steps.
[0096] The inorganic binder is a permanent binder that helps to fully bind the alumina particles and enhance the mechanical stability of the α-alumina molded body. Inorganic binders include those that only produce alumina when calcined. For the purpose of this application, these inorganic binders are called intrinsic inorganic binders. Such intrinsic inorganic binders include hydrated alumina as discussed above.
[0097] On the other hand, non-intrinsic inorganic binders do not produce only alumina when calcined. Suitable non-intrinsic inorganic binders should be understood to be any inorganic species conventionally used in the art, such as silicon-containing species, such as silicon dioxide or silicates, including clays, such as kaolinite, or metal hydroxides, metal carbonates, metal nitrates, metal acetates or metal oxides such as zirconium oxide, titanium dioxide or alkali metal oxides. Since non-intrinsic inorganic binders can introduce pollutants that may be harmful to catalyst performance, they are preferably included in controlled amounts. Preferably, the precursor material includes 0.0 to 5.0 weight %, preferably 0.05 to 1.0 weight % of non-intrinsic inorganic binder based on the inorganic solid content of the precursor material. In a preferred embodiment, the precursor material does not include non-intrinsic inorganic binder.
[0098] The precursor material is usually obtained by dry mixing its components and then optionally adding a liquid. The precursor material can be shaped into a shaped body by extrusion, tableting, granulation, casting, molding or microextrusion, in particular by extrusion or tableting.
[0099] The size and shape of the shaped body and thus the catalyst are selected so that the catalyst obtained from the shaped body is appropriately filled in the reactor tube. The catalyst obtained from the shaped body suitable for the catalyst of the present invention is preferably used for a reactor tube with a length of 6 to 14m and an inner diameter of 20mm to 50mm. In general, the support is composed of individuals with a maximum extension of 3 to 20mm, such as 4 to 15mm, in particular 5 to 12mm. The maximum extension is understood to refer to the longest straight line between two points on the outer circumference of the support.
[0100] The shape of the shaped body is particularly not limited and can be any technically feasible form, which depends, for example, on the forming process. For example, the carrier can be a solid extrudate or a hollow extrudate, such as a hollow cylinder. In another embodiment, the carrier can be characterized by a multi-leaf structure. A multi-leaf structure means a cylindrical structure with a plurality of void spaces, such as grooves or grooves, extending along the height of the cylinder at the outer periphery of the cylinder. Typically, these void spaces are arranged substantially equidistantly around the circumference of the cylinder.
[0101] Preferably, the support is in the shape of a solid extrudate, such as a pellet or cylinder, or a hollow extrudate, such as a hollow cylinder. In a preferred embodiment, the shaped body is formed by extrusion, such as microextrusion. In this case, the precursor material suitably comprises a liquid, in particular water, to form a ductile precursor material.
[0102] In a preferred embodiment, the extrusion comprises charging at least one solid component into a mixing device before the addition of the liquid. Preferably a mix-muller (H-roller) or a horizontal mixer, such as Mixer (from Gebrüder The formation of an extrudable paste of the precursor material can be monitored and controlled based on data reflecting the power consumption of the mixing device.
[0103] The precursor material is usually extruded through a die. The cross section of the die opening is adjusted according to the desired geometry of the shaped body.
[0104] The extrusion die may comprise a substrate and a mandrel, wherein the substrate substantially determines the circumferential shape of the shaped body, and the mandrel substantially determines the form, size and position of the channel (if present). Suitable extrusion dies are described in, for example, WO 2019 / 219892 A1.
[0105] The geometry of the shape of the shaped body is defined by the geometry of the extrusion apparatus through which the precursor material is extruded. Typically, the geometry of the shape of the extrudate differs slightly from the geometry of the extrusion apparatus while having substantially the geometric properties described above. Due to the high temperatures required to form the alpha alumina and the shrinkage of the extrudate as it cools, the absolute dimensions of the shape are typically slightly less than the dimensions of the extrudate. The degree of shrinkage depends on the temperature applied during calcination and the composition of the shaped body. Therefore, the dimensions of the extrusion die should be routinely adjusted in a manner that takes into account the shrinkage of the extrudate during subsequent calcination.
[0106] When a molded body comprises a plurality of channels, the axes of the channels generally run in parallel. However, the molded body may be slightly bent or twisted along its z-axis (height). The shape of the cross section of the channel may be slightly different from the perfect geometry envisaged above. When a large number of molded bodies are obtained, individual channels of a few molded catalyst bodies may be closed. Typically, due to the production process, the face sides of the molded catalyst bodies in the xy plane are more or less uneven rather than smooth. The height of the molded body (the length of the molded body in the z direction) is generally not exactly the same for all molded bodies, but rather constitutes a certain distribution having an average height as its arithmetic mean.
[0107] The extrudate is preferably cut to the desired length while still wet. The extrudate is preferably cut at an angle substantially perpendicular to its circumferential surface. In order to reduce undesirable deviations from the geometry of the extrusion device, the extrudate may alternatively be cut at an angle of up to 30°, such as 10° or 20°, relative to the angle perpendicular to the circumferential surface of the extrudate.
[0108] Geometric deviations such as those caused during the extrusion process and / or in the further processing of the extrudate, such as a cutting step, may also generally be present in the porous α-alumina catalyst support of the invention obtained in the process of the invention without substantially reducing the beneficial effects of its pore structure. The skilled person understands that, due to the inherent imprecision of all production methods to a certain extent, perfect geometric forms cannot be obtained at all.
[0109] In another embodiment, the precursor material is formed into a shaped body using a microextrusion method, such as the method described in WO 2019 / 072597 A1.
[0110] In another embodiment, the precursor material is formed into a shaped body using a gel casting method, such as the method described in WO 2020 / 053563A1.
[0111] In another embodiment, the precursor material is formed into a molded body by tableting. In this case, the precursor material does not usually contain liquid. Tableting is a press agglomeration process. Powdered or previously agglomerated bulk materials are introduced into a pressing tool with a mold between two punches, compacted and molded to obtain a solid compact by uniaxial compression. This operation is divided into four parts: metering introduction, compaction (elastic deformation), plastic deformation and discharge. For example, tableting is carried out on a rotary press or an eccentric press.
[0112] If necessary, the upper punch and / or the lower punch may contain projecting pins to form internal channels. It is also possible to equip the pressing punch with a plurality of movable pins so that the punch can be made, for example, of four pins to create a shaped body with four holes (channels). Typical design features of such tools can be found, for example, in US 8,865,614 B2.
[0113] The pressing force during tableting influences the compaction of the bulk material. In practice, it has been found to be useful to set the lateral compressive strength of the porous alpha-alumina catalyst support in a targeted manner by selecting an appropriate pressing force and to check this by random sampling. For the purposes of the present invention, the lateral compressive strength is the force which breaks the porous alpha-alumina catalyst support between two parallel plates, the two flat, parallel end faces of the catalyst support being at right angles to the parallel plates.
[0114] For tableting, it is generally preferred to use a lubricant, especially those discussed above. To improve the tableting properties, a pre-granulation and / or sieving step may be used. For pre-granulation, a roll compactor may be used, such as the Further information on tableting, in particular on pregranulation, sieving, lubricants and tools, can be found in WO 2010 / 000720 A2.
[0115] Prior to calcination, the shaped body may be dried, particularly when the precursor material comprises a liquid. Suitably, the drying is carried out at a temperature of 20 to 400° C., particularly 30 to 300° C., such as 70 to 150° C. Drying is generally carried out for a period of up to 100 hours, preferably 0.5 to 30 hours, more preferably 1 to 16 hours.
