A Ni-Mo / SiO2 catalyst for catalyzing the hydrodeoxygenation of bio-oil to produce hydrocarbon fuel

By adding the oxygen-philic additive M to the Ni-Mo/SiO2 catalyst to control the Ni site, the problems of high temperature and low carbon content of the product in the bio-oil hydrodeoxygenation reaction in the existing technology are solved, and high-efficiency catalytic biomass is achieved. Hydrodeoxygenation of oils and fats produces high-carbon hydrocarbon fuels and improves the activity and stability of the catalyst.

CN115999564BActive Publication Date: 2024-10-18XIANGTAN UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211539566.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-02
Publication Date
2024-10-18
Estimated Expiration
2042-12-02

AI Technical Summary

Technical Problem

When existing catalysts catalyze the hydrodeoxygenation reaction of bio-oils, the temperature is high, isoparaffins and light alkanes are present in the product, and the electron-rich sites of the Ni catalyst interact strongly with the C=O bond of the fatty acid methyl ester, which promotes the The generation of low-carbon fuels makes it difficult to prepare high-carbon hydrocarbon fuels.

Method used

By adding the oxygen-philic additive M to the Ni-Mo/SiO2 catalyst, the electron density and surrounding environment of the Ni site are controlled, the interaction between the electron-rich Ni and the C=O bond is weakened, the HDO reaction pathway is promoted, and high carbon content is prepared Hydrocarbon fuels.

Benefits of technology

Efficient catalytic hydrodeoxygenation of bio-oils is achieved to generate high-carbon hydrocarbon fuels. The catalyst has good activity and stability, high product selectivity, low cost and easy separation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure GDA0004095771990000011
    Figure GDA0004095771990000011
  • Figure GDA0004095771990000021
    Figure GDA0004095771990000021
  • Figure GDA0004095771990000022
    Figure GDA0004095771990000022
Patent Text Reader

Abstract

The present invention discloses a Ni-Mo / SiO2 catalyst for catalyzing the hydrodeoxygenation of bio-oil to prepare hydrocarbon fuel, which has low cost, high catalytic activity and n-C N 、n‑C N‑1 The alkane product is selective and easy to separate from the reaction system. When the mass ratio of Ni-Mo / SiO2 to bio-oil is 0.2:1, the hydrogen pressure is 3MPa, the reaction temperature is 300℃, and the reaction time is 4h, the conversion rate of methyl decanoate reaction is 98.7%, and n-C 10 , n-C9 alkane selectivity 81.4%, 17.3%; methyl laurate reaction conversion rate 97.9%, n-C 12 、n‑C 11 Alkane selectivity 79.7%, 18.2%; methyl myristic acid ester reaction conversion rate 98.5%, n-C 14 、n‑C 13 Selectivity 81.7%, 16.8%; methyl palmitate reaction conversion rate 99.1%, n-C 16 、n‑C 15 Selectivity 83.4%, 15.7%; methyl stearate reaction conversion rate 98.3%, n-C 18 、n‑C 17 Selectivity 82.5%, 15.8%; Jatropha curcas oil reaction conversion rate and n-C 13‑18 The molar yields were 93.5% and 89.6%; the conversion rate of waste cooking oil hydrodeoxygenation reaction and n-C 13‑18 The molar yields of alkanes were 86.8% and 78.5%, respectively.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of biomass energy catalysis and relates to a Ni-Mo / SiO2 catalyst for catalyzing the hydrodeoxygenation of bio-oil to prepare hydrocarbon fuel. 2 catalyst. Background Art

[0002] The catalytic hydrodeoxygenation reaction of bio-oil (taking fatty acid methyl ester as an example) is as follows: 1 For methyl:

[0003]

[0004] In a hydrogen atmosphere, the ester groups in the oil molecules are first hydrogenated to obtain fatty acids, and then converted into nC N or nC N-1 Alkanes (n-C N Alkanes or n-C N-1 In addition, due to the high temperature of catalytic oil hydrodeoxygenation reaction (>240℃), there are a certain amount of isoalkanes and light alkanes in the product. Among them, the hydrodeoxygenation HDO reaction pathway is the continuous hydrogenation of carboxyl groups to C-OH, and then CO hydrocracking deoxygenation to convert nC N Alkane hydrocarbon fuel and water, or dehydration to produce α-β and β-γ unsaturated olefins, and further hydrogenation to produce nC N Alkane hydrocarbon fuel. The decarbonylation DCN reaction pathway and the decarboxylation DCX reaction pathway are both to remove -COOH in fatty acids and to remove fatty acid hydrogenation intermediate fatty aldehyde -CHO to generate nC N-1 Alkane hydrocarbon fuel with by-product CO 2 and CO. The DCN and DCX reaction pathways above generate nC N-1 Alkanes are more likely to be generated by the HDO reaction pathway than by the N Alkanes have one less carbon, thus reducing the carbon content of the product hydrocarbon fuel.

[0005] When a single metal sulfur-free Ni-based catalyst is used for catalysis, the electron-rich Ni sites in the catalyst preferentially bind to the C δ+ =O δ -C δ+ Combine to form carboxylate or 1 (C)-acyl adsorption causes the CC bond adjacent to the C=O double bond in the bio-oil to be stretched and activated, thereby promoting the DCN / DCX reaction pathway. 2(C,O)-aldehyde adsorption is more stable and easier to activate the C=O bond, which is then dissociated by the metal active center to produce active H * , and then attack the fatty alcohol (R-CH 2 OH) intermediate, and then undergoes dehydration, hydrogenation or hydrogenolysis to form a hydrocarbon fuel with a high carbon content.

[0006]

[0007] The present invention utilizes the close correlation between the electron density on the Ni atom d orbital and the surrounding environment of the Ni atom and several adsorption configurations, and finely regulates the electron density of the Ni site and the microenvironment around the Ni site by adding an oxophilic additive M, thereby weakening the electron-rich Ni δ -With C δ+ The strong interaction between them and the simultaneous stretching of the C=O bond activates the C=O bond, thereby realizing the catalytic hydrodeoxygenation of bio-oils to prepare high-carbon hydrocarbon fuels through the HDO reaction pathway catalyzed by sulfur-free Ni-based catalysts. Summary of the invention

[0008] The present invention aims to provide a Ni-Mo / SiO catalyst for catalyzing the hydrodeoxygenation of bio-oil to prepare hydrocarbon fuels through the HDO reaction pathway. 2 catalyst.

