A modified metal organic adsorbent for precious metal recovery and its preparation method and application
Through the in-situ polymerization of zirconium salts and aromatic acid organic compounds and the loading of polyvalent porphine compounds, a modified metal-organic adsorbent is formed, which solves the problems of low adsorption rate and poor selectivity, and achieves efficient recovery and highly selective adsorption of precious metals. .
Patent Information
- Application Number
- CN202211650001.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-21
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-12-21
AI Technical Summary
Existing precious metal adsorbents have low adsorption rates and poor selectivity, making it difficult to efficiently recover precious metals.
In-situ polymerization of zirconium salts and aromatic acid organic compounds is used to form a metal-organic layer precursor, and the loading effect and stability of the adsorbent are improved by loading polyvalent porphine compounds to form a modified metal-organic adsorbent, using NH- and N - Multiple action mechanisms such as functional groups and porphyrin rings adsorb precious metal ions.
It achieves high selectivity, high adsorption rate and high adsorption capacity of precious metals, is suitable for a wide range of pH ranges and operating modes, reduces production costs, and facilitates industrial mass production.
Smart Images

Figure CN116020418B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of precious metal recovery, and relates to a modified metal organic adsorbent for precious metal recovery, a preparation method and application thereof. Background Art
[0002] Precious metals are widely used in the fields of chips, military industry, jewelry processing, etc., but their mineral reserves in nature are low and non-renewable, so their resource recovery is crucial. At present, precious metals are usually found in metallurgical wastewater and secondary resources. Common methods for recovering precious metals from wastewater include replacement, reduction precipitation, ion exchange, solvent extraction, liquid membrane and adsorption.
[0003] The replacement and reduction precipitation methods have been used earlier and more widely in the field of precious metal extraction. By adding active metal ions, precious metals can be replaced from waste liquids to achieve the purpose of separation and purification. The main disadvantages are high cost and lack of selectivity, and a large amount of active metals are required. The solvent extraction method uses the difference in solubility of metal ions in water and organic solvents (containing functional groups such as sulfur and phosphorus) to extract precious metals. The solvent extraction method is widely used but requires a large amount of organic solvents, is costly, and is complicated to operate. It is difficult to treat waste liquids with a large number of coexisting interfering metal ions.
[0004] Adsorption technology has shown great potential in the recovery of precious metal secondary resources due to its advantages such as simple operation, low operating cost, high recovery rate, and suitability for adsorption of low-concentration substances. This method is a precious metal recovery technology that uses adsorbents to selectively adsorb precious metals in secondary resource leaching solutions to achieve separation and enrichment. Commonly used adsorbents include metal-organic framework adsorbents. However, due to the tortuous channels within their three-dimensional network structure, the adsorption rate of this type of adsorbent is relatively low, resulting in a long processing time; and due to the lack of suitable active sites, metal-organic framework adsorbents also lack the ability to selectively adsorb precious metal ions. Therefore, it is very necessary to develop new adsorbents with fast adsorption rates and strong selectivity for precious metals. Summary of the invention
[0005] In view of the deficiencies of the prior art, the purpose of the present invention is to provide a modified metal organic adsorbent for precious metal recovery and a preparation method and application thereof, so as to solve the problems of low adsorption rate and poor selectivity of the current adsorbent.
[0006] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a modified metal organic adsorbent for precious metal recovery, the preparation method comprising the following steps:
[0008] (1) mixing a zirconium salt, an aromatic acid organic compound and a solvent, and reacting them to obtain a metal organic layer precursor;
[0009] (2) Mixing the metal organic layer precursor, the porphine compound and the solvent, and reacting them to obtain the modified metal organic adsorbent.
