Preparation method and application of supported Rh / TiO2-P catalyst
Through the preparation method of supported Rh/TiO2-P catalyst, the problem of homogeneous catalyst separation and immobilization is solved, the uniform dispersion of Rh and the sub-nanostructure of the catalyst are achieved, and the catalytic activity of 1-octene carbonylation reaction is improved and Selective.
Patent Information
- Application Number
- CN202211620390.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-12-15
AI Technical Summary
Homogeneous catalysts are difficult to separate and immobilize in industrial applications, resulting in poor loss and selectivity of precious metals Rh, and existing heterogeneous catalysts have problems with inactivation of expensive metals.
Using the preparation method of a supported Rh/TiO2-P catalyst, an impregnation liquid is formed by ultrasonic dispersing the Rh precursor and the TiO2 support, and ultrasonic impregnation and drying of the phosphorus source in an inert atmosphere to obtain a heterogeneous catalyst with a sub-nanostructure.
The uniform dispersion of Rh and the atomic dispersion of active metals are achieved, and the conversion activity and selectivity of the catalyst are improved, especially in the 1-octene carbonylation reaction, which shows excellent catalytic properties.
Smart Images

Figure CN115999539B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst synthesis, and in particular relates to a preparation method and application of a supported Rh / TiO2-P catalyst. Background Art
[0002] The hydroformylation of olefins refers to the process in which olefins and synthesis gas react under the catalysis of transition metal complexes to generate aldehydes with one more carbon atom than the raw olefins. The rapid development of petrochemicals in recent decades has provided cheap raw materials for the hydroformylation of olefins, making it have the material basis required for industrialization; with the gradual improvement of people's living standards, people's demand for material life has gradually increased, which has greatly promoted the rapid development of industries such as plastics, coatings, rubber, and detergents, thereby providing huge market conditions for the development of olefin hydroformylation. 1-Octene is mainly used as an intermediate for polyethylene comonomers, plasticizers, etc. It is particularly important to develop catalysts and processes for the highly selective synthesis of 1-octene by ethylene polymerization.
[0003] At present, in the context of the application of homogeneous catalysts, there are many urgent industrial problems to be solved. Since homogeneous catalysts are difficult to separate in the organic phase, a large amount of heat energy and equipment costs are required for industrial application. Therefore, in recent years, many researchers have begun to pay more attention to heterogeneous catalysts and homogeneous catalyst immobilization. Although such catalysts can easily achieve catalyst separation and recycling, they also face problems such as the loss, deactivation and poor selectivity of the expensive precious metal Rh. In order to solve such problems, in the direction of heterogeneous catalysts, a large amount of research has been invested in the research fields of homogeneous multiphase polymer catalysts, bimetallic catalysts and single atom catalysts or atomically dispersed catalysts. Atomic-level dispersed catalysts serve as a bridge between homogeneous and heterogeneous catalysts. While meeting the maximum atomic exposure rate, due to the reduction of the catalyst size to the atomic level, the catalyst energy level structure and electronic structure will undergo fundamental changes, such as a sharp increase in surface free energy, quantum size effect, unsaturated coordination environment and metal-support interaction, thereby showing excellent catalytic conversion activity. Summary of the invention
[0004] The first technical problem to be solved by the present invention is to provide a method for preparing a supported Rh / TiO2-P catalyst. The heterogeneous TiO2-supported phosphorus-functionalized Rh catalyst prepared by the preparation method has uniform metal dispersion and a sub-nanometer structure.
[0005] The second technical problem to be solved by the present invention is to provide the application of the above-mentioned supported Rh / TiO2-P catalyst.
