A material with highly conductive functional groups heterogeneously connected at zinc grain boundaries and a preparation method thereof

The preparation of heterogeneous connecting materials of high-conductivity functional groups at zinc grain boundaries through ball milling-high-speed heating curing method, solving the problems of zinc dendrites growth and negative electrode surface corrosion in zinc ion batteries, and achieving high stability and high conductivity Zinc-carbon composite material simplifies the preparation process and reduces costs.

CN116014093BActive Publication Date: 2024-11-08TIANJIN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211636312.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-15
Publication Date
2024-11-08
Estimated Expiration
2042-12-15

AI Technical Summary

Technical Problem

During the circulation process of existing zinc ion batteries, there are problems such as short circuit, negative electrode surface corrosion and passivation, resulting in low cycle performance attenuation and metal utilization, and the preparation process of three-dimensional structure zinc-carbon negative electrode composite materials is long and The cost is high and the carbon material bonding power is weak, which affects the stability of the battery.

Method used

The ball mill-high-speed heating curing method is used to prepare heterogeneous connecting materials of high-conductivity functional groups at zinc grain boundaries. The high-conductive carbon material forms a uniformly wound and interlaced strip-shaped conductive network and connects it to zinc particles to form a complete and uniform bridge structure. Ball milling and high-speed heating and curing processes realize the short process preparation of carbon-zinc composite materials, solving the problem of poor binding effect of carbon materials.

Benefits of technology

The composite materials at zinc grain boundaries with high cycle stability and high conductivity are achieved, which simplifies the preparation process, reduces production costs, can be produced on a large scale, and effectively suppresses the side reactions of zinc metal grain boundaries, and improves the reversibility of zinc. Deposition and peel properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116014093B_ABST
    Figure CN116014093B_ABST
Patent Text Reader

Abstract

The invention discloses a material with highly conductive functional groups heterogeneously connected at zinc grain boundaries and a preparation method thereof; a multidimensional zinc metal and highly conductive carbon nanotube composite material formed by ball milling-high-speed heating curing method. At the same time, the conductive carbon nanotubes are mutually bridged to form a conductive network. In the prepared composite material, the highly conductive carbon material aggregates at the boundary of the zinc grain boundary to form a band-shaped conductive network, which is evenly intertwined and staggered. The method has a simple preparation process, controllable process, good stability, can be mass-produced, and is suitable for large-scale preparation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of battery materials, and relates to a heterogeneously connected composite material and a preparation method thereof, and in particular to a highly stable heterogeneously connected material with highly conductive functional groups at zinc grain boundaries and a preparation method thereof. Background Art

[0002] The successive exhaustion of traditional fossil energy and the growing demand for energy will promote the efficient use of clean energy such as solar energy and wind energy and the transformation and upgrading of the energy structure. However, the application of these natural renewable energy sources is easily affected by geographical conditions, climate and natural environment, and has the characteristics of intermittent and random, and it is always difficult to directly integrate them into the existing power grid. The use of large-scale battery stack energy storage technology can effectively store intermittent wind / photovoltaic energy and effectively smooth the power generation output. At present, large-scale electrochemical energy storage is mainly based on lithium batteries and lead-acid batteries, but due to the insecurity and high price of lithium and the poor cycle stability and high toxicity of lead-acid batteries, it is difficult to meet the needs of large-scale energy storage. Therefore, the development of high-safety, high-stability, low-cost and environmentally friendly batteries remains the focus of future battery research.

[0003] Aqueous zinc-ion battery energy storage technology has attracted widespread attention from the society. Its main advantages are: 1. It has a theoretical high capacity (820mAh g -1 ); 2. It has a low oxidation / reduction potential (-0.762V) and can adapt to a variety of multivalent oxides for redox reactions; 3. Zinc can exist stably in air and water and has high safety; 4. It is rich in resources. This series of advantages makes aqueous zinc-ion batteries one of the most promising and valuable large-scale battery stack energy storage technologies. However, there are still some problems in the actual use of zinc ions. For example, zinc dendrites growing during the cycle will pierce the diaphragm and cause the battery to short-circuit, resulting in serious attenuation of the battery cycle performance; side reactions such as corrosion and passivation on the negative electrode surface will seriously reduce the metal utilization rate and cycle life, which will affect the overall electrochemical performance of the battery. At present, the modification methods for the above problems are mainly to perform surface modification at the zinc negative electrode-electrolyte interface. For example, Zhao et al. constructed an ultra-thin TiO2 coating on the surface of zinc foil to effectively avoid direct exposure of zinc metal to the electrolyte, thereby inhibiting the growth of dendrites during zinc deposition (AdvMater Interfaces, 2018, 5: 1800848). Wan et al. added Na-containing + Ionic additives effectively promote the uniform deposition of zinc ions through the electrostatic shielding effect (Nat Commun, 2018, 9: 1656). However, such measures can only effectively improve the surface utilization rate, and still have hidden dangers such as coating peeling and additive failure under high current charging and discharging.

