Selenium vacancy molybdenum selenide materials and their preparation and application in HER catalysis
By calcining MoSe2 under a reducing atmosphere and negative pressure, selenium vacancy defects are constructed, which solves the problem of insufficient HER catalytic performance of MoSe2, significantly improves its catalytic activity and charge transfer ability in acidic and alkaline media, and achieves excellent HER Catalytic performance.
Patent Information
- Application Number
- CN202310037332.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-10
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2043-01-10
AI Technical Summary
MoSe2 has problems with insufficient number of active sites and low electron transfer ability in terms of HER catalytic performance, which limits its widespread use in industrial applications.
By calcining under a reducing atmosphere and negative pressure, and controlling the calcining temperature, selenium vacancy defects are constructed, and the electroactive sites and electron transport capabilities on the MoSe2 surface are improved, thereby improving its HER catalytic performance.
It significantly improves the HER catalytic activity of MoSe2 in acidic and alkaline media, reduces the overpotential and Tafel slope, increases the charge transfer speed and active site density, and achieves excellent HER catalytic performance.
Smart Images

Figure CN116002633B_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of catalytic materials, and specifically to the field of HER catalytic materials. Background Art
[0002] As a clean energy source, hydrogen is expected to become a substitute for fossil fuels. Water electrolysis is an effective way to prepare high-purity hydrogen. However, the large-scale application of water electrolysis faces the problem of selecting electrocatalysts. So far, precious metal (such as platinum)-based catalysts are the most active electrocatalysts, and they have a near-zero overpotential for the cathode hydrogen evolution reaction (HER). However, the high cost and scarcity of precious metal catalysts severely limit their widespread application in industry. Therefore, it is essential to develop non-precious metal catalysts with low cost and high HER catalytic activity.
[0003] Density functional theory (DFT) calculations demonstrate the high HER reactivity at the edge sites of MoS2, with a ΔG of 2.3 Å at 50% hydrogen coverage. H* is close to zero, so MoS2 has been widely studied as an ideal HER catalyst. At the same time, MoSe2 has also received a lot of attention due to its similar physical and chemical properties to MoS2. Like MoS2, MoSe2 has abundant edge active sites and exhibits good HER performance. In addition, compared with S, since Se has more obvious metallic properties, MoSe2 has better conductivity and will become a better non-precious metal catalyst than MoS2. Although MoSe2 has many advantages, there are still many factors that limit its HER performance, such as the small number of exposed active sites and low electron transfer ability. Therefore, so far, the HER performance of MoSe2 has not stood out. Summary of the invention
[0004] In view of the problem that MoSe2 HER catalytic performance is not ideal, the first purpose of the present invention is to provide a selenium vacancy molybdenum selenide material, aiming to provide a new material that can exhibit excellent HER catalytic performance in both acid and alkaline systems.
[0005] The second object of the present invention is to provide a method for preparing the selenium vacancy molybdenum selenide material, aiming to prepare the new material with excellent HER activity.
[0006] The third object of the present invention is to provide the use of the selenium vacancy molybdenum selenide material as a HER catalyst.
[0007] The fourth object of the present invention is to provide an electrode containing the molybdenum selenide material with selenium vacancies.
[0008] The fifth object of the present invention is to provide a molybdenum selenide material containing the selenium vacancies for use in electrolyzing water to produce hydrogen.
[0009] A selenium vacancy molybdenum selenide material is a molybdenum selenide material with selenium vacancies on the surface.
[0010] The present invention provides a new molybdenum selenide material with selenium vacancies on the surface. The material has abundant electroactive sites and fast charge transfer capability, exhibits low overpotential and Tafel slope in both alkaline and acidic media, and can exhibit excellent HER catalytic activity.
[0011] The selenium vacancy molybdenum selenide material of the present invention comprises a hexagonal phase molybdenum selenide core and a selenium vacancy rough surface shell composited thereon, forming a core-shell structure.
[0012] The present invention also provides a method for preparing the selenium vacancy molybdenum selenide material, wherein MoSe2 is roasted in a reducing atmosphere and under negative pressure to obtain the selenium vacancy molybdenum selenide material; wherein the temperature in the roasting stage is 650-750°C.