[0006] In order to solve the above-mentioned first technical problem, the present invention adopts the following technical solution:
[0007] A method for preparing a supported Rh / TiO2-P catalyst comprises the following steps:
[0008] 1) dissolving the carrier raw material in an appropriate amount of ethanol, ultrasonically dispersing and stirring to form a carrier raw material suspension;
[0009] 2) dissolving the Rh precursor in an appropriate amount of ethanol, dispersing by ultrasonication and stirring evenly to form an active metal precursor solution;
[0010] 3) adding the active metal precursor solution to the carrier raw material suspension, stirring thoroughly and evenly, and then impregnating under uniform stirring to form an impregnation solution;
[0011] 4) separating the impregnation liquid, vacuum drying it, and grinding it into powder;
[0012] 5) calcining the ground powder and then cooling it to room temperature to obtain a catalyst carrier;
[0013] 6) dissolving the phosphorus source in an appropriate amount of toluene and dispersing by ultrasonication to form a toluene solution of the phosphorus source;
[0014] 7) Add the toluene solution of the phosphorus source into the reactor containing the catalyst carrier obtained in step 5), perform equal volume ultrasonic impregnation in an inert atmosphere, separate and dry to obtain the supported Rh / TiO2-P catalyst.
[0015] As an embodiment, in step 1), the carrier raw material is TiO2.
[0016] As an embodiment, in step 2), the Rh precursor is one or more of RhCl3·3H2O, Rh(NO3)3, Rh2(SO4)3, Rh2(CH3COO)4·2H2O; preferably, the Rh precursor is RhCl3·3H2O.
[0017] As an embodiment, in step 3), the stirring speed is 400-1000 r / min, and the immersion time is 2-48 h.
[0018] As an embodiment, in step 4), the separation method is evaporation separation; the evaporation separation conditions are: stirring at a temperature of 50-200°C to evaporate the solution until it becomes a viscous paste; preferably, the evaporation separation temperature is 80°C.
[0019] As an embodiment, in step 5), purging is performed before calcination.
[0020] As an embodiment, in step 5), the calcination treatment is carried out in two steps: in the first calcination treatment, the calcination atmosphere is air, the calcination temperature is 100-700°C, and the calcination time is 2-9h; in the second calcination treatment, the calcination atmosphere is H2 / Ar, the calcination temperature is 200-800°C, and the calcination time is 2-9h;
[0021] As a preferred embodiment, the calcination temperature of the first calcination treatment is 100-500°C, and the calcination time is 2-5h; the calcination temperature of the second calcination treatment is 200-500°C, and the calcination time is 2-5h.
[0022] As an embodiment, in step 6), the phosphorus source is triphenylphosphine or triphenylphosphine oxide; preferably, the phosphorus source is triphenylphosphine; and the concentration of the toluene solution of the phosphorus source is 0.05-1.0 g / ml.
[0023] As an embodiment, in step 7), the separation condition is to remove the organic solvent by vacuuming.
[0024] To solve the above second technical problem, the present invention adopts the following technical solution:
[0025] The present invention also provides an application of the supported Rh / TiO2-P catalyst obtained by the preparation method in the carbonylation of 1-octene.
[0026] Any range described in the present invention includes the end value and any numerical value between the end values and any sub-range formed by the end value or any numerical value between the end values.
[0027] Unless otherwise specified, all raw materials in the present invention can be purchased from the market, and the equipment used in the present invention can adopt conventional equipment in the relevant field or refer to the existing technology in the relevant field.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The invention obtains a supported Rh / TiO2-P catalyst, wherein the active metal Rh is evenly dispersed, has a sub-nano structure, and forms a coordination effect with a phosphorus source. Moreover, the catalyst exhibits excellent catalytic activity in the carbonylation reaction of 1-octene. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] The specific embodiments of the present invention will be further described in detail below with reference to the accompanying drawings.