[0004] Constructing a three-dimensional zinc negative electrode on a carbon substrate through bulk design is one of the effective strategies to solve the low surface utilization and poor deep charge and discharge performance. Carbon can not only ensure rapid electron transfer, reduce the zinc nucleation overpotential, and achieve highly reversible and uniform zinc deposition and stripping; it can also provide guidance for Zn 2+ Ion channels of the migration path. At present, in the preparation of three-dimensional structured zinc-carbon negative electrode composite materials, the array framework is mainly constructed in situ by the calcination template method, or zinc metal is electrodeposited on a porous carbon substrate. However, such methods not only have a long implementation cycle, but also require a large amount of energy (such as heat energy and electrical energy) consumption, which will lead to excessively high production costs and cannot be mass-produced on a large scale. Moreover, due to the weak bonding force of physically bonded carbon materials, the materials are unevenly composited during the sintering and deposition process, resulting in severe carbon aggregation or poor structural stability, which greatly affects the battery cycle stability. Summary of the invention

[0005] In view of the deficiencies in the above-mentioned prior art, the purpose of the present invention is to provide a highly stable heterogeneously connected material with highly conductive functional groups at zinc grain boundaries and a preparation method based on a short process of ball milling-high-speed heating solidification, which effectively solves the problems of long preparation process and weak carbon binding ability of three-dimensional structured carbon-zinc negative electrodes. The prepared composite material has high cycle stability and high conductivity and has extremely high practical value.

[0006] The purpose of the present invention is achieved through the following technical solutions:

[0007] The invention relates to a material with highly conductive functional groups heterogeneously connected at zinc grain boundaries, wherein highly conductive carbon materials in the material form a uniformly intertwined and staggered band-shaped conductive network, and aggregates at the boundaries of zinc grain boundaries are connected to form a complete and uniform bridging structure.

[0008] As an embodiment, the highly conductive carbon material is a nanocarbon material with a conjugated carbon skeleton, such as a composite carbon material containing a linear carbon material with a high aspect ratio and one or more combinations of graphene, graphene oxide, acetylene black, and carbon black; the linear carbon material with a high aspect ratio is a carbon nanotube or a carbon fiber.

[0009] As an embodiment, the zinc particles include one or more of zinc powder, zinc paste, zinc oxide powder, and basic zinc carbonate; preferably zinc powder and zinc paste.

[0010] The invention also relates to a method for preparing a material with highly conductive functional groups heterogeneously connected at zinc grain boundaries, which is prepared by a ball milling-high-speed heating and curing process.

[0011] Among them, the ball milling is to transfer the mixture of zinc powder, high-conductivity carbon material and process control agent into a high-speed ball mill, and perform variable speed ball milling in steps or multiple times to obtain a highly uniformly mixed carbon material mixed zinc powder material; the high-speed heating and curing is to put the obtained carbon material mixed zinc powder material into a mold; place it in a plasma machine for rapid temperature rise treatment, and use axial force and pulse current to achieve high-speed heating and curing treatment of the carbon material mixed zinc powder material to form a carbon-metal zinc bulk material with uniform and controllable size and thickness. In terms of process, the present invention realizes the short-process preparation of carbon-zinc composite materials through the technology of ball milling-high-speed heating and curing. At the same time, in terms of structure, not only the physical and mechanical properties of the material are lost little, but also the problem of poor physical bonding effect of carbon is effectively solved, and the bulk phase of porous carbon material and metal zinc is uniformly mixed. In addition, the band-shaped conductive network formed by the aggregates of the zinc particle grain boundary effectively inhibits the side reactions of the zinc metal grain boundary, which is conducive to the reversible deposition and stripping of zinc.