[0013] In the present invention, in order to successfully prepare the new material and improve its HER performance, it is necessary to solve the problem that selenium atoms on the surface of molybdenum selenide are difficult to escape from the lattice to form vacancies. In view of the difficulty in preparing the new material, the present invention innovatively finds that calcining MoSe2 under negative pressure and reducing atmosphere and controlling the calcination temperature can unexpectedly achieve synergy, construct selenium vacancy defects on the surface of MoSe2, improve active sites and electron transport capacity, and thus significantly improve the HER catalytic performance of the material.
[0014] In the present invention, the calcination conditions, i.e., the combined control of negative pressure, reducing atmosphere and temperature, are the key to the synergistic preparation of the new material and the improvement of its HER performance.
[0015] The initial MoSe2 of the present invention may be a commercial product or prepared based on an existing method. For example, it may be prepared based on a hydrothermal method. For example, in the present invention, the MoSe2 is obtained by hydrothermal reaction of an aqueous solution containing a molybdenum source, a selenium source, a reducing agent, and a carrier;
[0016] Preferably, the molybdenum source is at least one of molybdates including ammonium molybdate;
[0017] Preferably, the selenium source is at least one of elemental selenium and selenate;
[0018] Preferably, the molar ratio of Mo / Se in the molybdenum source and the selenium source is 1:2 to 2.2; preferably a stoichiometric ratio.
[0019] The present invention has no special requirements on the type of reducing agent. For example, the reducing agent is at least one of hydrazine hydrate and sodium borohydride; the amount thereof preferably exceeds the theoretical amount, and further preferably, the molar ratio of the selenium source to the reducing agent is 1:10-60.
[0020] In the present invention, there is no particular requirement for the type of carrier, for example, the carrier is a carbon carrier;
[0021] Preferably, the temperature of the hydrothermal reaction is greater than or equal to 180°C, more preferably 180-220°C;
[0022] Preferably, there is no particular requirement for the hydrothermal time, for example, 10 to 15 hours.
[0023] In the present invention, MoSe2 can be directly subjected to subsequent calcination treatment, or it can be pre-calcined in a protective atmosphere and then subjected to subsequent calcination treatment. The present invention has found that the pre-calcination helps to crystallize the material MoSe2, which helps to further cooperate with the subsequent calcination process and further improve the HER performance of the prepared material.
[0024] Preferably, the pre-baking temperature is 650-750°C;
[0025] Preferably, the pre-calcination time is 0.5 to 5 hours.
[0026] In the present invention, the combined control of the calcination conditions of MoSe2, such as negative pressure, reducing atmosphere, and temperature, helps to synergistically construct surface selenium vacancies, helps to regulate the microstructure, and helps to further synergistically improve the HER performance of the material.
[0027] In the present invention, during the calcination process, the reducing atmosphere is a hydrogen-containing atmosphere;
[0028] Preferably, the reducing atmosphere is at least one of hydrogen, a hydrogen-nitrogen mixture, and a hydrogen-inert gas mixture;
[0029] Preferably, the volume content of hydrogen in the reducing atmosphere is 10 to 100%, more preferably 5 to 15%;
[0030] Preferably, the negative pressure during the roasting stage is less than or equal to 250 Pa;
[0031] Preferably, the calcination temperature is 680-720° C. In the present invention, at this preferred temperature, it is helpful to further synergistically improve the HER performance of the prepared material.
[0032] In the present invention, there is no particular requirement for the rate of heating to the calcination temperature, which may be, for example, 1 to 20° C. / min, preferably 5 to 15° C. / min.
[0033] Preferably, the holding time at the roasting temperature is 0.5 to 5 hours, and more preferably 1 to 2 hours.
[0034] The present invention also provides an application of the selenium vacancy molybdenum selenide material as a HER catalyst.
[0035] In the present invention, the selenium vacancy molybdenum selenide material can be used to prepare the required HER catalytic device based on existing means. For example, it can be used as a HER catalyst for electrolysis of water to produce hydrogen.
[0036] The present invention also provides a HER catalytic electrode, which comprises the selenium vacancy molybdenum selenide material of the present invention.
[0037] In the present invention, the HER catalytic electrode, except for the active material added with the selenium vacancy molybdenum selenide material of the present invention, other auxiliary materials and structural components can be well-known.
[0038] The present invention also provides a method for producing hydrogen by electrolysis of water, which comprises the HER catalytic electrode. Similarly, the method for producing hydrogen by electrolysis of water described in the present invention, in addition to the active material containing the selenium vacancy molybdenum selenide material described in the present invention, can have other materials and structures that are well known.