[0031] Figure 1 is the X-ray diffraction (XRD) diagram of Example 1 of the present invention;
[0032] Figure 2The transmission electron microscope TEM and element mapping diagram of Example 1 of the present invention;
[0033] Figure 3 It is a schematic diagram of the catalytic activity (conversion rate and selectivity) of Example 1, Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention for the carbonylation of 1-octene. DETAILED DESCRIPTION
[0034] In order to explain the present invention more clearly, the present invention is further described below in conjunction with preferred embodiments. It should be understood by those skilled in the art that the following specific description is illustrative rather than restrictive, and should not be used to limit the scope of protection of the present invention.
[0035] As one aspect of the present invention, a method for preparing a supported Rh / TiO2-P catalyst comprises the following steps:
[0036] 1) dissolving the carrier raw material in an appropriate amount of ethanol, ultrasonically dispersing and stirring to form a carrier raw material suspension;
[0037] 2) dissolving the Rh precursor in an appropriate amount of ethanol, dispersing by ultrasonication and stirring evenly to form an active metal precursor solution;
[0038] 3) adding the active metal precursor solution to the carrier raw material suspension, stirring thoroughly and evenly, and then impregnating under uniform stirring to form an impregnation solution;
[0039] 4) separating the impregnation liquid, vacuum drying it, and grinding it into powder;
[0040] 5) calcining the ground powder and then cooling it to room temperature to obtain a catalyst carrier;
[0041] 6) dissolving the phosphorus source in an appropriate amount of toluene and dispersing by ultrasonication to form a toluene solution of the phosphorus source;
[0042] 7) Add the toluene solution of the phosphorus source into the reactor containing the catalyst carrier obtained in step 5), perform equal volume ultrasonic impregnation in an inert atmosphere, separate and dry to obtain the supported Rh / TiO2-P catalyst.
[0043] According to some embodiments of the present invention, in step 1), the carrier raw material is TiO2.
[0044] According to certain embodiments of the present invention, in step 2), the Rh precursor is one or more of RhCl3·3H2O, Rh(NO3)3, Rh2(SO4)3, and Rh2(CH3COO)4·2H2O; preferably, the Rh precursor is RhCl3·3H2O.
[0045] According to some embodiments of the present invention, in step 3), the stirring speed is 400-1000 r / min, and the immersion time is 2-48 h.
[0046] According to certain embodiments of the present invention, in step 4), the separation method is evaporation to dryness; the evaporation to dryness separation conditions are: stirring at a temperature of 50-200°C to evaporate the solution until it becomes a viscous paste; preferably, the evaporation to dryness separation temperature is 80°C.
[0047] According to some embodiments of the present invention, in step 5), purging is performed before the calcination process.
[0048] According to some embodiments of the present invention, in step 5), the calcination treatment is carried out in two steps: in the first step of the calcination treatment, the calcination atmosphere is air, the calcination temperature is 100-700°C, and the calcination time is 2-9h; in the second step of the calcination treatment, the calcination atmosphere is H2 / Ar, the calcination temperature is 200-800°C, and the calcination time is 2-9h;
[0049] According to some preferred embodiments of the present invention, the calcination temperature of the first calcination treatment is 100-500°C, and the calcination time is 2-5h; the calcination temperature of the second calcination treatment is 200-500°C, and the calcination time is 2-5h.
[0050] According to some embodiments of the present invention, in step 6), the phosphorus source is triphenylphosphine or triphenylphosphine oxide; preferably, the phosphorus source is triphenylphosphine; and the concentration of the toluene solution of the phosphorus source is 0.05-1.0 g / ml.
[0051] According to certain embodiments of the present invention, in step 7), the separation condition is to remove the organic solvent by vacuuming.
[0052] As another aspect of the present invention, the present invention also provides an application of the supported Rh / TiO2-P catalyst obtained by the above preparation method in the carbonylation of 1-octene.