[0012] As an embodiment, the method for preparing the material with highly conductive functional groups heterogeneously connected at zinc grain boundaries comprises the following steps:

[0013] S1. Pretreatment: Place the highly conductive carbon material and process control agent under low oxygen environment protection, add anhydrous solvent, and mix with powdered zinc material.

[0014] S2, ball milling: transferring the mixed material obtained in step S1 into a high-speed ball mill, and performing variable speed ball milling to obtain a highly uniformly mixed carbon material mixed with zinc powder material;

[0015] S3, high-speed heating and curing: putting the carbon material mixed with zinc powder obtained in S2 into a mold; performing rapid temperature treatment in a plasma machine, and using axial force and pulse current to achieve high-speed heating and curing of the above powder.

[0016] In step S1, since the highly conductive carbon material (carbon material aggregate) is light in texture and low in density, it is easy to suspend in the air and is not convenient for direct ball milling, which makes it difficult to mix it evenly with the metal powder. The addition of the process control agent will reduce the accumulation and agglomeration of the powder during the ball milling process, so that the metal zinc powder and the light carbon material aggregate are mixed evenly, and the powder yield is improved.

[0017] In step S3, high-speed heating and curing is to use axial force and pulse current to realize rapid curing of the above powder by flattening the carbon material metal zinc mixture at 20-75MPa. In the rapid sintering state, the zinc powder material generates a large number of directionally drifting free electrons, which are combined with the electrons of the lightweight carbon material aggregates, and the zinc is heterogeneously bridged with the high-conductivity functional groups at the zinc grain boundaries, and a high-conductivity and high-stability bulk composite material is quickly formed, which is heterogeneously bridged with the high-conductivity functional groups at the zinc grain boundaries.

[0018] As an embodiment, in step S1, the anhydrous solvent is one or more of anhydrous toluene, anhydrous methanol, anhydrous ethanol, anhydrous N,N-dimethylformamide, anhydrous dichloromethane, anhydrous acetone, anhydrous carbon tetrachloride, and anhydrous n-hexane. Preferably, the mass: volume ratio of the added zinc metal powder material: anhydrous solvent is 3:1 to 15:1.

[0019] As an embodiment, in step S1, the process control agent is one or more of stearic acid, sodium stearate, and titanate. If the amount of process control agent added is too little, it will lead to insufficient grinding; if the amount of process control agent added is too much, it will lead to more impurities in the carbon-zinc powder material, which is not conducive to subsequent sintering and curing. Therefore, the preferred mass ratio of the process control agent to the zinc-carbon mixed material is 1:15 to 1:45.

[0020] As an embodiment, in step S1, the hypoxic environment is a dry hypoxic environment with water and oxygen contents both lower than 1 ppm. Since the metal zinc powder is easy to absorb moisture, it needs to be protected in a dry hypoxic environment with water and oxygen contents both lower than 1 ppm.

[0021] As an embodiment, the content of highly conductive carbon material in the obtained zinc-carbon mixture will play an important role in the electrochemical performance of the composite material. If the mass is too low, it will not be able to play the role of improving conductivity; if the mass is high, not only the performance improvement effect tends to be saturated, but also the material of the subsequent sintering molding is brittle and soft, which is not conducive to storage and practical use. Therefore, the mass percentage content of highly conductive carbon material in the carbon material mixed zinc powder material obtained in step S2 is preferably 2 to 10wt%.

[0022] As an embodiment, in step S2, ball milling is performed in batches or continuously. Wet ball milling can make the lightweight carbon material and zinc powder material more evenly mixed, stably contact the surface and compound. If the ball milling speed is too low or the time is too short, it is easy to make the two-phase material mixed unevenly; if the dry ball milling speed is too high or the time is too long, it will waste energy and have low efficiency. Therefore, the speed is controlled at 100-1600r / min, the time is 10-60min, the material temperature is 20-90°C, and the ball-to-material ratio is controlled at 10:1-20:1. The preferred speed is 400-1600r / min, the ball-to-material ratio is 10:1, and the temperature is 35°C.

[0023] As an embodiment, in step S3, the scale mold is one or more of a cylindrical and a cubic type. The diameter of the cylindrical mold is 1 to 5 cm and the height is 0.3 to 2 cm. A mold with a diameter of 1 cm and a height of 0.5 cm is preferably used as a container for loading the ball-milled powder, and the flattening pressure is preferably 8 MPa.