[0116] Drying can be carried out in any atmosphere, such as in an oxygen-containing atmosphere, such as air, nitrogen or helium, or a mixture thereof, preferably in air. Drying is usually carried out in an oven. The type of oven is particularly unrestricted. For example, a fixed circulating air oven, a rotary cylindrical oven or a conveyor oven can be used. Heat can be applied directly and / or indirectly.
[0117] Preferably, flue gases (exhaust gases) from a combustion process having a suitable temperature are used in the drying step. The flue gases can be used in diluted or undiluted form to provide direct heating and remove evaporated moisture and other components released from the shaped bodies. The flue gases are usually passed through an oven as described above. In another preferred embodiment, exhaust gases from a calcination process step are used for direct heating.
[0118] Drying and calcining can be carried out sequentially in separate apparatuses and can be carried out in a batch or continuous process. Intermittent cooling can be applied. In another embodiment, drying and calcining are carried out in the same apparatus. In a batch process, a time-resolved temperature ramp (program) can be applied. In a continuous process, a space-resolved temperature ramp (program) can be applied, for example when the shaped body is continuously moved through regions (zones) of different temperatures.
[0119] Preferably, heat integration measures as known in the art are applied to improve energy efficiency. For example, relatively hot exhaust gas from one process step or stage can be used to heat feed gas, device or shaped body in another process step or stage by direct (mixing) or indirect (heat exchanger) means. Likewise, heat integration can also be used to cool relatively hot exhaust gas streams before further processing or discharge.
[0120] The shaped body is calcined to obtain a porous alpha-alumina catalyst support.Thus, the calcination temperature and duration are sufficient to convert at least a portion of the transition alumina into alpha-alumina, which means to convert at least a portion of the metastable alumina phase of the transition alumina into alpha-alumina.
[0121] The obtained porous α-alumina catalyst support generally contains a high proportion of α-alumina, for example at least 80 wt %, preferably at least 90 wt %, more preferably at least 95 wt %, most preferably at least 97.5 wt %, based on the total weight of the support. The amount of α-alumina can be determined, for example, by X-ray diffraction analysis.
[0122] Typically, calcination is carried out at a temperature of at least 1300° C., such as at least 1400° C., more preferably at least 1450° C. Preferably, calcination is carried out at an absolute pressure of 0.5 to 35 bar, especially 0.9 to 1.1 bar, for example at atmospheric pressure (about 1013 mbar). Typical total heating times are 0.5 to 100 hours, preferably 2 to 20 hours.
[0123] Calcination is usually carried out in a furnace. The type of furnace is not particularly limited. For example, furnaces such as stationary circulating air furnaces, rotary cylindrical furnaces or conveyor belt furnaces, or kilns such as rotary kilns or tunnel kilns, in particular roller kilns, can be used.
[0124] Calcination can be carried out in any atmosphere, such as in an oxygen-containing atmosphere, such as air, nitrogen or helium, or mixtures thereof. Preferably, in particular when the shaped body contains thermally decomposable material or burn-off material, calcination is at least partially or completely carried out in an oxidizing atmosphere, such as in an oxygen-containing atmosphere, such as air.
[0125] As mentioned above, pore formers and processing aids, such as organic binders and lubricants, preferably do not form significant amounts of volatile additional combustible components, such as carbon monoxide or combustible organic compounds, when the shaped body is calcined. An explosive atmosphere can be further avoided by limiting the oxygen concentration in the atmosphere during calcination, for example to an oxygen concentration below the limiting oxygen concentration (LOC) of the additional combustible components. The LOC, also known as the minimum oxygen concentration (MOC), is the limiting oxygen concentration below which oxidation cannot occur.
[0126] Suitably, a recycle stream of dilute air or gas with a limited oxygen content can be used together with an oxygen make-up stream, which also compensates for the gas purge stream. In another approach, an explosive atmosphere can be avoided by limiting the rate of formation of additional combustible components. The rate of formation of additional combustible components can be limited by heating to the calcination temperature by means of a slow temperature ramp or by stepwise heating. When heating stepwise, the temperature is suitably maintained at approximately the combustion temperature for several hours and then heated to a temperature of 1000° C. In a continuous calcination process, the feed rate of the shaped bodies to the calcination device, such as a furnace, can also be controlled to limit the rate of formation of additional combustible components.
[0127] Depending on the nature of the pore forming material, lubricant, organic binder and gas components, exhaust gas treatment may be applied to clean any exhaust gases obtained during calcination. Preferably, acidic or alkaline scrubbers, flare or catalytic combustion, DeNOx treatment or a combination thereof may be used for exhaust gas treatment.
[0128] Preferably, the heating is carried out in a stepwise manner. In stepwise heating, the shaped body can be placed on a high-purity and inert refractory saggar, which moves through a furnace having a plurality of heating zones, for example 2 to 8 or 2 to 5 heating zones. The inert refractory saggar can be made of α-alumina or corundum, in particular α-alumina.
[0129] The porous α-alumina catalyst carrier obtained by the method of the present invention generally has a diameter of 0.5 to 5.0 μm. 2 Preferably, the porous α-alumina catalyst support has a BET surface area in the range of 0.5 to 4.5 m 2 / g, more preferably 1.0 to 4.5 m 2 / g, most preferably 1.0 to 4.0 m 2 The BET surface area is in the range of 1000 Å / g.
[0130] The porous α-alumina catalyst support generally has a total pore volume of at least 0.2 mL / g as measured by mercury porosimetry. As measured by mercury porosimetry, the pore volume contained in the pores with a diameter in the range of 0.1 to 1 μm in the porous α-alumina catalyst support obtained by the method of the present invention is generally at least 40% of the total pore volume. Preferably, the pore volume contained in the pores with a diameter in the range of 0.1 to 1 μm in the porous α-alumina catalyst support is at least 50% of the total pore volume, more preferably at least 55% of the total pore volume, and most preferably at least 60% of the total pore volume, such as at least 65% or at least 70% of the total pore volume. Typically, the pore volume contained in the pores with a diameter in the range of 0.1 to 1 μm in the porous α-alumina catalyst support obtained by the method of the present invention is preferably 40 to 99%, more preferably 45 to 99%, and most preferably 50 to 97% of the total pore volume.
[0131] The porous α-alumina catalyst support generally has a ratio r of at most 0.50 of the pore volume contained in pores with a diameter in the range of greater than 1 to 10 μm to the pore volume contained in pores with a diameter in the range of 0.1 to 1 μm. pv Preferably, the ratio r pv In the range of 0.0 to 0.45, more preferably 0.0 to 0.40 or 0.0 to 0.35.
[0132] The porous alpha-alumina support generally comprises at least 80 wt%, preferably at least 90 wt%, more preferably at least 95 wt%, and most preferably at least 97.5 wt% alpha-alumina based on the total weight of the support.
[0133] In one embodiment, the porous alpha-alumina catalyst support comprises at least 80 wt.% alpha-alumina and has
[0134] -0.5 to 5.0m 2 BET surface area in the range of 1000 Å / g;
[0135] - a total pore volume of at least 0.2 mL / g as measured by mercury porosimetry; and
[0136] - the pore volume contained in pores with a diameter in the range of 0.1 to 1 μm, as determined by mercury porosimetry, is at least 40% of the total pore volume;
[0137] The ratio of the pore volume contained in pores with diameters greater than 1 to 10 μm to the pore volume contained in pores with diameters in the range of 0.1 to 1 μm is r pv The maximum value is 0.50.