[0009] Technical solution of the present invention

[0010] A Ni-Mo / SiO2 catalyst for hydrodeoxygenation of bio-oil to produce hydrocarbon fuels 2 A catalyst characterized by:

[0011] (1) The bio-oil is any one of methyl caprate, methyl laurate, methyl myristic acid, methyl palmitate, and methyl stearate, and the bio-oil is also derived from natural oil Jatropha curcas oil or waste cooking oil from restaurants, and the Ni-Mo / SiO 2 The catalyst is composed of Ni, Mo and SiO 2 Support composition, Ni, Mo and SiO 2 The carrier molar ratio is 0.1:0.03:1.

[0012] Table 1 Ni-M / SiO 2 Catalyst pore structure and composition data

[0013]

[0014] In Table 1: a Specific surface area, b Pore ​​volume, c Hole diameter, d ICP-OES method was used to determine EThe Ni particle diameter was calculated based on the half-peak width of XRD using the Debye-Scherrer formula. f HRTEM characterization shows the Ni particle diameter. g The dispersion of nano-Ni particles (dispersion refers to the ratio of the number of active metal atoms on the catalyst surface to the total number of metal atoms in the catalyst, which is measured by H 2 Pulse chemisorption measurement calculated), h 50℃~300℃H 2 -The Ni-H number on the catalyst surface determined by the TPD curve represents the adsorption and dissociation of H at the metal active site. 2 Produces active H(H * ) attack oxygen-containing functional groups (C=O, CO, C Ar -O(C Ar - represents benzene ring), i.e., the activity of catalyzing the hydrodeoxygenation of bio-oil.

[0015] Table 1 Ni-M / SiO 2 Catalyst acidity distribution (mmol·g -1 )

[0016]

[0017] The weak acid (<300℃), medium acid (300℃~500℃), and strong acid (>500℃) in Table 2 are based on NH 3 -determined by TPD curve;

[0018] Ni-Mo / SiO 2 The catalyst is a mesoporous particle structure with a rough surface, a pore size of 5.48 nm, a particle size of 100-200 nm, and a pore volume of 0.33 cm 3 / g, specific surface area 185m 2 Table 1 and Table 2 respectively list several Ni-M / SiO modified by oxygen-affinity additive M. 2 The comparison of the pore structure, component data, acid distribution and its strength of the catalyst shows that Ni-Mo / SiO 2 The pore structure and component data of the catalyst are relatively good: the particle size of the nano-Ni particles is 3.84-4.9nm, the dispersion of the nano-Ni particles is 2.35%, and the chemical adsorption of Ni-H is 78.3mol / g. Therefore, Ni-Mo / SiO 2 The catalytic activity is good, and its acid distribution and acid strength are moderate.

[0019] (2) In Ni-Mo / SiO 2The mass ratio of catalyst to raw material bio-oil was 0.2:1, the hydrogen pressure was 3MPa, the reaction temperature was 300℃, and the high pressure closed reaction was carried out for 4h. After cooling and centrifugation to separate the catalyst, the product hydrocarbon fuel was obtained. The results are shown in Table 3:

[0020] Table 3 Ni-M / SiO 2 Catalytic hydrodeoxygenation of fatty acid methyl esters

[0021]

[0022] Ni-Mo / SiO 2 The conversion rate of catalytic methyl decanoate reaction was 98.7%, and the product nC 10 、nC 9 The selectivity of alkanes was 81.4% and 17.3% respectively; the conversion rate of methyl laurate catalyzed reaction was 97.9%, and the product nC 12 、nC 11 The selectivity of alkanes was 79.7% and 18.2% respectively; the conversion rate of methyl myristic acid ester was 98.5%, and the product nC 14 、nC 13 The selectivities were 81.7% and 16.8% respectively; the conversion rate of catalytic palmitic acid methyl ester reaction was 99.1%, and the product nC 16 、nC 15 The selectivities were 83.4% and 15.7% respectively; the conversion rate of catalytic stearic acid methyl ester reaction was 98.3%, and the product nC 18 、nC 17 The selectivity of alkanes was 82.5% and 15.8% respectively; the conversion rate of catalytic natural oil Jatropha curcas oil and nC 13-18 The molar yields of alkanes were 93.5% and 89.6%, respectively, of which nC N 、nC N-1 The selectivity of alkanes (N=14, 16, 18) was 80.3% and 15.5% respectively; the conversion rate and nC 13-18 The molar yields of alkanes were 86.8% and 78.5% respectively. 2 Comparative results of the hydrodeoxygenation of natural oils Jatropha oil and waste cooking oil catalyzed by catalysts.

[0023] Table 4 Ni-M / SiO 2 Catalytic hydrodeoxygenation of jatropha oil and waste cooking oil

[0024]

[0025] From the reaction results in Table 3 and Table 4 above, it can be seen that Ni-Mo / SiO has the best catalytic effect.

[0026] (3) ICP-AES was used to analyze the Ni ion content in the reaction solution after the catalyst was used for 5 consecutive cycles. The results showed that Ni-M / SiO 2 The Ni loss is 0.038%, but the Ni / SiO 2 The Ni loss is 0.48%.

[0027] TEM characterization of the catalyst after five consecutive cycles showed that Ni / SiO 2 The agglomeration of medium-nanometer Ni particles is serious, and Ni-W / SiO 2 and Ni-Fe / SiO 2 Next is Ni-Mo / SiO 2 The nano-Ni particles in the catalyst are only slightly agglomerated.

[0028] Raman spectroscopy was performed on the catalysts after five cycles of use. All four catalysts showed a D band at 1261 cm -1 Department and G belt 1593cm -1 There is a broad peak at the D band and the G band. The former is the defect site of highly active amorphous carbon species, and the latter is the tangential vibration of CC bonds in graphite carbon structure, i.e. hard carbon species. The intensity ratio of D band to G band is I D / I G for Ni-Mo / SiO 2 3.38>Ni-W / SiO 2 3.15>Ni-Fe / SiO 2 1.95>Ni / SiO 2 1.41, indicating that Ni-Mo / SiO 2 The carbon deposits formed on the surface are mainly renewable amorphous carbon species, and to remove the hard carbon, high-temperature calcination above 600°C is generally required. However, such high-temperature calcination will promote the agglomeration of Ni nanoparticles and deactivate the catalyst.

[0029] (4)Ni-Mo / SiO 2 The catalyst was prepared by the following method: 0.424 g Ni(CH 3 COO 2 , 0.085 g (NH 4 ) 6 Mo 7 O 24 and 2.865 g tetraethyl orthosilicate (C 8 H 20 O 4Si) was dissolved in 30 mL of double distilled water in an eggplant-shaped bottle, stirred continuously at 45 °C for 4 h, and then 20 mL of 30 wt% ammonia solution was added to control its pH value to 13 to precipitate metal ions and hydrolyze tetraethyl orthosilicate. After stirring continuously for 2 h, the water was removed by rotary evaporation at 70 °C for 1 h, dried at 100 °C in an oven for 8 h, and heated to 500 °C in a muffle furnace at a rate of 2 °C / min for calcination for 6 h to obtain Ni-Mo / SiO 2 Oxide, Ni-Mo / SiO 2 The oxide is placed in a hydrogen atmosphere in a tube furnace, H 2 The flow rate was 45 mL / min, the heating rate was 2 °C / min and the temperature was raised to 500 °C for 4 h to obtain Ni-Mo / SiO 2 Bimetallic catalysts.