[0039] Beneficial Effects
[0040] 1. The present invention provides a new molybdenum selenide material with surface selenium vacancies, which has abundant electroactive sites and fast charge transfer capability, exhibits low overpotential and Tafel slope in both alkaline and acidic media, and can exhibit excellent HER catalytic activity.
[0041] 2. In order to overcome the problem that surface selenium atoms are difficult to escape from the lattice and form suitable vacancies in the preparation of molybdenum selenide with selenium vacancies, the present invention innovatively bakes MoSe2 under negative pressure and reducing atmosphere, and controls the baking temperature, which can unexpectedly achieve synergy, construct selenium vacancy defects on the MoSe2 surface, improve active sites and electron transport capabilities, and thus significantly improve the HER catalytic performance of the material.
[0042] 3. The hydrothermal method is further used in combination with pre-calcination to obtain MoSe2, and then combined with the calcination treatment under the negative pressure and reducing atmosphere, the HER performance of the material can be further synergistically improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 MoSe2-Se prepared in step 2 of Example 1 v And the MoSe2 prepared by pre-calcination in step 1 of Example 2, and the MoSe2-A-Se prepared in step 2 vHER performance of the material in 1M KOH electrolyte. (a) Polarization curve; (b) Tafel slope diagram; (c) Impedance Nyquist diagram and equivalent circuit diagram when η=173mV; (d) Exchange current density (j0).
[0044] Figure 2 MoSe2-Se prepared in step 2 of Example 1 v And the MoSe2 prepared by pre-calcination in step 1 of Example 2, and the MoSe2-A-Se prepared in step 2 v HER performance of the material in 0.5M H2SO4 electrolyte. (a) Polarization curve; (b) Tafel slope diagram; (c) Nyquist curve and equivalent circuit diagram when η=158mV; (d) Exchange current density (j0).
[0045] Figure 3 MoSe2-Se prepared in Example 1 v XRD patterns of the materials.
[0046] Figure 4 Polarization curves and Tafel slopes of the materials prepared in Comparative Example 1 and Example 2, where (a, b) are polarization curves and Tafel slopes in 1M KOH electrolyte; (c, d) are polarization curves and Tafel slopes in 0.5M H2SO4 electrolyte. DETAILED DESCRIPTION
[0047] Example 1
[0048] Step (1): Preparation of initial molybdenum selenide (MoSe2)
[0049] A 2 cm × 5 cm piece of carbon cloth (CC) was ultrasonically treated with acetone, deionized water and ethanol for 20 minutes each to remove surface impurities and then dried for later use. 0.316 g of selenium powder was dispersed in 10 mL of N2H4·H2O and ultrasonically treated for 5 min to obtain a Se mixed solution. At the same time, (NH4)6Mo7O 24 ·4H2O was dispersed in 30mL deionized water and ultrasonically treated for 5min to obtain a Mo mixed solution. Then, the Mo mixed solution was added dropwise to the Se mixed solution at a Mo / Se molar ratio of 1:2 during stirring to obtain a Mo / Se mixed solution. Then, the pretreated CC and the Mo / Se mixed solution were transferred to a 70mL polytetrafluoroethylene reactor and maintained at 200℃ for 12 hours. Then, the CC with MoSe2 grown was rinsed with deionized water and ethanol several times and dried at room temperature to obtain the initial MoSe2.
[0050] Step (2): Molybdenum selenide (MoSe2-Se v ) Preparation of electrocatalysts
[0051] The initial MoSe2 obtained in step (1) was calcined in a hydrogen (H2) (10% H2 and 90% Ar) atmosphere at 700°C for 1 hour at a heating rate of 10°C / min while maintaining a vacuum state (pressure P is less than or equal to 250 Pa), and then cooled to room temperature to obtain MoSe2-Se v .
[0052] Example 2
[0053] Compared with Example 1, the only difference is that a protective atmosphere calcination crystallization step is added after step (1), as follows:
[0054] The initial MoSe2 carbon cloth obtained by hydrothermal heating was calcined at 700°C in a high-purity argon (Ar) atmosphere for 1 hour at a heating rate of 10°C / min, and then cooled to room temperature to obtain a crystalline MoSe2 sample, i.e. Figure 1 and Figure 2 MoSe2 as described in.
[0055] Compared with Example 1, the second difference is that the initial MoSe2 calcined under negative pressure and reducing atmosphere in step (2) is replaced with the crystalline MoSe2 of Example 2, and the obtained sample is Figure 1 and Figure 2 MoSe2-A-Se v .