[0138] In a preferred embodiment, the porous α-alumina carrier is in the form of a single shaped body, such as the shape described above. Preferably, the porous α-alumina catalyst carrier is in the form of a single shaped body having a circumferential surface, a first side surface, a second side surface, and at least one internal channel extending from the first side surface to the second side surface.
[0139] Preferably, the geometric surface area SA of the catalyst support geo The geometric volume V of the catalyst support geo The quotient (SA geo / V geo ) is at least 1.1 mm -1 and up to 10mm -1 Preferably, SA geo With V geo The quotient is 1.15mm -1 Up to 5.0mm -1 The range is preferably 1.2 mm. -1 Up to 2.0mm -1 The geometric surface area SA geo and the geometric volume V geo is derived from the external macroscopic dimensions of the porous α-alumina catalyst support, taking into account the cross-sectional area, height and, if applicable, the number of internal channels. In other words, the geometric volume V of the catalyst support geo is the volume of a solid structure with the same external dimensions minus the volume occupied by the channels. Similarly, the geometric surface area SA geo It consists of a circumferential surface, first and second face side surfaces and, if applicable, a surface defining a channel. The first and second face side surfaces are respectively the surface area enclosed by the circumference of the face side less the cross-sectional area of the channel. The surface defining a channel is the surface area of the channel lining.
[0140] SA in the preferred range geo With V geo The quotient of makes it possible to obtain better contact of the reaction gases with the catalyst surface, which promotes the conversion of the reactants and limits internal diffusion phenomena, thereby improving the reaction selectivity.
[0141] The porous α-alumina support preferably has no wash-coat particles or a wash-coat layer on its surface in order to sufficiently maintain the porosity of the uncoated support.
[0142] The porous α-alumina catalyst support may contain impurities such as sodium, potassium, magnesium, calcium, silicon, iron, titanium and / or zirconium. These impurities may be introduced by components of the precursor material, in particular an inorganic binder or a mechanical stability enhancer. In one embodiment, the porous α-alumina catalyst support comprises, relative to the total weight of the support,
[0143] - sodium and potassium in amounts up to 1,500 ppmw;
[0144] - up to 2,000 ppmw calcium;
[0145] - up to 1,000 ppmw magnesium;
[0146] - up to 10,000 ppmw of silicon;
[0147] - up to 1,000 ppmw of titanium;
[0148] - up to 1,000 ppmw iron; and / or
[0149] - Up to 10,000 ppmw zirconium.
[0150] Low sodium content is preferred to prevent metal segregation of the load and to prevent compositional changes of the load.
[0151] The invention further relates to a shaped catalyst body for producing ethylene oxide by selective gas phase oxidation (epoxidation) of ethylene, i.e. an epoxidation catalyst, comprising at least 15% by weight of silver, relative to the total weight of the shaped catalyst body, deposited on a porous alpha-alumina catalyst support as described above.
[0152] The shaped catalyst body generally comprises 15 to 70% by weight of silver, preferably 20 to 60% by weight of silver, more preferably 25 to 50% by weight or 30 to 50% by weight of silver, relative to the total weight of the shaped catalyst body. A silver content within this range enables a favorable balance between the turnover rate caused by each shaped catalyst body and the cost efficiency of preparing the shaped catalyst body.
[0153] In addition to silver, the shaped catalyst body may also contain one or more promoters. Promoters refer to components that provide improvements in one or more catalytic properties of the catalyst compared to a catalyst that does not contain the components. Promoters can be any of those species known in the art for improving the catalytic properties of silver catalysts. Examples of catalytic properties include operability (resistance to runaway), selectivity, activity, turnover rate, and catalyst life.
[0154] The shaped catalyst body may contain a promoting amount of a transition metal or a mixture of two or more transition metals. Suitable transition metals may include, for example, elements from Group IIIB (scandium), Group IVB (titanium), Group VB (vanadium), Group VIB (chromium), Group VIIB (manganese), Group VIIIB (iron, cobalt, nickel), Group IB (copper), and Group IIB (zinc) of the periodic table and combinations thereof. More typically, the transition metal is a pre-transition metal, i.e., from Group IIIB, IVB, VB, or VIB, such as hafnium, yttrium, molybdenum, tungsten, rhenium, chromium, titanium, zirconium, vanadium, tantalum, niobium, or a combination thereof. In one embodiment, the transition metal promoter is present in a total amount of 150 ppm to 5,000 ppm, typically 225 ppm to 4,000 ppm, and most typically 300 ppm to 3,000 ppm relative to the gross weight of the shaped catalyst body, expressed as metal.
[0155] Of the listed transition metal promoters, rhenium (Re) is a particularly effective promoter for ethylene epoxidation high selectivity catalysts. The rhenium component of the shaped catalyst body may be in any suitable form, but is more typically one or more rhenium-containing compounds (eg, rhenium oxide) or complexes.
[0156] In some embodiments, the shaped catalyst body may include a promoting amount of an alkali metal or a mixture of two or more alkali metals. Suitable alkali metal promoters include, for example, lithium, sodium, potassium, rubidium, cesium, or a combination thereof. The amount of alkali metal, such as potassium, is typically 50 ppm to 5,000 ppm, more typically 300 ppm to 2,500 ppm, and most typically 500 ppm to 1,500 ppm, expressed as alkali metal, relative to the total weight of the shaped catalyst body. The amount of alkali metal depends on the amount of alkali metal contributed by the porous alpha-alumina catalyst support and the amount of alkali metal contributed by the impregnation solution described below.
[0157] Combinations of heavy alkali metals such as cesium (Cs) or rubidium (Rb) and light alkali metals such as lithium (Li), sodium (Na) and potassium (K) are particularly preferred.
[0158] The shaped catalyst body may also include a Group IIA alkaline earth metal or a mixture of two or more Group IIA alkaline earth metals. Suitable alkaline earth metal promoters include, for example, beryllium, magnesium, calcium, strontium and barium or a combination thereof. The alkaline earth metal promoter may be used in an amount similar to that of an alkali metal or transition metal promoter.
[0159] The shaped catalyst body may also include a promoting amount of a main group element or a mixture of two or more main group elements. Suitable main group elements include any element in Group IIIA (boron group) to Group VIIA (halogen group) of the periodic table. For example, the shaped catalyst body may include a promoting amount of sulfur, phosphorus, boron, halogen (e.g., fluorine), gallium, or a combination thereof.
[0160] The shaped catalyst body may also include a promoting amount of a rare earth metal or a mixture of two or more rare earth metals. Rare earth metals include any element with an atomic number of 57-103. Some examples of these elements include lanthanum (La), cerium (Ce), and samarium (Sm). The amount of rare earth metal promoter used may be similar to the amount of transition metal promoter used.
[0161] The present invention further relates to a method for preparing a shaped catalyst body as described above, comprising
[0162] a) impregnating a porous α-alumina catalyst support as described above with a silver impregnation solution, preferably under reduced pressure; and optionally subjecting the impregnated porous alumina support to drying; and
[0163] b) subjecting the impregnated porous α-alumina support to a heat treatment;
[0164] wherein steps a) and b) are optionally repeated.
[0165] It is to be understood that all embodiments of the shaped catalyst bodies also apply, if applicable, to the method for producing the shaped catalyst bodies.
[0166] In order to obtain a shaped catalyst body with a high silver content, steps i) and ii) can be repeated several times. In this case, it is understood that the intermediate product obtained after the first (or subsequent up to the penultimate) impregnation / calcination cycle contains part of the total amount of the target Ag and / or promoter concentration. This intermediate product is then impregnated again with the silver impregnation solution and calcined to obtain the target Ag and / or promoter concentration.