[0030] Comparative catalyst Ni / SiO 2 (without additives), Ni-W / SiO 2 、Ni-Fe / SiO 2 Preparation process and preparation of Ni-Mo / SiO 2 The catalysts are similar, but no additives are added or the additives added are 0.127 g ammonium metatungstate and 0.083 g FeCl 3 .

[0031] (5)Ni-Mo / SiO 2 The catalyst characteristics are as follows:

[0032] To compare Ni-Mo / SiO 2 The characterization properties of the catalyst are also listed below: Ni / SiO 2 、Ni-W / SiO 2 、Ni-Fe / SiO 2 Comparative characterization data of Ni / SiO 2 、Ni-W / SiO 2 、Ni-Fe / SiO 2 、Ni-Mo / SiO 2 Abbreviated as four catalysts.

[0033] XRD characterization showed that all four catalysts showed a phase at 22.8°, which was attributed to amorphous SiO 2 The broad peak of Ni in the catalyst is 44.5°, 51.7° and 76.1°, which are attributed to Ni(111), Ni(200) and Ni(220 crystal plane), respectively. There are no obvious characteristic diffraction peaks of Mo, W and Fe oxide additives, indicating that these additive oxides are highly dispersed in the catalyst. The diffraction intensity of Ni characteristic diffraction peak in the catalyst is Ni-Mo / SiO 2 <Ni-W / SiO2 <Ni / SiO 2 <Ni-Fe / SiO 2 , indicating that Ni-Mo / SiO 2 The Ni nanoparticles are well dispersed, and the introduction of Mo inhibits the agglomeration of the nano-Ni particles in the nanocatalyst.

[0034] Field emission SEM and HRTEM characterization Field emission SEM showed that the four catalysts all showed nearly spherical particle morphology, except for Ni-Mo / SiO 2 and Ni-W / SiO 2 The uniformly dispersed metal nanoparticles are clearly observed on the surface, and the Ni-Fe / SiO 2 and Ni / SiO 2 No uniformly dispersed metal nanoparticles were observed; high-resolution HRTEM characterization showed that Ni-Mo / SiO 2 The minimum particle size of medium-nano Ni particles is 3.84nm <Ni-W / SiO 2 The particle size of the nano Ni particles is 5.86nm <Ni / SiO 2 The particle size of the nano Ni particles is 6.56 nm <Ni-Fe / SiO 2 The particle size of the nano-Ni particles in the catalyst is 9.53 nm, indicating that the Mo additive is more effective in promoting the dispersion of nano-Ni particles in the catalyst.

[0035] STEM-EDX spectrum characterizationSTEM-EDX spectrum characterization shows that Ni-Mo / SiO 2 and Ni-W / SiO 2 Ni, Mo and W are uniformly dispersed in Ni-Mo / SiO 2 and Ni-W / SiO 2 The distance between Ni-Mo and Ni-W is closer, which is more conducive to the formation of Ni-Mo and Ni-W during the catalyst reduction process and inhibits the agglomeration of nano-Ni particles.

[0036] H 2 -TPR characterization of catalysts in H 2 -TPR spectrum shows three types of characteristic peaks: (i) α characteristic peak in the range of 50-300℃, which is attributed to the partial reduction of the surface of M oxide particles, accompanied by the oxidation of O V Species formation; (ii) β characteristic peak in the range of 300-390℃, which is attributed to amorphous NiO and SiO 2 NiO reduction with weak interaction with the carrier; (iii) γ characteristic peak in the range of 390-470℃, which is attributed to Ni 2+-M oxide and the support have strong interaction with each other, indicating that there is a strong interaction between Ni and the additive M oxide; Ni-Mo / SiO 2 There is an α peak and a very broad γ peak, indicating that Ni-Mo / SiO 2 The Ni species mainly come from type (iii) NiO reduction.

[0037] EPR characterization EPR was used to characterize the O V Content characterization, Ni-Mo / SiO 2 、Ni-W / SiO 2 、Ni-Fe>SiO 2 There is a sharp characteristic peak at g = 2.005, which is attributed to O V Species formation, its intensity Ni-Mo / SiO 2 >Ni-W / SiO 2 >Ni-Fe>SiO 2 , indicating that Ni-Mo / SiO 2 Medium V The content is high, which is beneficial to the adsorption and activation of C=O / CO in the reactants.

[0038] Characterization of magnetic saturation intensity Saturation magnetization intensity of four catalysts Ni-Mo / SiO 2 Minimum 0.48emu / g Ni This is consistent with the change in the size of nano-Ni in the four catalysts, which is attributed to the different interactions between Ni-M oxides in the catalysts. The stronger the interaction between Ni-M oxides, the stronger the sintering resistance of the catalyst during high-temperature reduction, thereby forming small-sized nano-Ni particles, resulting in lower saturation magnetization.

[0039] XPS characterization XPS was used to characterize the valence and content of elements on the catalyst surface. The results are shown in Table 5:

[0040] Table 5 Ni-M / SiO 2 Catalyst surface component data (determined by XPS)

[0041]

[0042] Table 5 L , O V , O -OH represent lattice oxygen, oxygen vacancies, and catalyst surface hydroxyl groups, respectively. M+ oxides come from the partial reduction of the additive metal M oxide nanoparticles. This process often produces O V ;

[0043] Ni-Mo / SiO 2Ni 2p appeared at 852.93, 854.71, 856.24 and 861.34 eV 3 / 2 orbital characteristic peaks, which are respectively attributed to Ni 0 、Ni 2+ and its corresponding satellite peaks, Ni 0 -Mo has a maximum binding energy of 852.93 eV, which is greater than that of bulk Ni 0 The binding energy is 852.7 eV, indicating that Ni-Mo / SiO 2 The electrons at the Ni site transfer from Ni to Mo oxide, which reduces the charge density at the Ni site, thereby inhibiting the adsorption of highly active amorphous carbon produced during the catalytic hydrodeoxygenation reaction of bio-oil by electron-rich Ni, and preventing the Ni site from being covered by carbon deposits and deactivating. 2 Surface nano-Ni 0 The highest particle content is 36.05%. Mo reduces the surface energy of Ni nanoparticles, thereby inhibiting the agglomeration of Ni nanoparticles. The smaller the size of Ni nanoparticles, the more it adsorbs and dissociates H 2 The stronger the activity, the more Ni-H species there are, and the higher the catalytic activity;