[0024] As an embodiment, in step S3, the heating rate is 50°C / min.

[0025] As an embodiment, in step S3, the high-speed heating curing (plasma sintering) temperature is 200-700°C, the holding time is 5-30 minutes, and the axial force pressure is 20-75 MPa.

[0026] As an embodiment, starting from the pretreatment, the subsequent processes are all carried out in a dry low-oxygen environment with water and oxygen contents below 1 ppm, otherwise it is easy to cause oxidation of metallic zinc.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] 1) The ball milling-high-speed heating curing process adopted in the present invention is used to prepare a highly stable material with highly conductive functional groups heterogeneously connected at the zinc grain boundary. The method is simple, the process is stable, and the preparation process is short. It can realize a uniform composite material of carbon material and metallic zinc in a mild and dry environment, and can be used for large-scale production;

[0029] 2) In the composite material produced, the highly conductive carbon material forms a band-shaped conductive network at the grain boundary of zinc particles, which is evenly intertwined and staggered; the special bridging structure effectively inhibits the side reaction of the zinc metal grain boundary, which is conducive to the reversible deposition and stripping of zinc;

[0030] 3) The heterogeneously connected materials with highly conductive functional groups at the zinc grain boundaries produced have excellent conductivity and structural stability. They are highly stable functional materials required for aqueous zinc-based batteries and are expected to be used on a large scale in the energy field.

[0031] 4) In the heterogeneous composite material synthesized in the present invention, it is not a simple composite at the physical level. In the heating and curing process, due to the strong electric field force provided by the plasma machine, the interface of the conductive carbon material and the metal zinc is connected through the grain boundary to form a strong bond. Among them, the highly conductive carbon material plays the role of "electronic bridge" at the zinc-zinc interface, ensuring the rapid transfer of electrons, regulating the electric field in the zinc body phase, and increasing the stability of the material in the electrochemical cycle. The zinc-carbon composite material obtained by the vacuum hot pressing sintering process, for example, only uses high temperature and high pressure to shape the powder into a block material, and cannot form this kind of heterogeneous special structure at the zinc grain boundary. In addition, since the temperature and pressure required by the vacuum hot pressing sintering process are much higher than the rapid heating and curing method used in the present invention, the particle size of the internal zinc grains is large, and the interior is too dense, resulting in uneven deposition-peeling of zinc on the block surface during the battery cycle, resulting in the growth of zinc dendrites and the aggravation of uneven deposition, affecting the electrochemical performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0033] Figure 1 This is a process flow chart of ball milling-high-speed heating curing;

[0034] Figure 2 TEM image of carbon nanotubes;

[0035] Figure 3 TEM image of highly stable zinc grain boundary with highly conductive functional groups heterogeneously connected materials (50nm);

[0036] Figure 4 TEM image of highly stable zinc grain boundary with highly conductive functional groups heterogeneously connected materials (5nm);

[0037] Figure 5 This is the XRD diagram of the highly stable material with highly conductive functional groups heterogeneously connected at the zinc grain boundary;

[0038] Figure 6 The internal resistance diagram of the material with highly conductive functional groups heterogeneously connected at the highly stable zinc grain boundary;

[0039] Figure 7 This is a symmetric battery performance diagram of a material with highly stable and highly conductive functional groups heterogeneously connected at the zinc grain boundary;

[0040] Figure 8 This is the SEM image of the material with highly conductive functional groups heterogeneously connected at the zinc grain boundary prepared by ball milling-high-speed heating solidification method after cycling;

[0041] Fig. 9 The SEM image of the zinc negative electrode material after cycling prepared by simple mixing-high-speed heating and curing method;

[0042] Fig.10 SEM image of the zinc bulk composite material after cycling, which was prepared by only ball milling and vacuum hot pressing sintering. DETAILED DESCRIPTION

[0043] The present invention is described in detail below in conjunction with embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, some adjustments and improvements can also be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.

[0044] Example 1

[0045] In this embodiment, carbon nanotubes and zinc powder are used as raw materials to prepare a highly stable material with highly conductive functional groups at zinc grain boundaries. The preparation method is a ball milling-high-speed heating curing process, such as Figure 1 As shown:

[0046] (1) Pretreatment: 0.4 g of highly conductive carbon nanotubes and 0.4 g of process control agent stearic acid were placed in a low-water and low-oxygen argon atmosphere, 3 mL of anhydrous ethanol was added, and mixed with 10 g of zinc metal powder. The microscopic size of the highly conductive carbon material is shown in FIG. Figure 2 shown.