[0167] Any silver impregnation solution known in the art to be suitable for impregnating refractory supports may be used. The silver impregnation solution generally contains a silver carboxylate, such as silver oxalate, or a combination of a silver carboxylate and oxalic acid, in the presence of an amine complexing agent, such as a Cl-C 10- in the presence of an alkylenediamine, in particular ethylenediamine. Suitable impregnation solutions are described in EP 0 716 884 A2, EP 1 115 486 A1, EP 1 613428 A1, US 4,731,350 A, WO 2004 / 094055 A2, WO 2009 / 029419 A1, WO 2015 / 095508 A1, US 4,356,312 A, US 5,187,140 A, US 4,908,343 A, US 5,504,053 A and WO 2014 / 105770 A1. For a discussion of suitable silver impregnation solutions, see also Kunz, C. et al., On the Nature of Crystals Precipitating from Aqueous Silver Ethylenediamine Oxalate Complex Solutions., Z. Anorg. Allg. Chem., 2021, 647, DOI: 10.1002 / zaac.202100079.
[0168] During the heat treatment, the liquid components of the silver impregnation solution evaporate, so that silver compounds containing silver ions precipitate from the solution and deposit on the porous support. At least a portion of the deposited silver ions are subsequently converted to metallic silver upon further heating. Preferably, at least 70 mol% of the silver compound, preferably at least 90 mol%, more preferably at least 95 mol%, most preferably at least 99.5 mol% or at least 99.9 mol%, i.e., substantially all of the silver ions, are present, based on the total molar amount of silver in the impregnated porous α-alumina support, respectively. The amount of silver ions converted to metallic silver can be determined, for example, by an X-ray diffraction (XRD) pattern.
[0169] Heat treatment may also be referred to as calcination process. Any calcination process known in the art for this purpose may be used. Suitable examples of calcination processes are described in US 5,504,052 A, US 5,646,087 A, US 7,553,795 A, US 8,378,129 A, US 8,546,297 A, US2014 / 0187417 A1, EP 1 893 331 A1 or WO 2012 / 140614 A1. Heat treatment may be carried out in straight-through mode or with at least partial recirculation of the calcination gas.
[0170] The heat treatment is usually carried out in a furnace. The type of furnace is not particularly limited. For example, a stationary circulating air furnace, a rotary cylindrical furnace or a conveyor belt furnace can be used. In one embodiment, the heat treatment comprises passing a heated gas stream through the impregnated body. The duration of the heat treatment is usually in the range of 5 min to 20 h, preferably 5 min to 30 min.
[0171] The temperature of the heat treatment is generally in the range of 200 to 800° C., preferably 210 to 650° C., more preferably 220 to 500° C., most preferably 220 to 350° C. Preferably, the heating rate in the temperature range of 40 to 200° C. is at least 20 K / min, more preferably at least 25 K / min, such as at least 30 K / min. High heating rates can be achieved by passing the heating gas through the impregnated refractory support or the impregnated intermediate catalyst at a high gas flow rate.
[0172] Suitable flow rates of the gas may be, for example, 1 to 1,000 Nm / kg of impregnated material. 3 / h, 10 to 1,000 Nm 3 / h, 15 to 500Nm 3 / h or 20 to 300Nm 3 / h range. In a continuous process, the term "kilogram of impregnation" is understood to mean the amount of impregnation (in kg / h) multiplied by the time (in hours) that the gas stream passes through the impregnation. It has been found that when the gas stream passes through a higher amount of impregnation, for example 15 to 150 kg of impregnation, the flow rate can be selected in the lower part of the above range while achieving the desired effect.
[0173] Directly measuring the temperature of the heated impregnated body may present practical difficulties. Therefore, when heated gas is passed through the impregnated body during the heat treatment, the temperature of the heated impregnated body is taken to be the temperature of the gas just after the gas has passed through the impregnated body. In a practical embodiment, the impregnated body is placed on a suitable surface, such as a wire mesh or a perforated calcining belt, and the temperature of the gas is measured by one or more thermocouples placed adjacent to the other side of the impregnated body opposite to the side that first contacts the gas. The thermocouple is suitably placed close to the impregnated body, for example 1 to 30 mm, such as 1 to 3 mm or 15 to 20 mm from the impregnated body.
[0174] The use of multiple thermocouples can improve the accuracy of the temperature measurement. Where several thermocouples are used, these may be evenly spaced over the area where the impregnated body is located on the wire mesh or over the width of the perforated calcining belt. The average value is taken to be the temperature of the gas just after the gas has passed through the impregnated body. In order to heat the impregnated body to the temperatures mentioned above, the gas typically has a temperature of from 220 to 800° C., more preferably from 230 to 550° C., most preferably from 240 to 350° C.
[0175] Preferably, the heating is carried out in a stepwise manner. In stepwise heating, the impregnated body is placed on a moving belt which moves through a furnace having a plurality of heating zones, for example 2 to 8 or 2 to 5 heating zones. The heat treatment is preferably carried out in an inert atmosphere, such as nitrogen, helium or mixtures thereof, in particular nitrogen.
[0176] The invention further relates to a process for producing ethylene oxide by selective gas-phase oxidation (epoxidation) of ethylene, which comprises reacting ethylene and oxygen in the presence of a shaped catalyst body as described above.
[0177] It is to be understood that all embodiments of the shaped catalyst bodies also apply, if applicable, to the process for producing ethylene oxide in the presence of the shaped catalyst bodies.
[0178] The epoxidation can be carried out by all methods known to the person skilled in the art. It is possible to use all reactors which can be used in the prior art ethylene oxide production processes; for example, externally cooled shell-and-tube reactors (see Ullmann's Encyclopedia of Industrial Chemistry, 5th edition, volume A-10, pages 117-135, 123-125, VCH-Verlagsgesellschaft, Weinheim 1987) or reactors with loose catalyst beds and cooling tubes, for example DE 34 14 717 A1, EP 0 082 609 A1 and EP 0 339 748 The reactor described in .
[0179] The epoxidation is preferably carried out in at least one tubular reactor, preferably in a shell-and-tube reactor. On a commercial scale, ethylene epoxidation is preferably carried out in a multi-tube reactor containing thousands of tubes. The catalyst is filled into the tubes, which are placed in a shell filled with a coolant. In commercial applications, the inner tube diameter is typically in the range of 20 to 40 mm (see, e.g., US 4,921,681 A) or greater than 40 mm (see, e.g., WO 2006 / 102189 A1).
[0180] For the preparation of ethylene oxide from ethylene and oxygen, it is possible to carry out the reaction under the customary reaction conditions described, for example, in DE 25 21 906 A, EP 0 014 457 A2, DE 23 00 512 A1, EP 0 172 565 A2, DE 24 54 972 A1, EP 0 357 293 A1, EP 0 266 015 A1, EP 0 085 237 A1, EP 0 082 609 A1 and EP 0 339 748 A2. Inert gases such as nitrogen or gases which are inert under the reaction conditions, such as steam, methane, and optionally reaction moderators, such as halogenated hydrocarbons such as ethyl chloride, vinyl chloride or 1,2-dichloroethane, may additionally be admixed to the reaction gas comprising ethylene and molecular oxygen.
[0181] The oxygen content of the reaction gas is advantageously within a range in which no explosive gas mixture is present. Suitable compositions of the reaction gas for preparing ethylene oxide may, for example, contain ethylene in an amount of 10 to 80% by volume, preferably 20 to 60% by volume, more preferably 25 to 50% by volume, particularly preferably 25 to 40% by volume, based on the total volume of the reaction gas. The oxygen content of the reaction gas is advantageously within a range of not more than 10% by volume, preferably not more than 9% by volume, more preferably not more than 8% by volume, very particularly preferably not more than 7.5% by volume, based on the total volume of the reaction gas.