[0044] The O1s spectrum of the catalyst was separated by Gaussian peak fitting method to obtain O L , O V and O -OH Three peaks: (1) lattice oxygen (529.78 eV), (2) oxygen vacancy (530.76 eV), (3) chemically adsorbed oxygen (531.47 eV), Ni-Mo / SiO 2 Catalyst O V / (O L +O V +O -OH ) is up to 32.72%, indicating that its surface O V The more the species content, the more conducive it is to the adsorption and activation of C=O / CO in the reactants, and the more conducive it is to the formation of Ni-O V -MoO x Interface sites, promoting the charge transfer from Ni to MoO x The oxygen vacancies are transferred to the upper part, thereby reducing the charge density of the Ni site and its adsorption degree to C atoms, thereby improving the carbon deposition resistance;

[0045] Further analysis of Mo 3d, W 4f, Fe 2p 3 / 2 Track, M oxide content Ni-Mo / SiO 2 The highest is 36.09%; M δ+ The oxides come from the partial reduction of the additive metal M oxide nanoparticles, which often produces O V, which is beneficial to the adsorption of carbonyl oxygen in the reaction raw materials and increase the catalytic activity;

[0046] Ni-M / SiO 2 The charge density on the Ni site is composed of M oxide and M 0 Jointly determined, Ni-Mo / SiO 2 The Mo oxide content is higher than Mo 0 , and Ni and Mo have similar electronegativity, so Ni will not take charge from Mo atoms, but O in Mo oxide V There are many sites, which can capture more charges from Ni atoms, so Ni-Mo / SiO 2 The Ni charge density is reduced;

[0047] In situ FT-IR spectroscopy of CO adsorption In situ FT-IR characterizes the effect of the oxophilic additive M on the electron density at the Ni site in the catalyst. The strong absorption peak represents the Ni··C=O adsorption configuration, including the linear adsorption of C=O (2125~1975cm -1 , linear ν CO ) and bridge adsorption (1975~1850cm -1 , bridge type ν CO ); at 2070cm -1 and 2014cm -1 The characteristic peak of stretching vibration at the position is attributed to the linear adsorption of CO molecules on Ni by coordination. 0 At the top position, the oxophilic additive M did not have a significant effect on the vibration frequency corresponding to the adsorption configuration; however, after the introduction of the oxophilic additive Mo, the vibration frequency at 1947 cm -1 and 1915cm -1 A new weaker CO molecular stretching vibration characteristic peak (CO bridge adsorption) appears at the position, which is attributed to the adsorption of CO molecules on the coordination unsaturated sites (such as O V site); Ni-Mo / SiO 2 The CO bridge adsorption characteristic peak is the strongest, indicating that O V A large number of sites; Ni-Mo / SiO 2 The characteristic peaks of mid-bridge CO adsorption showed a certain blue shift (1921→1930→1947cm -1 ), indicating that there is a certain interaction between Ni-Mo oxides, which further weakens the electron density on the Ni site, and the charge is transferred from Ni-O V -MO x Interface from Ni 0 O V Site transfer; Ni 0 The reduction of the charge density on the site is beneficial to reduce the Ni 0 For C=O functional groups in bio-oils δ+The strong adsorption of Ni 0 The charge density on the site can also weaken the Ni 0 The adsorption of highly active amorphous carbon produced during the catalytic hydrodeoxygenation reaction of bio-oil prevents the Ni site from being covered by carbon deposits and deactivating it.

[0048] The Ni-Mo / SiO2 catalyst for catalyzing the hydrodeoxygenation of bio-oil to produce hydrocarbon fuels is described above. 2 The catalyst is characterized by a Ni-Mo / SiO catalyst for catalyzing the hydrodeoxygenation of bio-oil to produce hydrocarbon fuels. 2 The technical solution of the catalyst is briefly described as follows:

[0049] (1) The bio-oil is any one of methyl caprate, methyl laurate, methyl myristic acid, methyl palmitate, and methyl stearate; the bio-oil may also be derived from natural oil such as jatropha curcas oil or waste cooking oil from restaurants;

[0050] (2) The Ni-Mo / SiO 2 The catalyst is composed of Ni, Mo and SiO 2 Support composition, Ni, Mo and SiO 2 Support molar ratio 0.1:0.03:1; Ni-Mo / SiO 2 The catalyst is a mesoporous particle structure with a rough surface, a pore size of 5.48 nm, a particle size of 100-200 nm, and a pore volume of 0.33 cm 3 / g, specific surface area 185m 2 / g;Ni-Mo / SiO 2 The Ni loading in the catalyst is 9.73% (wt.%), the particle size of the nano-Ni particles is 3.84-4.9 nm, and the dispersion of the nano-Ni particles is 2.35%; Ni-Mo / SiO 2 The chemical adsorption Ni-H number of the catalyst is 78.3 μmol / g, and the total acidity is 0.146 mmol·g -1 ;

[0051] (3) In Ni-Mo / SiO 2 The mass ratio of catalyst to raw material bio-oil was 0.2:1, the hydrogen pressure was 3MPa, the reaction temperature was 300℃, and the high pressure and closed reaction was carried out for 4h. After cooling and centrifugation to separate the catalyst, the product hydrocarbon fuel was obtained: the conversion rate of methyl decanoate was 98.7%, and the product nC 10 、nC 9 The selectivity of alkanes was 81.4% and 17.3% respectively; the conversion rate of methyl laurate catalyzed reaction was 97.9%, and the product nC 12 、nC 11The selectivity of alkanes was 79.7% and 18.2% respectively; the conversion rate of methyl myristic acid ester was 98.5%, and the product nC 14 、nC 13 The selectivities were 81.7% and 16.8% respectively; the conversion rate of catalytic palmitic acid methyl ester reaction was 99.1%, and the product nC 16 、nC 15 The selectivities were 83.4% and 15.7% respectively; the conversion rate of catalytic stearic acid methyl ester reaction was 98.3%, and the product nC 18 、nC 17 The selectivity of alkanes was 82.5% and 15.8% respectively; the conversion rate of catalytic natural oil Jatropha curcas oil and nC 13-18 The molar yields of alkanes were 93.5% and 89.6%, respectively, of which nC N 、nC N-1 The selectivity of alkanes (N=14, 16, 18) was 80.3% and 15.5% respectively; the conversion rate and nC 13-18 The molar yields of alkanes were 86.8% and 78.5%, respectively;

[0052] (4) Analysis of Ni-Mo / SiO by ICP-AES 2 The Ni ion content in the reaction solution after the catalyst was used for 5 consecutive cycles was obtained. 2 The Ni loss in the catalyst was 0.038%; the Ni-Mo / SiO 2 TEM characterization of the catalyst showed that Ni-Mo / SiO 2 The nano-Ni particles in the catalyst were only slightly agglomerated; the Ni-Mo / SiO 2 Mann spectroscopy characterization of the catalyst, at D band 1261 cm -1 Department and G belt 1593cm -1 There is a broad peak at each of the two bands. The former is the defect site of highly active amorphous carbon species, and the latter is the tangential vibration of CC bonds in graphite carbon structure, i.e. hard carbon species. The intensity ratio of D band to G band is I D / I G is 3.38, indicating that Ni-Mo / SiO 2 The carbon deposits formed on the surface are mainly renewable amorphous carbon, and to remove the hard carbon, high-temperature calcination above 600°C is required. However, such high-temperature calcination will promote the agglomeration of Ni nanoparticles and deactivate the catalyst.