[0053] Example 1
[0054] A method for preparing a supported Rh / TiO2-P catalyst comprises the following steps:
[0055] 1) Dissolve 0.5g TiO2 in an appropriate amount of ethanol, thoroughly sonicate and stir to form a carrier suspension;
[0056] 2) Dissolve 2.076 mg of RhCl3·3H2O in an appropriate amount of ethanol, disperse by ultrasonication, and stir well to form an active metal precursor solution;
[0057] 3) Add the active metal precursor solution to the carrier suspension, stir well to form an impregnation solution, and perform impregnation at a rate of 400-1000 r / min for 12 hours;
[0058] 4) heating the impregnation solution to 80°C and stirring to evaporate the solution until it becomes a viscous paste, vacuum drying it, and grinding it into powder;
[0059] 5) The ground powder was calcined and purged before calcination for 90 minutes. The first step of calcination was carried out in an air atmosphere at 150° C. for 3 hours. The second step of calcination was carried out in a H2 / Ar atmosphere at 300° C. for 3 hours and then cooled to room temperature to obtain a catalyst carrier.
[0060] 6) Dissolve 0.1 g of triphenylphosphine (PPh3) in an appropriate amount of toluene and disperse by ultrasonication to form a PPh3 toluene solution;
[0061] 7) Add the PPh3 toluene solution into the Schlenk bottle containing the catalyst support prepared in step 5), perform equal volume ultrasonic immersion for 30 min in an inert atmosphere, remove the organic solvent by vacuum evacuation and vacuum dry at 60°C for 12 h to obtain the supported Rh / TiO2-P catalyst.
[0062] Material Characterization and Testing:
[0063] Figure 1 The X-ray diffraction (XRD) pattern of the supported Rh / TiO2-P catalyst obtained in Example 1 of the present invention;
[0064] like Figure 1 As shown, there is only the diffraction peak of the carrier TiO2, but no diffraction peak of the metal Rh, which indicates that the Rh supported by this catalyst should be dispersed at the atomic level;
[0065] Figure 2 The transmission electron microscope TEM and element mapping diagram of the supported Rh / TiO2-P catalyst obtained in Example 1 of the present invention are shown in FIG. Figure 2 As shown, only the carrier TiO2 can be seen, and there are no obvious metal particles, which further verifies that the supported Rh / TiO2-P catalyst is dispersed at the atomic level;
[0066] Example 2
[0067] Example 1 was repeated, except that the amount of triphenylphosphine (PPh3) in step 6) was 0.2 g.
[0068] Example 3
[0069] Repeat Example 1 The only difference is that the heating rate of calcination in step 5) is 10°C / min.
[0070] Comparative Example 1
[0071] Example 1 was repeated except that step 6) was omitted and triphenylphosphine (PPh3) was not added.
[0072] Comparative Example 2
[0073] Example 1 was repeated, except that the order of step 4) and step 5) was switched, i.e., PPh3 was impregnated first and then calcined.
[0074] Comparative Example 3
[0075] Example 1 was repeated, except that the carrier in step 1) was CeO2.
[0076] Application Experiment Example
[0077] An application of the supported Rh / TiO2-P catalyst obtained by the above preparation method in the carbonylation of 1-octene comprises the following steps and conditions:
[0078] 1) Cleaning the high pressure reactor;
[0079] 2) Adding appropriate amounts of toluene solvent and 1-octene into the reactor, and adding appropriate amounts of catalyst;
[0080] 3) Repeatedly introduce synthesis gas to fully purge the reactor and drive away the air in the reactor. After the purge is completed, introduce 2-6MPa synthesis gas and heat it to 80-140℃ for 2-7h.
[0081] 4) After the reaction is completed, the temperature is lowered to room temperature, the pressure is lowered to normal pressure, and a certain amount of the reaction solution is passed into a gas chromatograph to analyze the product to obtain performance data.
[0082] Material Characterization and Testing: Figure 3 It is a schematic diagram of the catalytic activity (conversion rate and selectivity) of the catalysts obtained in Example 1, Example 2, Comparative Example 1, Comparative Example 2 and Comparative Example 3 of the present invention for the carbonylation of 1-octene.