[0182] The reaction gas preferably contains a chlorine-containing reaction moderator such as ethyl chloride, vinyl chloride or 1,2-dichloroethane in an amount of 0 to 15 ppm by weight, preferably 0.1 to 8 ppm by weight, based on the total weight of the reaction gas. The remainder of the reaction gas generally contains hydrocarbons such as methane and inert gases such as nitrogen. In addition, other materials such as steam, carbon dioxide or noble gases may also be contained in the reaction gas.
[0183] The carbon dioxide concentration in the feed (i.e., the gas mixture fed into the reactor) generally depends on the catalyst selectivity and the efficiency of the carbon dioxide removal device. The carbon dioxide concentration in the feed is preferably at most 3 volume %, more preferably less than 2 volume , and most preferably less than 1 volume , relative to the total volume of the feed. An example of a carbon dioxide removal device is provided in US 6,452,027 B1.
[0184] The above-mentioned components of the reaction mixture may optionally each have a small amount of impurities. Ethylene can be used, for example, in any purity suitable for the gas phase oxidation according to the invention. Suitable purities include, but are not limited to, "polymer grade" ethylene, which usually has a purity of at least 99%, and "chemical grade" ethylene, which usually has a purity of less than 95%. Impurities usually include, in particular, ethane, propane and / or propylene.
[0185] The reaction or oxidation of ethylene to ethylene oxide is usually carried out at an elevated catalyst temperature. Preference is given to catalyst temperatures in the range of 150 to 350° C., more preferably 180 to 300° C., particularly preferably 190 to 280° C., especially preferably 200 to 280° C. The present invention therefore also provides a process as described above, wherein the oxidation is carried out at a catalyst temperature of 180 to 300° C., preferably 200 to 280° C. The catalyst temperature can be determined by thermocouples located in the catalyst bed. As used herein, the catalyst temperature or the temperature of the catalyst bed is considered to be the weight average temperature of the catalyst particles.
[0186] The reaction (oxidation) according to the present invention is preferably carried out at a pressure of 5 to 30 bar. Unless otherwise indicated, all pressures herein are absolute pressures. The oxidation is more preferably carried out at a pressure of 5 to 25 bar, such as 10 bar to 24 bar, particularly 14 bar to 23 bar. The present invention therefore also provides a method as described above, wherein oxidation is carried out at a pressure of 14 bar to 23 bar.
[0187] It has been found that the physical properties of the shaped catalyst bodies, in particular the BET specific surface area and the pore size distribution, have a significant positive influence on the catalyst selectivity. This effect is particularly pronounced when the catalyst is operated at very high working rates, i.e. at high levels of oxidized olefin production.
[0188] The process according to the invention is preferably carried out under conditions conducive to obtaining a reaction mixture containing at least 2.3% by volume of ethylene oxide. In other words, the ethylene oxide outlet concentration (ethylene oxide concentration at the reactor outlet) is preferably at least 2.3% by volume. The ethylene oxide outlet concentration is more preferably in the range of 2.5 to 4.0% by volume, most preferably in the range of 2.7 to 3.5% by volume.
[0189] The oxidation is preferably carried out in a continuous process. If the reaction is carried out continuously, the GHSV (gas hourly space velocity) is preferably in the range of 800 to 10,000 / h, preferably in the range of 2,000 to 8,000 / h, more preferably in the range of 2,500 to 6,000 / h, most preferably in the range of 4,500 to 5,500 / h, depending on the type of reactor selected, for example on the size / cross-sectional area of the reactor, the shape and size of the catalyst, wherein the indicated values are based on the volume of the catalyst.
[0190] According to a further embodiment, the present invention also relates to a process for preparing ethylene oxide (EO) by gas phase oxidation of ethylene with the aid of oxygen as disclosed above, wherein the measured EO space-time yield is greater than 180 kg EO / (m 3 cat h), preferably greater than 200 kg EO / (m 3 cath) If it is greater than 250kg EO / (m 3 cat h) More than 280kg EO / (m 3 cat h) or more than 300kg EO / (m 3 cat h) EO space-time yield. The measured EO space-time yield is preferably less than 500 kg EO / (m 3 cat h), the EO space-time yield is more preferably less than 350 kg EO / (m 3 cat h).
[0191] The preparation of ethylene oxide from ethylene and oxygen can advantageously be carried out in a recycling process. After each pass, newly formed ethylene oxide and by-products formed in the reaction are removed from the product gas stream. The remaining gas stream is supplemented with the required amount of ethylene, oxygen and reaction moderator and reintroduced into the reactor. Separation of ethylene oxide from the product gas stream and its aftertreatment can be carried out by conventional methods of the prior art (see Ullmann's Encyclopedia of Industrial Chemistry, 5th edition, volume A-10, pages 117-135, 123-125, VCH-Verlagsgesellschaft, Weinheim 1987).
[0192] The invention is described in more detail by means of the accompanying drawings and the following examples.
[0193] Figure 1 The log differential intrusion [mL / g] and the cumulative intrusion [mL / g] vs. the pore diameter [mL / g] of the porous α-alumina catalyst support A of the present invention obtained by the method according to the present invention are shown.
[0194] Figure 2 The logarithmic differential intrusion amount [mL / g] and the cumulative intrusion amount [mL / g] vs. the pore diameter [mL / g] of the porous α-alumina catalyst support B of the present invention obtained by the method according to the present invention are shown.
[0195] Figure 3 The logarithmic differential intrusion amount [mL / g] and cumulative intrusion amount [mL / g] of the comparative porous α-alumina catalyst support C are shown vs. the pore diameter [mL / g].
[0196] Figure 4The logarithmic differential intrusion amount [mL / g] and the cumulative intrusion amount [mL / g] vs. the pore diameter [mL / g] of the porous α-alumina catalyst support D of the present invention obtained by the method according to the present invention are shown.
[0197] Figure 5 The logarithmic differential intrusion amount [mL / g] and the cumulative intrusion amount [mL / g] vs. the pore diameter [mL / g] of the porous α-alumina catalyst support E of the present invention obtained by the method according to the present invention are shown.
[0198] Figure 6 The logarithmic differential intrusion amount [mL / g] and the cumulative intrusion amount [mL / g] of the comparative porous α-alumina catalyst support F are shown vs. the pore diameter [mL / g].
[0199] Figure 7 An image of the porous α-alumina catalyst support D of the present invention obtained by scanning electron microscopy is shown.
[0200] Figure 8 An image of a comparative porous alpha-alumina catalyst support F obtained by scanning electron microscopy is shown.
[0201] Fig. 9 The shapes of porous α-alumina catalyst supports S and T are shown.
[0202] Method 1: Nitrogen adsorption
[0203] Nitrogen adsorption measurements were performed using a Micrometrics ASAP 2420. Nitrogen porosity was determined according to DIN 66134. The samples were degassed under vacuum at 200 °C for 16 h before the measurements.
[0204] Method 2: Mercury porosimetry
[0205] Mercury porosimetry was performed using a Micrometrics AutoPore V 9600 mercury porosimeter (140 degree contact angle, 485 dynes / cm Hg surface tension, 61,000 psia maximum head pressure). Mercury porosity was determined according to DIN 66133.
[0206] The samples were dried at 110°C for 2 hours and degassed under vacuum before analysis to remove any physically adsorbed species, such as moisture, from the sample surface.