[0056] like Figure 1 and Figure 2 As shown, the HER performance of the samples obtained under negative pressure and reducing atmosphere of initial MoSe2 and crystalline MoSe2 is almost the same, indicating that selenium vacancies are also formed in crystalline MoSe2 under negative pressure and reducing atmosphere, and also indicating that the source of molybdenum selenide does not affect the formation of selenium vacancies.
[0057] In order to determine the effect of Se vacancies on HER performance, MoSe2 (the sample prepared in step 1 of Example 2. In order to eliminate the influence of temperature in step 2 of Example 1, it is necessary to compare with the sample prepared in step 1 of Example 2) and MoSe2-Se v The HER performance of the sample (prepared in step 2 of Example 1) was tested. Figure 1 a is MoSe2 and MoSe2-Se v The polarization curve (after iR compensation) is shown in Figure 2. When the current density is 10 mA cm -2 When the overpotential of MoSe2 is 196mV, while that of MoSe2-Se vThe overpotential of the 2000 nanostructured carbon nanotubes is only 165 mV, which is 31 mV lower than that of MoSe2. -2 When the overpotential of MoSe2 is even higher than that of MoSe2-Se v The result shows that the formation of Se vacancies increases the number of active sites, thereby improving the HER performance of the electrocatalyst. In addition, the present invention also calculates the Tafel slope ( Figure 1 b) and test Nyquist curve ( Figure 1 c) to explore the effect of Se vacancies on the HER reaction kinetics. As we all know, the smaller the Tafel slope value, the smaller the overpotential increase when the same current density is increased, the lower the energy consumption required, which means the faster the charge transfer rate. Figure 1 As shown in b, the Tafel slope of MoSe2 is 116 mV dec -1 , while MoSe2-Se v Shows a smaller Tafel slope of 81mV dec -1 This shows that MoSe2-Se v With faster reaction kinetics, it has better HER performance. Figure 1 c is MoSe2 and MoSe2-Se v The Nyquist curve of MoSe2-Se v It shows a smaller semicircle diameter than MoSe2, indicating that MoSe2-Se v The smaller charge transfer resistance than MoSe2 further proves that the presence of Se vacancies increases the density of active sites and accelerates the HER reaction rate. Finally, the Tafel slope of MoSe2 and MoSe2-Se v The exchange current density (j0) of Se vacancies is used to study the effect of the presence of Se vacancies on the intrinsic HER activity. The larger the j0, the stronger the ability of HER to gain or lose electrons, and the easier the HER reaction is. Figure 1 As shown in d, MoSe2-Se v (0.21mA cm -2 ) than MoSe2 (0.15 mA cm -2 ) has a larger exchange current density, indicating that MoSe2-Se v The intrinsic HER activity of the catalyst is higher.
[0058] In addition, MoSe2 and MoSe2-Se were also tested in 0.5M H2SO4. v HER performance, such as Figure 2At a current density of 10 mA cm -2 When MoSe2 and MoSe2-Se v The overpotentials of MoSe2-Se v The overpotential of MoSe2 is 70mV lower than that of MoSe2. v The Tafel slopes are 117 mV dec -1 and 69mVdec -1 According to the Nyquist curve, it can be seen that MoSe2-Se v It has a smaller semicircular diameter than MoSe2, that is, MoSe2-Se v It has a smaller charge transfer resistance. In addition, MoSe2-Se v (0.093mA cm -2 ) than MoSe2 (0.056 mA cm -2 ) has a larger exchange current density. In summary, MoSe2-Se v It exhibits good HER performance in both acidic and alkaline media.
[0059] In order to explore the MoSe2-Se v The crystal form of MoSe2-Se v Perform X-ray diffraction (XRD), such as Figure 3 As shown, the synthesized MoSe2-Se v It is a hexagonal crystal system (JCPDS no.17-0887).
[0060] Comparative Example 1
[0061] Compared with Example 2, the only difference is that in step (2), the calcination treatment is not performed under vacuum. That is, during the calcination treatment, the pressure P is 1 atm (standard atmospheric pressure), and the other operations and parameters are the same as those in Example 2. The product finally prepared in step (2) is marked as (MoSe2-H non-vacuum).