[0047] (2) High-energy ball milling: The mixed material obtained in the previous step is transferred into a high-speed ball mill. Under sufficient argon protection, the rotation speed is maintained at 400 rpm for 1 hour, the ball-to-material ratio is 10:1, and the reaction temperature is controlled at about 35°C to obtain a highly uniformly mixed carbon material mixed with zinc powder.

[0048] (3) High-speed heating and curing: The obtained carbon material mixed with zinc powder is placed in a mold of a specific size (a cylindrical mold with a diameter of 1 cm and a height of 0.5 cm), and flattened at a pressure of 8 MPa. A rapid heating treatment is carried out in a plasma machine, wherein the heating rate is 50°C / min, the sintering temperature is 350°C, the holding time is 10 minutes, and the axial force pressure applied in the plasma machine is 50 MPa. The axial force and pulse current are used to achieve high-speed heating and curing of the above powder. A block composite material with high conductivity and high stability is formed, in which the zinc grain boundaries are connected to the heterogeneous bridges of high-conductivity functional groups.

[0049] Figure 3-Figure 8 The following are the TEM image, XRD image, internal resistance image of zinc battery, symmetric battery image and SEM image after long-term cycling of the prepared high-conductivity functional group heterogeneous connected material at the zinc grain boundary. Figure 3 and Figure 4 It can be seen that there are a large number of heterogeneously connected and intertwined carbon nanotubes between zinc-zinc particles. These carbon nanotubes play a "bridging" role between grain boundaries, reducing the internal resistance at the grain boundaries. Figure 5 It can be seen that there is only the characteristic peak of zinc in the composite material, indicating that this process can not change the structure of the material or generate other phases. Figure 6 It can be seen that compared with the battery assembled with the zinc sheet obtained by the preparation method of the present invention, the internal resistance of the zinc ion battery constructed by the composite material is significantly reduced to only about 10Ω. Figure 7 It can be seen that at 1A / cm 2 At a current density of , the composite material synthesized by the preparation method of the present invention not only has smaller polarization, but also exhibits an ultra-long cycle stability of more than 240 h. Figure 8 The electrode surface after long-term cycling is still uniform and smooth without dendrite formation.

[0050] Example 2

[0051] This embodiment uses carbon nanotubes, carbon black and zinc powder as raw materials to prepare a highly stable material with highly conductive functional groups heterogeneously connected at zinc grain boundaries, and the preparation method is a ball milling-high-speed heating and curing process.

[0052] (1) Pretreatment: 0.3 g of highly conductive carbon nanotubes, 0.3 g of carbon black and 0.3 g of process control agent stearic acid were placed in a low-water and low-oxygen argon atmosphere, 3 mL of anhydrous ethanol was added, and mixed with 10 g of zinc metal powder.

[0053] (2) High-energy ball milling: The mixed material obtained in the previous step is transferred into a high-speed ball mill. Under sufficient argon protection, the rotation speed is maintained at 600 rpm for 1 hour, the ball-to-material ratio is 10:1, and the reaction temperature is controlled at about 35°C to obtain a highly uniformly mixed carbon material mixed with zinc powder.

[0054] (3) High-speed heating and curing: The obtained carbon material mixed with zinc powder material is placed in a mold of a specific size (a cylindrical mold with a diameter of 1 cm and a height of 0.5 cm), and flattened at a pressure of 8 MPa. Rapid heating treatment is carried out in a plasma machine, wherein the heating rate is 50°C / min, the sintering temperature is 350°C, the holding time is 10 min, and the axial force pressure is 50 MPa. High-speed heating and curing of the above powder is achieved by using axial force and pulse current. A block composite material with high conductivity and high stability is formed, in which the zinc grain boundaries are connected to heterogeneous bridges of high-conductivity functional groups. The composite material synthesized by the preparation method of the present invention exhibits high cyclic stability at 1A / cm 2 The cycle time is 180h at a current density of . It also shows high conductivity, with an internal resistance of only about 15Ω.