[0207] Method 3: Loose Bulk Density
[0208] The loose bulk density is determined by pouring the transition alumina or hydrated alumina into a graduated cylinder through a funnel, taking care not to move or vibrate the cylinder. The volume and weight of the transition alumina or hydrated alumina are determined. The loose bulk density is determined by dividing the volume in milliliters by the weight in grams.
[0209] Method 4: BET surface area
[0210] The BET surface area was determined according to DIN ISO 9277 using nitrogen physisorption at 77 K. The surface area was obtained from a 5-point BET plot. The samples were degassed under vacuum at 200° C. for 16 hours before the measurement. In the case of the shaped α-alumina support, more than 4 grams of sample were used due to its relatively low BET surface area.
[0211] Method 5: Scanning Electron Microscopy
[0212] Scanning electron microscopy using Hitachi SU3500 VP SEM (12 nm Pt coating) Method 6: Total analysis of Ca-, Mg-, Si-, Fe-, K- and Na-contents in α-alumina supports
[0213] 6A. Sample Preparation for Measurement of Ca, Mg, Si, and Fe
[0214] About 100 to 200 mg (±0.1 mg error tolerance) of the support sample is weighed into a platinum crucible. 1.0 gram of lithium metaborate (LiBO2) is added. The mixture is melted in an automated melting apparatus with a temperature ramp up to 1150°C.
[0215] After cooling, the melt was dissolved in deionized water by careful heating. Subsequently, 10 ml of semi-concentrated hydrochloric acid (concentrated HCl diluted with deionized water, volume ratio 1:1, equivalent to about 6 M) were added. Finally, the solution was filled to a volume of 100 ml with deionized water.
[0216] 6B. Measurement of Ca, Mg, Si and Fe
[0217] The amount of Ca, Mg, Si and Fe was determined from the solution described in item 5A by inductively coupled plasma-optical emission spectroscopy (ICP-OES) using an ICP-OES Varian Vista Pro. Parameters:
[0218] Wavelength [nm]: Ca 317.933
[0219] Mg 285.213
[0220] Si 251.611
[0221] Fe 238.204
[0222] Integration time: 10s
[0223] Atomizer: Conikal 3ml
[0224] Atomizer pressure: 270kPa
[0225] Pump speed: 30rpm
[0226] Calibration: External (matrix matched standard)
[0227] 6C. Sample preparation for K and Na measurements
[0228] About 100 to 200 mg (±0.1 mg error tolerance) of the carrier sample is weighed into a platinum dish. A mixture of 10 ml of concentrated H2SO4 aqueous solution (95 to 98%) and deionized water (volume ratio 1:4) and 10 ml of hydrofluoric acid aqueous solution (40%) are added. The platinum dish is placed on a sand bath and boiled to dryness. After cooling the platinum dish, the residue is dissolved in deionized water by careful heating. Subsequently, 5 ml of semi-concentrated hydrochloric acid (concentrated HCl diluted with deionized water, volume ratio 1:1, equivalent to about 6M) is added. Finally, the solution is filled to a volume of 50 ml with deionized water.
[0229] 6D. Measurement of K and Na
[0230] The amounts of K and Na were determined from the solution described in Item 5C by flame atomic absorption spectrometry (F-AAS) using F-AAS Shimadzu AA-7000.
[0231] parameter:
[0232] Wavelength [nm]: K 766.5 Na 589.0
[0233] Gas: Air / Acetylene
[0234] Slit width: 0.7nm(K) / 0.2nm(Na)
[0235] Atomizer pressure: 270kPa
[0236] Calibration: External (matrix matched standard)
[0237] Preparation of porous α-alumina catalyst carrier
[0238] The properties of the alumina raw materials used to obtain the porous α-alumina catalyst support are shown in Table 1. Transition alumina and hydrated alumina were obtained from Sasol ( and ) and UOP α-Alumina was prepared by heating Puralox TH 200 / 70 at 1200°C for 4 hours.
[0239] Table 1
[0240]
[0241]
[0242] *Measured by nitrogen adsorption
[0243] ** Determined by mercury porosimetry
[0244] ***Puralox products are transition aluminas, i.e. boehmite, derived from Pural products;
[0245] Versal VGL-15 is a gamma-alumina, pseudo-boehmite, derived from Versal V-250
[0246] Example 1 - Preparation of carriers A, B, C and G
[0247] The alumina raw materials as specified in Table 1 were mixed to obtain a powder mixture. VA64 (vinyl pyrrolidone-vinyl acetate copolymer from BASF) was added to the powder mixture. Water was then added to obtain a ductile precursor material. The amounts of all components are shown in Table 2.
[0248] The ductile precursor material was mixed to homogeneity by a mixer mill and then extruded using a plunger extruder to form a molded body. The molded body was in the form of a hollow cylinder having an outer diameter of about 10 mm and an inner diameter of about 5 mm. The extrudate was dried at 110° C. for about 16 hours and then heat treated at 600° C. for 2 hours at a ramp rate of 5° C. / min in a muffle furnace and then heat treated at 1,500° C. for 2 hours at a ramp rate of 2° C. / min. The heat treatment was performed in an air atmosphere.
[0249] Example 2 - Preparation of Vectors D, E, F, H, I, J and K.
[0250] Alumina raw materials as specified in Table 1 were mixed to obtain a powder mixture. Colloidal silica ( AS 40, Grace & Co.) and petrolatum ( Unilever) was added to the powder mixture. Water was then added to obtain a ductile precursor material. The amounts of all components are shown in Table 2.
[0251] The ductile precursor material was mixed to homogeneity by a mixer mill and then extruded using a plunger extruder to form a molded body. The molded body was in the form of a hollow cylinder having an outer diameter of about 10 mm and an inner diameter of about 5 mm. The extrudate was dried at 110° C. for about 16 hours and then heat treated at 600° C. for 2 hours at a ramp rate of 5° C. / min in a muffle furnace and then heat treated at 1,425° C. for 4 hours at a ramp rate of 2° C. / min. The heat treatment was performed in an air atmosphere.
[0252] Example 3 - Preparation of carriers L, M, N, O, P, Q and R
[0253] The alumina raw materials as specified in Table 1 were mixed to obtain a powder mixture. Dispersible boehmite ( HP 14 / 7, Sasol) and petrolatum ( Unilever) was added to the powder mixture. Water was then added to obtain a ductile precursor material. The amounts of all components are shown in Table 2.
[0254] The ductile precursor material was mixed to homogeneity by a mixer mill and then extruded using a plunger extruder to form a molded body. The molded body was in the form of a hollow cylinder having an outer diameter of about 10 mm and an inner diameter of about 5 mm. The extrudate was dried at 110° C. for about 16 hours and then heat treated at 600° C. for 2 hours at a ramp rate of 5° C. / min in a muffle furnace and then heat treated at 1,425° C. for 4 hours at a ramp rate of 2° C. / min. The heat treatment was performed in an air atmosphere.
[0255] Table 2
[0256]
[0257]
[0258]
[0259]
[0260] *Comparative ratio
[0261] Table 3 shows the physical properties of all supports prepared as shown in Table 2. Figures 1 to 6 The log differential intrusion and cumulative intrusion vs. pore diameter are shown for all supports prepared as shown in Table 2.
[0262] Table 3
[0263]
[0264]
[0265] *Comparative ratio
[0266] ** Determined by mercury porosimetry
[0267] ***r pv = ratio of the pore volume contained in pores with diameters greater than 1 to 10 μm to the pore volume contained in pores with diameters in the range of 0.1 to 1 μm
[0268] It is apparent that the carrier of the invention exhibits an advantageously high proportion of pores having a diameter in the range of 0.1 to 1 μm compared to the comparative carriers C, F and Q. The carrier of the invention also exhibits a lower r pv The surface area of the carrier of the present invention is significantly larger than that of the comparative carriers C, F and Q.