[0053] (5)Ni-Mo / SiO 2 The catalyst was prepared by the following method: 0.424 g Ni(CH 3 COO 2, 0.085 g (NH 4 ) 6 Mo 7 O 24 and 2.865 g tetraethyl orthosilicate (C 8 H 20 O 4 The mixture was stirred for 4 h at 45 °C, and 20 mL of 30 wt% ammonia solution was added to precipitate metal ions and hydrolyze tetraethyl orthosilicate. After stirring for 2 h, the mixture was evaporated at 70 °C for 1 h to remove water, dried at 100 °C for 8 h in an oven, and heated to 500 °C in a muffle furnace at a rate of 2 °C / min for 6 h to obtain Ni-Mo / SiO 2 Oxide, Ni-Mo / SiO 2 The oxide is placed in a hydrogen atmosphere in a tube furnace, H 2 The flow rate was 45 mL / min, the heating rate was 2 °C / min and the temperature was raised to 500 °C for 4 h to obtain Ni-Mo / SiO 2 catalyst.

[0054] Technical advantages, features and effects of the present invention

[0055] 1. The catalyst of the present invention has low cost, high catalytic activity and nC N 、nC N-1 The alkane product is selective and easy to separate from the reaction system.

[0056] 2. When Ni-Mo / SiO 2 The mass ratio of bio-oil to 0.2:1, hydrogen pressure 3MPa, reaction temperature 300℃, reaction time 4h, catalytic methyl decanoate reaction conversion rate 98.7%, nC 10 、nC 9 Alkane selectivity 81.4%, 17.3%; methyl laurate reaction conversion rate 97.9%, nC 12 、nC 11 Alkane selectivity 79.7%, 18.2%; methyl myristic acid ester reaction conversion rate 98.5%, nC 14 、nC 13 Selectivity 81.7%, 16.8%; methyl palmitate reaction conversion rate 99.1%, nC 16 、nC 15 Selectivity 83.4%, 15.7%; methyl stearate reaction conversion rate 98.3%, nC 18 、nC 17 Selectivity 82.5%, 15.8%; Jatropha curcas oil reaction conversion rate and nC 13-18The molar yields were 93.5% and 89.6%; the conversion rate and nC 13-18 The molar yields of alkanes were 86.8% and 78.5%, respectively.

[0057] The technical solution of the present invention and its implementation methods are described below by way of examples, but the technical solution of the present invention is not limited to the following examples.

[0058] Example 1 0.424 g Ni(CH 3 COO 2 , 0.085 g (NH 4 ) 6 Mo 7 O 24 and 2.865 g tetraethyl orthosilicate (C 8 H 20 O 4 Si) was dissolved in 30 mL of double distilled water in an eggplant-shaped bottle, stirred continuously at 45 °C for 4 h, and then 20 mL of 30 wt% ammonia solution was added to control its pH value to 13 to precipitate metal ions and hydrolyze tetraethyl orthosilicate. After stirring continuously for 2 h, the water was removed by rotary evaporation at 70 °C for 1 h, dried at 100 °C in an oven for 8 h, and heated to 500 °C in a muffle furnace at a rate of 2 °C / min for calcination for 6 h to obtain Ni-Mo / SiO 2 Oxide, Ni-Mo / SiO 2 The oxide is placed in a hydrogen atmosphere in a tube furnace, H 2 The flow rate was 45 mL / min, the heating rate was 2 °C / min and the temperature was raised to 500 °C for 4 h to obtain Ni-Mo / SiO 2 Bimetallic catalysts.

[0059] Comparative catalyst Ni / SiO 2 (without additives), Ni-W / SiO 2 、Ni-Fe / SiO 2 Preparation process and Ni-Mo / SiO 2 Similar, but no additives are added or the additives added correspond to 0.127 g ammonium metatungstate and 0.083 g FeCl 3 .

[0060] Example 2 In Ni-Mo / SiO 2 The mass ratio of catalyst to raw material bio-oil was 0.2:1, the hydrogen pressure was 3MPa, the reaction temperature was 300℃, and the high pressure and closed reaction was carried out for 4h. After cooling and centrifugation to separate the catalyst, the product hydrocarbon fuel was obtained. The conversion rate of methyl decanoate reaction was 98.7%, and the product nC 10 、nC 9The selectivity of alkanes was 81.4% and 17.3% respectively; the conversion rate of methyl laurate catalyzed reaction was 97.9%, and the product nC 12 、nC 11 The selectivity of alkanes was 79.7% and 18.2% respectively; the conversion rate of methyl myristic acid ester was 98.5%, and the product nC 14 、nC 13 The selectivities were 81.7% and 16.8% respectively; the conversion rate of catalytic palmitic acid methyl ester reaction was 99.1%, and the product nC 16 、nC 15 The selectivities were 83.4% and 15.7% respectively; the conversion rate of catalytic stearic acid methyl ester reaction was 98.3%, and the product nC 18 、nC 17 The selectivities of alkanes are 82.5% and 15.8% respectively.

[0061] Example 3 has the same reaction conditions and process as Example 2, Ni-Mo / SiO 2 Catalytic reaction conversion rate and nC of natural oil Jatropha curcas oil 13-18 The molar yields of alkanes were 93.5% and 89.6%, respectively, of which nC N 、nC N-1 The selectivities of alkanes (N=14, 16, 18) were 80.3% and 15.5%, respectively.

[0062] Example 4 has the same reaction conditions and process as Example 2, Ni-Mo / SiO 2 Conversion rate and nC of catalytic hydrodeoxygenation reaction of waste cooking oil 13-18 The molar yields of alkanes were 86.8% and 78.5%, respectively.