[0055] Example 3

[0056] Carbon nanotubes and zinc oxide are used as raw materials to prepare a highly stable material with highly conductive functional groups heterogeneously connected at zinc grain boundaries, and the preparation method is a ball milling-high-speed heating solidification process.

[0057] (1) Pretreatment: 0.3 g of highly conductive carbon nanotubes and 0.2 g of process control agent stearic acid were placed in a low-water and low-oxygen argon atmosphere, 2 mL of anhydrous ethanol was added, and mixed with 8 g of zinc oxide powder.

[0058] (2) High-energy ball milling: The mixed material obtained in the previous step is transferred into a high-speed ball mill. Under sufficient argon protection, the rotation speed is maintained at 600 rpm for 1 hour, the ball-to-material ratio is 15:1, and the reaction temperature is controlled at about 35°C to obtain a highly uniformly mixed carbon material mixed with zinc powder.

[0059] (3) High-speed heating and curing: The obtained carbon material mixed with zinc powder is placed in a mold of a specific size (a cylindrical mold with a diameter of 1 cm and a height of 0.5 cm) and flattened at a pressure of 8 MPa. A rapid heating treatment is performed in a plasma machine, wherein the heating rate is 50°C / min, the sintering temperature is 450°C, the holding time is 10 minutes, and the axial force pressure is 50 MPa. The axial force and pulse current are used to achieve high-speed heating and curing of the above powder.

[0060] The composite material synthesized by the preparation method of the present invention exhibits high cycle stability, with a cycle time of 120 hours at a current density of 1 A / cm2. It also exhibits high conductivity, with an internal resistance of only about 32Ω.

[0061] Comparative Example 1

[0062] The zinc metal material is made from zinc powder without ball milling and is only heated and solidified at high speed.

[0063] High-speed heating and curing: 10g zinc powder is placed in a cylindrical mold with a specific size, 1cm in diameter and 0.5cm in height, and flattened at a pressure of 8MPa. Rapid heating treatment is carried out in a plasma machine, wherein the heating rate is 50℃ / min, the sintering temperature is 350℃, the holding time is 10min, and the axial force pressure is 50MPa. A block of metallic zinc negative electrode material is obtained.

[0064] like Figure 7 As shown in the figure, the internal resistance of the obtained zinc material was not improved without carbon mixing treatment, which was 200Ω. Even at a current density of 1A / cm2, it showed a polarization voltage of nearly 50mV. And due to the large growth of zinc dendrites during the charge and discharge process, the battery had a short circuit at 40h.

[0065] Comparative Example 2

[0066] The zinc-carbon composite negative electrode material is made from zinc powder and carbon nanotubes, through a simple mixing process and then rapid heating and curing.

[0067] (1) 0.4 g of highly conductive carbon nanotubes and 10 g of zinc powder were mixed by simple mechanical grinding in an argon atmosphere for 30 min.

[0068] (2) High-speed heating and curing: Zinc powder is placed in a mold of a specific size, such as a cylindrical mold with a diameter of 1 cm and a height of 0.5 cm, and flattened at a pressure of 8 MPa. Rapid heating treatment is performed in a plasma machine, wherein the heating rate is 50°C / min, the sintering temperature is 350°C, the insulation time is 10 min, and the pressure is 50 MPa. A zinc-carbon composite negative electrode material is obtained.

[0069] The internal resistance of this comparative example is 187Ω. Although the addition of conductive carbon material reduces the internal resistance of the battery, the effect is not significant. Moreover, at 1A / cm 2 At a current density of , the cycle life is only 46h. By performing SEM tests on the electrodes after the cycle, Fig. 9 Under short-term charge and discharge, a large number of dendrites are formed at the electrode-electrolyte interface, which shows that the simple mixed composite material cannot effectively deposit zinc ions evenly, resulting in a micro short circuit in the battery.

[0070] Comparative Example 3

[0071] The block composite material is prepared by using zinc powder and carbon nanotubes as raw materials, without high-speed heating curing, but only by ball milling and vacuum hot pressing curing.

[0072] (1) Pretreatment: 0.4 g of highly conductive carbon nanotubes and 0.4 g of process control agent stearic acid were placed in a low-water and low-oxygen argon atmosphere, 3 mL of anhydrous ethanol was added, and mixed with 10 g of zinc metal powder.