[0083] Depend on Figure 3 It can be seen that all the examples of the present invention have high olefin conversion and aldehyde selectivity, and more importantly, the ratio of normal aldehyde to isomeric aldehyde is higher. However, the olefin conversion, aldehyde selectivity and the ratio of normal aldehyde to isomeric aldehyde of the comparative examples all show a decrease to varying degrees, which indicates that the impregnation of the phosphorus source, the order of the calcination steps, the properties of the carrier, etc. all have a certain influence on the performance of the catalyst in catalyzing the carbonylation of 1-octene.
[0084] In summary, in the preparation method of a supported Rh / TiO2-P catalyst of the present invention, the Rh precursor, impregnation method, calcination conditions, etc. have an important influence on the preparation of the product. They need to be organically coordinated and cooperate with each other to form a complete technical solution in order to obtain the supported Rh / TiO2-P catalyst required by the present invention.
[0085] Obviously, the above embodiments of the present invention are merely examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is impossible to list all implementation methods here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.
Claims
1. A method for preparing a supported Rh / TiO2-P catalyst, characterized in that: The steps include: 1) dissolving the carrier raw material in an appropriate amount of ethanol, ultrasonically dispersing and stirring to form a carrier raw material suspension; 2) dissolving the Rh precursor in an appropriate amount of ethanol, dispersing by ultrasonication and stirring evenly to form an active metal precursor solution; 3) adding the active metal precursor solution to the carrier raw material suspension, stirring thoroughly and evenly, and then impregnating under uniform stirring to form an impregnation solution; 4) separating the impregnation liquid, vacuum drying it, and grinding it into powder; 5) calcining the ground powder and then cooling it to room temperature to obtain a catalyst carrier; 6) dissolving the phosphorus source in an appropriate amount of toluene and dispersing by ultrasonication to form a toluene solution of the phosphorus source; 7) adding the toluene solution of the phosphorus source into the reactor containing the catalyst support obtained in step 5), performing equal volume ultrasonic impregnation in an inert atmosphere, separating and drying to obtain a supported Rh / TiO2-P catalyst; In step 1), the carrier raw material is TiO2; In step 2), the Rh precursor is one or more of RhCl3·3H2O, Rh(NO3)3, Rh2(SO4)3, and Rh2(CH3COO)4·2H2O; In step 3), the stirring speed is 400-1000 r / min, and the immersion time is 2-48 h; In step 4), the separation method is evaporation to dryness; the evaporation to dryness separation conditions are: stirring at a temperature of 50-200° C. to evaporate the solution until it becomes a viscous paste; In step 5), the calcination treatment is carried out in two steps: in the first calcination treatment, the calcination atmosphere is air, the calcination temperature is 100-700°C, and the calcination time is 2-9h; in the second calcination treatment, the calcination atmosphere is H2 / Ar, the calcination temperature is 200-800°C, and the calcination time is 2-9h.
2. The method for preparing the supported Rh / TiO2-P catalyst according to claim 1, characterized in that: In step 5), purging is performed before the calcination treatment.
3. The method for preparing the supported Rh / TiO2-P catalyst according to claim 1, characterized in that: The calcination temperature of the first calcination treatment is 100-500°C, and the calcination time is 2-5h; the calcination temperature of the second calcination treatment is 200-500°C, and the calcination time is 2-5h.
4. The method for preparing the supported Rh / TiO2-P catalyst according to claim 1, characterized in that: In step 6), the phosphorus source is triphenylphosphine or triphenylphosphine oxide; the concentration of the toluene solution of the phosphorus source is 0.05-1.0 g / ml.
5. The method for preparing the supported Rh / TiO2-P catalyst according to claim 1, characterized in that: In step 7), the separation condition is to remove the organic solvent by vacuuming.
6. Use of a supported Rh / TiO2-P catalyst obtained by any preparation method according to claim 1 to 5 in the carbonylation of 1-octene.