[0063] Example 5 As a comparison, under the same reaction conditions and processes as in Examples 2, 3, and 4, Tables 3 and 4 in the above technical scheme respectively list several Ni-M / SiO 2 The results of hydrodeoxygenation of fatty acid methyl ester, natural oil jatropha oil or catering waste cooking oil catalyzed by the catalyst are shown in Table 3 and Table 4. It can be seen that Ni-Mo / SiO has the best catalytic effect.

[0064] Example 6 ICP-AES was used to analyze the Ni ion content in the reaction solution after the catalyst was used for 5 consecutive cycles. The results showed that Ni-M / SiO 2 The Ni loading in the catalyst lost 0.038%, but the Ni / SiO 2 The catalyst Ni loading loss was 0.48%.

[0065] TEM characterization of the catalyst after 5 consecutive cycles showed that Ni / SiO 2The agglomeration of medium-nanometer Ni particles is serious, and Ni-W / SiO 2 and Ni-Fe / SiO 2 Next is Ni-Mo / SiO 2 The nano-Ni particles in the catalyst are only slightly agglomerated.

[0066] Raman spectroscopy was used to characterize the catalysts after five cycles. All four catalysts showed a D band at 1261 cm -1 Department and G belt 1593cm -1 There is a broad peak at the D band and the G band. The former is the defect site of highly active amorphous carbon species, and the latter is the tangential vibration of CC bonds in graphite carbon structure, i.e. hard carbon species. The intensity ratio of D band to G band is I D / I G for Ni-Mo / SiO 2 3.38>Ni-W / SiO 2 3.15>Ni-Fe / SiO 2 1.95>Ni / SiO 2 1.41, indicating that Ni-Mo / SiO 2 The carbon deposits formed on the surface are mainly renewable amorphous carbon species, and to remove the hard carbon, high-temperature calcination above 600°C is generally required. However, such high-temperature calcination will promote the agglomeration of Ni nanoparticles and deactivate the catalyst.

[0067] Example 7Ni-Mo / SiO 2 Catalyst characterization

[0068] To compare Ni-Mo / SiO 2 The characterization properties of the catalyst are also listed below: Ni / SiO 2 、Ni-W / SiO 2 、Ni-Fe / SiO 2 Comparative characterization data of Ni / SiO 2 、Ni-W / SiO 2 、Ni-Fe / SiO 2 、Ni-Mo / SiO 2 Abbreviated as four catalysts.

[0069] XRD characterization showed that all four catalysts showed a phase at 22.8°, which was attributed to amorphous SiO 2 The broad peak of Ni in the catalyst is shown in Figure 2. The characteristic diffraction peaks of Ni metal appear at 44.5°, 51.7°, and 76.1°, which are attributed to Ni(111), Ni(200), and Ni(220 crystal plane), respectively. There are no obvious characteristic diffraction peaks of Mo, W, and Fe oxide additives, indicating that these additive oxides are highly dispersed in the catalyst. The diffraction intensity of Ni characteristic diffraction peak in the catalyst is Ni-Mo / SiO 2<Ni-W / SiO 2 <Ni / SiO 2 <Ni-Fe / SiO 2 , indicating that Ni-Mo / SiO 2 The Ni nanoparticles are well dispersed, and the introduction of Mo inhibits the agglomeration of the nano-Ni particles in the nanocatalyst.

[0070] Field emission SEM and HRTEM characterization Field emission SEM showed that the four catalysts all showed nearly spherical particle morphology, except for Ni-Mo / SiO 2 and Ni-W / SiO 2 The uniformly dispersed metal nanoparticles are clearly observed on the surface, and the Ni-Fe / SiO 2 and Ni / SiO 2 No uniform dispersion of metal nanoparticles was observed; high-resolution HRTEM characterization showed that Ni-Mo / SiO 2 The minimum particle size of medium-nano Ni particles is 3.84nm <Ni-W / SiO 2 The particle size of the nano Ni particles is 5.86nm <Ni / SiO 2 The particle size of the nano Ni particles is 6.56 nm <Ni-Fe / SiO 2 The particle size of the nano-Ni particles in the sample is 9.53 nm, which further indicates that the Mo additive is more effective in dispersing the nano-Ni particles. HRTEM characterization determines that the Ni-Mo / SiO 2 、Ni-W / SiO 2 The lattice spacings of Ni-Mo / SiO are 0.203 and 0.205 nm, respectively, indicating that the Ni(111) crystal plane is exposed on the surface of these catalysts. No obvious lattice spacings attributable to Mo, W, and Fe oxides are observed, which is due to the high dispersion of Mo, W, and Fe oxides. 2 and Ni-W / SiO 2 The lattice spacing of the Ni(111) crystal plane is slightly larger than that of Ni-Fe / SiO 2 The reason is that some Ni atoms in the Ni(111) lattice are replaced by Mo and W atoms with larger atomic radius, which causes lattice distortion and increases the lattice spacing. This also indirectly indicates that the Ni-Mo / SiO 2 and Ni-W / SiO 2 The contact between the medium-nano Ni particles and Mo oxides and W oxides is closer than that between the Ni particles and Fe oxides.

[0071] STEM-EDX spectrum characterizationSTEM-EDX spectrum characterization shows that Ni-Mo / SiO 2 and Ni-W / SiO 2 Ni, Mo and W are uniformly dispersed in Ni-W / SiO2 There is still slight aggregation of nano-Ni particles in some areas of the spectrum; although Ni-Fe / SiO 2 The Fe species in the measured area showed a high dispersion state, but the aggregation of nano-Ni particles was also obvious; Ni-Mo / SiO 2 and Ni-W / SiO 2 The distance between Ni-Mo and Ni-W is closer, which is more conducive to the formation of Ni-Mo and Ni-W during the catalyst reduction process and inhibits the agglomeration of nano-Ni particles.