[0073] (2) High-energy ball milling: The mixed material obtained in the previous step is transferred into a high-speed ball mill. Under sufficient argon protection, the rotation speed is maintained at 600 rpm for 1 hour, the ball-to-material ratio is 10:1, and the reaction temperature is controlled at about 35°C to obtain a highly uniformly mixed carbon material mixed with zinc powder.

[0074] (3) Vacuum hot pressing curing: The obtained carbon-zinc mixed material is placed in a vacuum hot pressing sintering mold and hot pressed in a vacuum hot pressing furnace. The pressing pressure is 180 MPa, the sintering temperature is 550°C, and the sintering time is 600 min to obtain a carbon nanotube and zinc block composite material.

[0075] The internal resistance of this comparative example is 193Ω. 2 At a current density of , the cycle life is only 38h. By performing SEM tests on the electrodes after the cycle, Fig.10 Obtained. Under short-term charge and discharge, it was found that the electrode-electrolyte interface was uneven, causing a micro-short circuit in the battery. This is because the zinc-carbon composite material that has not been treated with high-speed heating and curing cannot form a heterogeneous structure with the conductive functional group at the zinc grain boundary, and cannot improve key properties such as conductivity and cycle stability. Moreover, under the high-pressure and high-temperature treatment of vacuum hot pressing technology, the interior of the block is too dense, and the uneven deposition / stripping of zinc ions is easy to exist on the surface of the block during the charge and discharge process, resulting in the aggravation of zinc dendrite growth and uneven deposition, which reduces its cycle stability.

[0076] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A material with highly conductive functional groups heterogeneously connected at zinc grain boundaries, characterized in that: The highly conductive carbon material in the material forms a uniformly intertwined and interlaced band-shaped conductive network, which is connected at the boundary aggregates of each zinc particle grain boundary to form a complete and uniform bridge structure; the highly conductive carbon material is a nano-carbon material with a conjugated carbon skeleton; the highly conductive carbon material is a linear carbon material with an aspect ratio, or a composite carbon material composed of a linear carbon material with an aspect ratio and one or more of graphene, graphene oxide, acetylene black, and carbon black; the linear carbon material with an aspect ratio is a carbon nanotube or a carbon fiber; The zinc grain boundary highly conductive functional group heterogeneous connected material is prepared by a method comprising the following steps: S1. Pretreatment: placing the highly conductive carbon material and the process control agent under low oxygen environment protection, adding anhydrous solvent, and mixing with the powdered zinc material; the process control agent is one or more of stearic acid, sodium stearate, and titanate; S2, ball milling: transferring the mixed material obtained in step S1 into a high-speed ball mill, and performing variable speed ball milling to obtain a carbon material mixed with zinc powder material; the mass percentage content of the high-conductivity carbon material in the carbon material mixed with zinc powder material is 2-10 wt%; S3, high-speed heating and curing: the carbon material mixed with zinc powder obtained in S2 is placed in a mold; the temperature is rapidly increased in a plasma machine, and the carbon material mixed with zinc powder is cured by high-speed heating using axial force and pulse current; the high-speed heating and curing temperature is 200-700°C, the holding time is 5-30 min, and the axial force pressure is 20-75 MPa.

2. The material of highly conductive functional groups heterogeneously connected at zinc grain boundaries according to claim 1, characterized in that: The zinc particles include one or more of zinc powder, zinc paste, zinc oxide powder, and basic zinc carbonate.

3. The material of highly conductive functional groups heterogeneously connected at zinc grain boundaries according to claim 1, characterized in that: In step S1, the anhydrous solvent is one or more of anhydrous toluene, anhydrous methanol, anhydrous ethanol, anhydrous N, N-dimethylformamide, anhydrous dichloromethane, anhydrous acetone, anhydrous carbon tetrachloride, and anhydrous n-hexane.

4. The material of highly conductive functional groups heterogeneously connected at zinc grain boundaries according to claim 1, characterized in that: In step S1, the hypoxic environment is a dry hypoxic environment with water and oxygen contents both lower than 1 ppm; in step S2, ball milling is performed in batches or continuously, with a rotation speed of 100-1600 r / min, a time of 10-60 min, and a material temperature of 20-90°C.

5. The material of highly conductive functional groups heterogeneously connected at zinc grain boundaries according to claim 1, characterized in that: In step S3, the mold is one or more of a cylindrical and a cubic shape, with a diameter of 1 to 5 cm and a height of 0.3 to 2 cm.