[0062] The polarization curves and Tafel slopes of the prepared materials are shown in Figure 4 .Note Figure 4 In the embodiment, MoSe2 is the product prepared in step (1) of Example 2. v - Vacuum is the product prepared in step (2) of Example 2.
[0063] The results show that no surface selenium vacancies are formed, the overpotential is similar to that of MoSe2 (prepared in step (1)) in Example 2, and the HER performance is not ideal.
Claims
1. A method for preparing a selenium vacancy molybdenum selenide material, characterized in that: The MoSe2 is calcined under negative pressure and reducing atmosphere to obtain the selenium vacancy molybdenum selenide material; The temperature of the roasting stage is 650-750° C., and the negative pressure of the roasting stage is less than or equal to 250 Pa.
2. The method for preparing the selenium vacancy molybdenum selenide material according to claim 1, characterized in that: The selenium vacancy molybdenum selenide material comprises a hexagonal phase molybdenum selenide core and a selenium vacancy rough surface shell composited thereon, forming a core-shell structure.
3. The method for preparing the selenium vacancy molybdenum selenide material according to claim 1, characterized in that: The MoSe2 is obtained by hydrothermal reaction of an aqueous solution containing a molybdenum source, a selenium source, a reducing agent and a carrier.
4. The method for preparing the selenium vacancy molybdenum selenide material according to claim 3, characterized in that: The molybdenum source is at least one of molybdates including ammonium molybdate.
5. The method for preparing the selenium vacancy molybdenum selenide material according to claim 3, characterized in that: The selenium source is at least one of elemental selenium and selenate.
6. The method for preparing the selenium vacancy molybdenum selenide material according to claim 3, characterized in that: The molar ratio of Mo / Se elements in the molybdenum source and the selenium source is 1:2~2.
2.
7. The method for preparing the selenium vacancy molybdenum selenide material according to claim 3, characterized in that: The reducing agent is at least one of hydrazine hydrate and sodium borohydride.
8. The method for preparing the selenium vacancy molybdenum selenide material according to claim 3, characterized in that: The carrier is a carbon carrier.
9. The method for preparing the selenium vacancy molybdenum selenide material according to claim 3, characterized in that: The temperature of the hydrothermal reaction is greater than or equal to 180°C.
10. The method for preparing the selenium vacancy molybdenum selenide material according to any one of claims 3 to 9, characterized in that: MoSe2 is directly subjected to subsequent calcination treatment, or it is pre-calcined in a protective atmosphere and then subjected to subsequent calcination treatment.
11. The method for preparing the selenium vacancy molybdenum selenide material according to claim 10, characterized in that: The pre-calcination temperature is 650~750℃.
12. The method for preparing the selenium vacancy molybdenum selenide material according to claim 10, characterized in that: The pre-calcination time is 0.5~5h.
13. The method for preparing the selenium vacancy molybdenum selenide material according to any one of claims 1 or 3 to 9, characterized in that: During the calcination process, the reducing atmosphere is a hydrogen-containing atmosphere and is maintained at a negative pressure.
14. The method for preparing the selenium vacancy molybdenum selenide material according to any one of claims 1 or 3 to 9, characterized in that: The reducing atmosphere is at least one of hydrogen, a hydrogen-nitrogen mixed gas, and a hydrogen-inert gas mixed gas.
15. The method for preparing the selenium vacancy molybdenum selenide material according to any one of claims 1 or 3 to 9, characterized in that: In the reducing atmosphere, the volume content of hydrogen is 10-100%.
16. The method for preparing the selenium vacancy molybdenum selenide material according to any one of claims 1 or 3 to 9, characterized in that: The calcination temperature is 680~720℃.
17. The method for preparing the selenium vacancy molybdenum selenide material according to any one of claims 1 or 3 to 9, characterized in that: The holding time for calcination is 0.5~5h.
18. Use of the selenium vacancy molybdenum selenide material prepared by the method for preparing the selenium vacancy molybdenum selenide material according to any one of claims 1 or 3 to 9, characterized in that: It is used as a HER catalyst.
19. The use according to claim 18, characterized in that It is used as a HER catalyst for hydrogen production by water electrolysis.
20. A HER catalytic electrode, characterized in that: A selenium vacancy molybdenum selenide material prepared by the method for preparing a selenium vacancy molybdenum selenide material according to any one of claims 1 to 9.
21. A method for producing hydrogen by electrolysis of water, characterized in that: The HER catalytic electrode according to claim 20 is used to electrolyze water to produce hydrogen.