[0072] H 2 -TPR characterization of catalysts in H 2 -TPR spectrum shows three types of characteristic peaks: (i) α characteristic peak in the range of 50-300℃, which is attributed to the partial reduction of the surface of M oxide particles, accompanied by the oxidation of O V Species formation; (ii) β characteristic peak in the range of 300-390℃, which is attributed to amorphous NiO and SiO 2 NiO reduction with weak carrier interaction; (iii) γ characteristic peak in the range of 390-470℃, which is attributed to Ni 2+ -M oxide and the support have strong interaction with each other, indicating that there is a strong interaction between Ni and the additive M oxide; Ni / SiO 2 Only β peak, Ni-W / SiO 2 There are α, β and γ peaks, Ni-Fe / SiO 2 There are α and β peaks, Ni-Mo / SiO 2 There is an α peak and a very broad γ peak, indicating that Ni-Mo / SiO 2 The Ni species in the solution mainly come from the reduction of type (iii) NiO species, Ni-Fe / SiO 2 The Ni species in the Ni-W / SiO 2 The Ni species in the Ni-Fe / SiO are mainly from the reduction of NiO species of type (ii) and (iii). 2 There is no obvious reduction characteristic peak of NiO species belonging to type (iii), but Ni-Fe / SiO 2 The β peak position is 395℃, which is higher than Ni / SiO 2 348℃, indicating that Ni-Fe / SiO 2 There is still a certain role of Ni-Fe oxide in the 2 Reduction characteristics and Ni-W / SiO 2 The γ peak position of 484℃ is higher than that of Ni-Mo / SiO 2 461℃, indicating that Ni2+ -M oxide strength Ni-W / SiO 2 >

[0073] Ni-Mo / SiO 2 >Ni-Fe / SiO 2 This is consistent with the strong affinity of the three additives to Ni, and the dissociation energy is WO (653 kJ / mol)> Mo-O (607 kJ / mol)> Fe-O (407 kJ / mol)> Ni-O (366 kJ / mol); Ni 2+ The changes in the interaction between -M oxides further illustrate that the introduction of oxophilic additives is beneficial to improving the thermal stability and dispersibility of nano-Ni particles in the catalyst.

[0074] EPR characterization EPR was used to characterize the O V Content characterization, Ni-Mo / SiO 2 、Ni-W / SiO 2 、Ni-Fe>SiO 2 There is a sharp characteristic peak at g = 2.005, which is attributed to O V Species formation, its intensity Ni-Mo / SiO 2 >Ni-W / SiO 2 >Ni-Fe>SiO 2 , indicating that Ni-Mo / SiO 2 Medium V The content is high, which is beneficial to the adsorption and activation of C=O / CO in the reactants.

[0075] Magnetic saturation intensity characterization of Ni / SiO 2 Saturation magnetization 5.88emu / g Ni , which is much lower than the magnetic saturation intensity of large-particle bulk metal Ni (2-3 μm), 55 emu / g Ni This is due to the Ni / SiO 2 The reason why the medium-nanometer Ni particle size is 6.56nm is small;

[0076] Ni-Mo / SiO 2 and Ni-W / SiO 2 With lower saturation magnetization, 0.48 and 1.89emu / g respectively Ni , but Ni-Fe / SiO 2 The saturation magnetization is 7.12emu / g Ni , the saturation magnetization of the four catalysts Ni-Fe / SiO 2 >Ni / SiO 2 >

[0077] Ni-W / SiO2 >Ni-Mo / SiO 2 , which is consistent with the change in the size of nano-Ni in the four catalysts, which is attributed to the different interactions between Ni-M oxides in the catalysts. The stronger the interaction between Ni-M oxides, the stronger the sintering resistance of the catalyst during high-temperature reduction, thereby forming small-sized nano-Ni particles, resulting in lower saturation magnetization.

[0078] XPS characterization XPS was used to characterize the valence and content of elements on the catalyst surface. 2 Ni 2p appeared at 852.93, 854.71, 856.24 and 861.34 eV 3 / 2 orbital characteristic peaks, which are respectively attributed to Ni 0 、Ni 2+ and its corresponding satellite peaks, Ni 0 -M binding energy is Ni-Mo / SiO 2 852.93eV>Ni-W / SiO 2 852.58eV>Ni-Fe / SiO 2 852.14eV, Ni-Mo / SiO 2 The Ni-Mo binding energy is greater than that of bulk Ni 0 The binding energy is 852.7eV, which means electron loss, and the charge density on the Ni site decreases; in addition, Ni-Mo / SiO 2 Chinese Ni 0 The binding energy is 852.93 eV, which is higher than that of bulk Ni. 0 852.7eV, indicating that Ni-Mo / SiO 2 The electrons at the Ni site transfer from Ni to Mo oxide, resulting in a decrease in the charge density at the Ni site. 2 and Ni-Fe / SiO 2 In their Ni 0 The electron binding energy reduction values ​​are 0.12 and 0.56 eV respectively, and the electrons are transferred from the additive oxide to the Ni site (WO x →Ni、FeO x →Ni), which increases the charge density on the Ni site, indicating that among the three catalysts, Ni-Mo / SiO 2 The Ni site has the lowest charge density, which inhibits the adsorption of electron-rich Ni on the highly active amorphous carbon produced during the hydrodeoxygenation reaction of bio-oils, thus preventing the Ni site from being covered by carbon deposits and deactivating. 2 Surface nano-Ni 0 Particle content 36.05%>Ni-W / SiO 2 Ni 0Particle content 31.96%>Ni-Fe / SiO 2 Ni 0 The particle content is 15.4%. Mo reduces the surface energy of Ni nanoparticles, thereby inhibiting the agglomeration of Ni nanoparticles. The smaller the size of Ni nanoparticles, the more it adsorbs and dissociates H 2 The stronger the activity, the more Ni-H species there are, and the higher the catalytic activity.

[0079] The O1s spectrum of the catalyst was separated by Gaussian peak fitting method to obtain O L , O V and O -OH Three peaks: (1) lattice oxygen (529.78 eV), (2) oxygen vacancies (530.76 eV), and (3) chemically adsorbed oxygen species (531.47 eV). V / (O L +O V +O -OH ) ratios are Ni-Mo / SiO 2 32.72%>Ni-W / SiO 2 28.87%>Ni-Fe / SiO 2 21.45% of the surface O V The more the species content, the more conducive it is to the adsorption and activation of C=O / CO in the reactants, and the more conducive it is to the formation of Ni-O V -MoO x Interface sites, promoting the charge transfer from Ni to MoO x The oxygen vacancies on the Ni site are transferred, thereby reducing the charge density of the Ni site and its adsorption degree to C atoms, thereby improving the anti-carbon deposition property.

[0080] Further analysis of Mo 3d, W 4f, Fe 2p 3 / 2 Orbital, metal removal in catalysts 0 In addition to the single substance, M δ+ Oxide, Ni-Mo / SiO 2 Medium δ+ Oxide content 36.09%>Ni-Fe / SiO 2 Medium δ+ Oxide content 23.11%>Ni-W / SiO 2 Medium δ+ The oxide content is 22.82%, while Ni-W / SiO 2 Medium 0 Content 22.5% <Ni-Mo / SiO 2 Medium 0 Content 24.84% <Ni-Fe / SiO 2 Medium 0Content 59.46%; M δ+ The oxides come from the partial reduction of the additive metal M oxide nanoparticles, which often produces O V The stronger the metal-oxygen bond, the more difficult it is to reduce the additive oxide particles, increasing the O V The difficulty of forming carbonyl oxygen leads to a decrease in the number of carbonyl oxygen adsorption sites and a decrease in catalytic activity; however, too low metal-oxygen bond strength will cause M oxide to be further reduced to M 0 The catalytic activity is reduced by forming Ni-M alloy or Ni-M intermetallic compound with Ni site.