[0269] Compared to comparative supports G and R derived from alpha-alumina, the supports of the present invention exhibit significantly greater total pore volume and BET surface area.
[0270] At the same time, if Figure 7 (vector D of the present invention) and Figure 8 As is apparent from the comparison of (Comparative Support F), the support of the present invention exhibits a more open pore structure than the comparative support.
[0271] Example 4 - Preparation of Carriers S and T for Catalyst Performance Testing
[0272] The transition alumina and hydrated alumina as specified in Table 1 were mixed to obtain a powder mixture. The processing aid ( Unilever and glycerol, Sigma-Aldrich) and water were added to the powder mixture. MCC Spheres 200 (microcrystalline cellulose, JRS Pharma) was added to the mixture. Additional water was then added to obtain a ductile precursor material. The total amounts of all components are shown in Table 4.
[0273] Table 4
[0274]
[0275] *Comparative ratio
[0276] The ductile precursor material is mixed to homogeneity by a mixer and then extruded by a ram extruder to form a molded body. Fig. 9The extrudates were dried overnight at 110°C (approximately 16 hours) and then heat treated in a muffle furnace at 600°C for 2 hours at a ramp rate of 5°C / min, followed by heat treatment at elevated temperature (1475°C for support S and 1430°C for support T) for 4 hours at a ramp rate of 2°C / min. The heat treatment was carried out in an air atmosphere.
[0277] The dimensions of the dry carrier were determined using a caliper. The diameter of the circumscribed circle of the cross section perpendicular to the carrier height was 11.6 cm. The term "circumscribed circle" refers to the smallest circle within which the trilobal cross section is completely contained. The diameter of the inscribed circle of the cross section perpendicular to the carrier height is 5.3 cm. The term "inscribed circle" refers to the largest possible circle that can be drawn within the trilobal cross section. The central channel has a diameter of 1.92 cm. The three outer channels have a diameter of 1.46 cm.
[0278] The obtained supports S and T have an α-alumina content of more than 98% by weight and a Na-, K-, Mg-, Ca-content of less than 100 ppm. The Fe content in both supports is 200 ppm. The Si content in support S is 100 ppm. The Si content in support T is 200 ppm.
[0279] Table 5 shows the physical properties of the carrier S of the present invention and the comparative carrier T.
[0280] Table 5
[0281]
[0282] *Comparative ratio
[0283] ** Determined by mercury porosimetry
[0284] ***r pv = ratio of the pore volume contained in pores with diameters greater than 1 to 10 μm to the pore volume contained in pores with diameters in the range of 0.1 to 1 μm
[0285] Example 5 - Preparation of Catalyst
[0286] The shaped catalyst bodies were prepared by impregnating the supports S and T with the silver impregnation solution. The catalyst compositions are shown in Table 6 below. The silver content is given as a percentage relative to the total weight of the catalyst. The dopant values are given as parts per million relative to the total weight of the catalyst.
[0287] Table 6: Catalyst composition (Ag content is reported as weight percent of the total catalyst, dopant values are reported as parts per million by weight of the total catalyst)
[0288]
[0289]
[0290] *Comparative ratio
[0291] **Values for Ag and all accelerators are calculated;
[0292] ***K ADD is understood to refer to the amount of potassium added during the impregnation process and does not include the amount of potassium contained in the alumina support before impregnation.
[0293] 5.1 Production of Silver Complex Solution
[0294] The silver complex solution was prepared according to Production Example 1 of WO 2019 / 154863 A1. The silver complex solution had a density of 1.529 g / mL, a silver content of 29.3 wt %, and a potassium content of 90 ppm.
[0295] 5.2. Preparation of intermediate catalyst
[0296] 100.0 grams of carrier S (intermediate 1.1) and 100.4 grams of carrier T (intermediate 1.2) were each placed in a 2-liter glass flask. The flask was connected to a rotary evaporator, which was set at a vacuum pressure of 80 millibars. The rotary evaporator system was set to rotate at 30 rpm. Under a vacuum pressure of 80 millibars, 76.55 grams (intermediate 1.1) or 76.86 grams (intermediate 1.2) of the silver complex solution prepared according to step 2.1 were added to carrier S (intermediate 1.1) or carrier T (intermediate 1.2) over 15 minutes. After the silver complex solution was added, the rotary evaporator system continued to rotate under vacuum for another 15 minutes. The impregnated carrier was then left in the device for 1 hour at room temperature (approximately 25°C) and atmospheric pressure, gently mixing every 15 minutes.
[0297] The impregnated material was placed on the net to form 1 to 2 layers. The net was subjected to 23 Nm 3 / h air flow, wherein the air flow was preheated to a temperature of 305°C. The impregnated material was heated to a temperature of 290°C at a heating rate of about 30K / min and then kept at 290°C for 8 minutes to obtain an Ag-containing intermediate product according to Table 7. The temperature was measured by placing three thermocouples 1 mm below the mesh. Subsequently, the catalyst was cooled to ambient temperature by removing the intermediate catalyst body from the mesh using an industrial vacuum cleaner.
[0298] Table 7: Ag-containing intermediate catalysts (Ag content is reported as weight percent of the total catalyst, dopant values are reported as parts per million by weight of the total intermediate catalyst)
[0299] Intermediates Carrier <![CDATA[Ag CAT **[wt.-%]]]> <![CDATA[K ADD ***[ppm]]]> 1.1 S 18.3 56 1.2 T* 18.3 56
[0300] *Comparative ratio
[0301] **Values for Ag and all accelerators are calculated;
[0302] ***K ADD is understood to refer to the amount of potassium added during the impregnation process and does not include the amount of potassium contained in the alumina support before impregnation.
[0303] 5.3. Catalyst preparation
[0304] 120.5 grams of Ag-containing intermediate product 1.1 or 122.2 grams of Ag-containing intermediate product 1.2 prepared as in step 2.2 are placed in a 2-liter glass flask. The flask is connected to a rotary evaporator, which is set at a vacuum pressure of 80 mbar. The rotary evaporator system is set to rotate at 30 rpm. For catalyst 1, 53.80 grams of the silver complex solution prepared according to step 2.1 are mixed with 2.16 grams of promoter solution I, 2.80 grams of promoter solution II and 4.69 grams of promoter solution III. For catalyst 2, 54.56 grams of the silver complex solution prepared according to step 2.1 are mixed with 2.19 grams of promoter solution I, 2.84 grams of promoter solution II and 4.76 grams of promoter solution III.
[0305] Promoter solution I was obtained by dissolving lithium nitrate (Merck, 99.995%) and ammonium sulfate (Merck, 99.4%) in DI water to achieve a Li content of 2.85 wt.-% and an S content of 0.22 wt.-%. Promoter solution II was obtained by dissolving tungstic acid (HC Starck, 99.99%) in DI water and cesium hydroxide in water (HC Starck, 50.42%) to achieve a target Cs content of 5.0 wt.-% and a W content of 3.0 wt.-%. Promoter solution III was obtained by dissolving ammonium perrhenate (Buss & Buss Spezialmetalle GmbH, 99.9%) in DI water to achieve a Re content of 3.7 wt.-%.
[0306] The combined impregnation solution containing the silver complex solution and the promoter solutions I, II and III was stirred for 5 minutes. The combined impregnation solution was added to each silver-containing intermediate product 1.1 or 1.2 under a vacuum pressure of 80 mbar over 15 minutes. After the addition of the combined impregnation solution, the rotary evaporator system continued to rotate under vacuum for another 15 minutes. The impregnated support was then left in the apparatus at room temperature (approximately 25° C.) and atmospheric pressure for 1 hour, with gentle mixing every 15 minutes.