[0081] Ni-M / SiO 2 The charge density on the Ni site is composed of M oxide and M 0 Joint determination; Ni-Fe / SiO 2 Medium 0 The content is much higher than Ni-W / SiO 2 、Ni-W / SiO 2 , and the electronegativity of Ni atom 1.88 is greater than that of Fe atom 1.83, resulting in the charge transfer from Fe to Ni; while Ni-Mo / SiO 2 The Mo-O bond strength is moderate, O V The species content is the highest, which is conducive to accelerating the hydrogenation conversion of C=O / CO bonds; Ni-W / SiO 2 The W oxide content is slightly higher than that of W 0 However, the electronegativity of Ni is 1.88, which is higher than that of W, which is 1.7. Ni is more capable of taking charge from W atoms than O in W oxide. V The site can capture the charge of Ni atoms, so Ni-W / SiO 2 The Ni charge density in Ni-Mo / SiO 2 The Mo oxide content is higher than Mo 0 , and Ni and Mo have similar electronegativity, so Ni will not take charge from Mo atoms, but O in Mo oxide V There are many sites, which can capture more charges from Ni atoms, so Ni-Mo / SiO 2 The Ni charge density decreases.

[0082] In situ FT-IR spectroscopy of CO adsorption In situ FT-IR characterizes the effect of the oxophilic additive on the electron density at the Ni site in the catalyst. The strong absorption peak represents the Ni··C=O adsorption configuration, including the linear adsorption of C=O (2125~1975cm -1 , linear ν CO ) and bridge adsorption (1975~1850cm -1 , bridge type ν CO ); at 2070cm -1and 2014cm -1 The characteristic peak of stretching vibration at the position is attributed to the linear adsorption of CO molecules on Ni by coordination. 0 The top position, the oxophilic additives did not have a significant effect on the vibration frequency corresponding to the adsorption configuration; however, after the introduction of the oxophilic additive Mo, the vibration frequency at 1947 cm -1 and 1915cm -1 A new weaker CO molecular stretching vibration characteristic peak (CO bridge adsorption) appears at the position, which is attributed to the adsorption of CO molecules on the coordination unsaturated sites (such as O V site); the intensity of CO bridge adsorption characteristic peaks in the three catalysts Ni-Mo / SiO 2 >Ni-W / SiO 2 >Ni-Fe / SiO 2 , which indicates that Ni-Mo / SiO 2 Medium V There are many sites; in addition, compared with Ni-Fe / SiO 2 Comparison, Ni-Mo / SiO 2 and Ni-W / SiO 2 The characteristic peaks of the mid-bridge CO adsorption showed a certain blue shift phenomenon (1921→1930→1947cm -1 ,1892→1903→1915cm -1 ), which indicates that Ni-MO x There is a certain interaction between them, and Ni-Mo>Ni-W>Ni-Fe, which further weakens the electron density on the Ni site; while in Ni / SiO 2 There is no obvious bridge CO adsorption characteristic peak in the solution, indicating that the introduction of oxygen-affinity additives can produce a certain amount of O V site, which is consistent with the EPR characterization results; Ni-Mo / SiO 2 and Ni-W / SiO 2 The blue shift of the mid-bridge CO molecule indicates that the electron density on the Ni site decreases and the charge shifts from Ni-O V -MO x Interface from Ni 0 To its neighbor MO x O on the particle surface V Site transfer; Ni 0 The reduction of the charge density on the site is beneficial to reduce the Ni 0 For C=O functional groups in bio-oils δ+ The strong adsorption of Ni 0 The charge density on the site can weaken the Ni 0 The adsorption of highly active amorphous carbon produced during the catalytic hydrodeoxygenation reaction of bio-oil prevents the Ni site from being covered and deactivated by carbon deposits.

Claims

1. A method for obtaining hydrocarbon fuel by hydrodeoxygenation of bio-oil catalyzed by Ni-Mo / SiO2 catalyst, characterized in that: (1) The Ni-Mo / SiO2 catalyst is prepared by the following method: 0.424 g Ni(CH3COO)2, 0.085 g (NH4)6Mo7O 24 and 2.865 g tetraethyl orthosilicate (C8H 20 O4Si) was dissolved in 30mL of double distilled water in an eggplant-shaped bottle, stirred continuously at 45°C for 4h, and then 20mL of 30 wt% ammonia solution was added to control its pH value to 13 to precipitate metal ions and hydrolyze tetraethyl orthosilicate. After stirring continuously for 2h, the water was removed by rotary evaporation at 70°C for 1h, dried in an oven at 100°C for 8h, and calcined at 500°C at a heating rate of 2°C / min in a muffle furnace for 6h to obtain Ni-Mo / SiO2 oxide. The Ni-Mo / SiO2 oxide was reduced in a tubular furnace in a hydrogen atmosphere with a H2 flow rate of 45mL / min and a heating rate of 2°C / min to 500°C for 4h to obtain a Ni-Mo / SiO2 bimetallic catalyst; (2) The Ni-Mo / SiO2 catalyst is composed of Ni, Mo and SiO2 carrier, and the molar ratio of Ni, Mo and SiO2 carrier is 0.1:0.03:1; the Ni-Mo / SiO2 catalyst is a mesoporous particle structure with a rough surface, a pore size of 5.48nm, a particle size of 100-200nm, and a pore volume of 0.33cm 3 / g, specific surface area 185m 2 / g; the nano-Ni particles in the Ni-Mo / SiO2 catalyst have a small particle size of 3.84-4.9nm, a good dispersion of 2.35%, and a large amount of chemically adsorbed Ni-H 78.3mol / g, so the Ni-Mo / SiO2 catalytic activity is good, and its acidity distribution is moderate: weak acid 0.122mmol·g -1 、Medium acid 0.025mmol·g -1 , total acidity 0.146mmol·g -1 ; (3) The bio-oil is any one of methyl caprate, methyl laurate, methyl myristic acid, methyl palmitate, and methyl stearate; the bio-oil also comes from natural oil Jatropha curcas oil or waste cooking oil from restaurants; the mass ratio of Ni-Mo / SiO2 catalyst to the reaction raw material bio-oil is 0.2:1, the hydrogen pressure is 3MPa, the reaction temperature is 300°C, the high-pressure closed reaction is carried out for 4h, cooled, and the catalyst is separated by centrifugation to obtain the product hydrocarbon fuel.

Citation Information

Patent Citations

  • Catalyst for reforming mathand and carbon dioxide to synthesize gas

    CN1344671A