[0307] The impregnated material was placed on the net to form 1 to 2 layers. The net was subjected to 23 Nm 3 / h nitrogen flow (oxygen content: <20 ppm), wherein the gas flow was preheated to a temperature of 305° C. The impregnated material was heated to a temperature of 290° C. at a heating rate of approximately 30 K / min and then kept at 290° C. for 7 minutes to obtain the catalyst according to Table 4. The temperature was measured by placing three thermocouples 1 mm below the mesh. Subsequently, the catalyst was cooled to ambient temperature by removing the catalyst body from the mesh using an industrial vacuum cleaner.
[0308] Example 6 - Catalyst Testing
[0309] The epoxidation reaction was carried out in a vertically placed test reactor made of stainless steel with an inner diameter of 6 mm and a length of 2.2 m. The reactor was heated at a specified temperature using hot oil contained in a heating jacket. All temperatures below refer to the temperature of the hot oil. 9 grams of inert steatite balls (0.8 to 1.1 mm) were filled into the reactor, 26.4 grams of crushed catalyst sieved to a desired particle size of 1.0 to 1.6 mm were filled thereon, and another 29 grams of inert steatite balls (0.8-1.1 mm) were filled thereon. The inlet gas was introduced into the top of the reactor in a "once-through" operating mode.
[0310] The catalyst was loaded into the reactor at a reactor temperature of 90°C at a nitrogen flow rate of 130NL / h at 1.5 bar absolute pressure. The reactor temperature was then ramped up to 210°C at a heating rate of 50K / h, and the catalyst was maintained under this condition for 15 hours. The nitrogen flow was then replaced with 114NL / h methane and 1.5NL / h CO2. The reactor was pressurized to 16 bar absolute pressure. A mixture of 30.4NL / h ethylene and 0.8NL / h of 500ppm ethylene dichloride in methane was then added. Oxygen was then introduced in a stepwise manner to reach a final flow of 6.1NL / h. At this point, the inlet composition consisted of 20% by volume ethylene, 4% by volume oxygen, 1% by volume carbon dioxide, and 2.5 parts per million by volume (ppmv) ethylene dichloride (EC) moderator, with methane used as the balance at a total gas flow rate of 152.8NL / h. The reactor temperature was ramped up to 225°C at a heating rate of 5 K / h and thereafter ramped up to 240°C at a heating rate of 2.5 K / h. The catalyst was kept under these conditions for 135 hours. Thereafter, the EC concentration was reduced to 2.2 ppmv and the temperature was reduced to 225°C. The inlet gas composition was then gradually changed to 35 vol% ethylene, 7 vol% oxygen, 1 vol% carbon dioxide, using methane as the balance and a total gas flow of 147.9 NL / h. The temperature was adjusted to achieve an ethylene oxide (EO) concentration of 3.05% in the outlet gas. The EC concentration was adjusted to optimize the selectivity. The results of the catalyst tests are summarized in Table 8.
[0311] Table 8: Summary of catalyst testing
[0312]
[0313] *Comparative ratio
[0314] **Run time starts when oxygen is introduced into the ethylene-containing feed
[0315] It is clear that catalyst 1 obtained from support S according to the invention exhibits a much higher selectivity than catalyst 2 obtained from comparative support T.
Claims
1. A method for producing a porous α-alumina catalyst carrier, comprising i) preparing a precursor material comprising, based on inorganic solid content, - at least 50 wt.% of a transition alumina having a loose bulk density of at most 600 g / L, a pore volume of at least 0.6 mL / g and a median pore diameter of at least 15 nm; and - up to 30% by weight of hydrated aluminum oxide; ii) shaping the precursor material into a shaped body; and iii) calcining the shaped body to obtain a porous α-alumina catalyst support.
2. The method according to claim 1, wherein the transition alumina has a loose bulk density of 50 to 600 g / L and a pore volume of 0.6 to 2.0 mL / g.
3. The method according to claim 1, wherein the precursor material comprises 1 to 30 wt% hydrated aluminum oxide.
4. The method according to claim 2, wherein the precursor material comprises 1 to 30 wt% hydrated aluminum oxide.
5. The method according to any one of claims 1 to 4, wherein the transition alumina comprises a phase selected from the group consisting of gamma-alumina, delta-alumina and theta-alumina.
6. The method according to claim 5, wherein the transition alumina comprises a phase selected from the group consisting of gamma-alumina and delta-alumina.
7. The method according to claim 5, wherein the transition alumina comprises at least 50 wt% of transition alumina having an average particle size of 10 to 100 μm, based on the total weight of the transition alumina.
8. The method according to claim 5, wherein the transition alumina comprises at least 50 wt% of transition alumina having an average particle size of 20 to 50 μm, based on the total weight of the transition alumina.
9. The method according to claim 7, wherein the hydrated alumina comprises boehmite and / or pseudo-boehmite.
10. The method according to claim 9, wherein the precursor material further comprises a liquid.
11. The method according to claim 9, wherein the precursor material further comprises water.
12. The method according to claim 10, wherein the precursor material further comprises a pore-forming material, a lubricant, an organic binder and / or an inorganic binder.
13. The method according to claim 12, wherein the precursor material is formed into a shaped body by extrusion, tableting, pelletizing, casting, molding or microextrusion.
14. The method according to claim 12, wherein the precursor material is formed into a shaped body by extrusion or tableting.
15. The method according to claim 13, wherein the calcining is carried out at a temperature of at least 1300°C.
16. The method according to claim 15, wherein the calcination is carried out at a temperature of at least 1400°C.
17. The method according to claim 15, wherein the calcining is carried out at a temperature of at least 1450°C.
18. A shaped catalyst body for the production of ethylene oxide by gas phase oxidation of ethylene, comprising at least 15% by weight of silver, relative to the total weight of the catalyst, deposited on a porous alpha-alumina catalyst support obtained in a process according to any one of claims 1 to 17.
19. The shaped catalyst body according to claim 18, comprising from 15 to 70% by weight of silver, relative to the total weight of the shaped catalyst body.
20. The shaped catalyst body according to claim 18, comprising 20 to 60% by weight of silver, relative to the total weight of the shaped catalyst body.
21. The shaped catalyst body according to claim 18, comprising 25 to 50% by weight of silver, relative to the total weight of the shaped catalyst body.
22. The shaped catalyst body according to claim 18, comprising 30 to 50% by weight of silver, relative to the total weight of the shaped catalyst body.
23. A method for preparing a shaped catalyst body according to any one of claims 18 to 22, comprising a) impregnating a porous α-alumina catalyst support obtained in a process according to any one of claims 1 to 17 with a silver impregnation solution; and optionally subjecting the impregnated porous alumina support to drying; and b) subjecting the impregnated porous α-alumina support to a heat treatment; wherein steps a) and b) are optionally repeated.
24. The method of claim 23, wherein the porous alpha-alumina catalyst support is impregnated with the silver impregnation solution under reduced pressure.
25. A process for producing ethylene oxide by gas phase oxidation of ethylene, which comprises reacting ethylene and oxygen in the presence of a shaped catalyst body according to any one of claims 18 to 22.
Citation Information
Patent Citations
DE117135A
silver catalysts, processes for their preparation and their use
DE2300512A1
Silver olefin oxidation catalysts - supported on specified carriers and promoted esp. with barium
DE2454972A1
silver catalyst and its use
DE2521906A1
Process and reactor for carrying out exothermic catalytic reactions
DE3414717A1