[0010] The preparation method involved in the present invention adopts low-cost production raw materials, simple process, and is convenient for industrial mass production. It first uses a solvothermal method to in-situ polymerize zirconium salts and aromatic acid organic compounds in a solvent to form a metal organic layer precursor, and then uses a loading modification method, that is, using the metal organic layer precursor as a loading substrate, and loading multi-porphine compound molecules on the surface to obtain a new type of modified metal organic adsorbent. The multi-porphine compound can be in-situ loaded on the surface of the metal organic layer precursor, effectively improving the loading effect; at the same time, active sites such as unsaturated zirconium atoms on the surface of the metal organic layer precursor can also participate in the loading reaction, further enhancing the stability of the adsorbent; and the metal organic layer precursor has a large specific surface area, which can increase the loading ratio of the multi-porphine compound, and finally increase the adsorption capacity.
[0011] The prepared modified metal organic adsorbent can adsorb precious metal ions through multiple effects such as coordination adsorption between NH- and N- functional groups contained on the surface of the adsorbent and precious metal ions, electrostatic adsorption between porphyrin rings in porphyrin compounds and precious metal ions, and reduction adsorption, and has high selectivity, high adsorption rate and high adsorption capacity for precious metals. At the same time, the modified metal organic adsorbent has flexible characteristics, which can change the fluid state on the surface of the adsorbent, thereby increasing the contact opportunity between the precious metal ions in the waste liquid and the modified metal organic adsorbent, thereby enhancing the adsorption rate. Moreover, the modified metal organic adsorbent has a wide suitable pH range, and can achieve selective and rapid adsorption of precious metal ions in the pH range of 0-9. In addition, the modified metal organic adsorbent is suitable for sequencing batch and continuous flow operation modes, and has good application prospects.
[0012] Preferably, the zirconium salt includes any one of zirconium chloride, zirconium oxychloride, zirconium nitrate or zirconium bromide, or a combination of at least two thereof.
[0013] Preferably, the aromatic acid organic compound includes any one of 1,3,5-tris(4-carboxyphenyl)benzene, 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine or 1,3,5-tris(4-carboxyphenylethynyl)benzene or a combination of at least two thereof.
[0014] Preferably, the porphine compound contains a porphyrin ring, including any one of meso-tetraphenylporphine, 5,10,15,20-tetrakis(2,6-dichlorophenyl)porphine, meso-tetrakis(4-carboxyphenyl)porphine, meso-tetrakis(isobenzoic acid)porphine, 5,10,15,20-tetrakis(4-carboxyphenyl)porphine tetramethyl ester, racemic-tetrakis(N-methyl-3-pyridyl)tetrachloroporphine, 5,10,15,20-tetrakis(4-carboxymethoxyphenyl)-21H,23H-porphine, 5-(4-methoxycarbonylphenyl)-10,15,2-triphenylporphine or 5,10,15,20-tetrakis(4-pyridyl)porphyrin, or a combination of at least two thereof.
[0015] Preferably, the molar ratio of the zirconium salt to the aromatic acid organic compound in step (1) is 1:(0.1-10), for example 1:0.5, 1:0.8, 1:1, 1:2, 1:4, 1:6, 1:8, 1:10, etc.
[0016] Preferably, the solvent in step (1) is a mixed solvent of an organic solvent, a carboxylic acid and water.
[0017] Preferably, the organic solvent includes any one of N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone, or a combination of at least two thereof.
[0018] Preferably, the carboxylic acid includes any one of formic acid, acetic acid, propionic acid or trifluoroacetic acid, or a combination of at least two thereof.
[0019] Preferably, the volume ratio of the organic solvent, carboxylic acid and water in the mixed solvent is 8:(0.1-2):(0.1-2), wherein the specific point values in (0.1-2) can be selected from 0.1, 0.3, 0.5, 0.8, 1, 1.2, 1.5, 2, etc.
[0020] Preferably, the molar volume ratio of the aromatic acid organic compound to the organic solvent is 0.1-5 mol / L, for example, 0.1 mol / L, 0.3 mol / L, 0.5 mol / L, 0.8 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, etc.
[0021] Preferably, stirring and / or ultrasonic treatment is performed before the reaction in step (1).
[0022] Preferably, the stirring speed is 100-600rpm, for example, 100rpm, 200rpm, 300rpm, 400rpm, 500rpm, 600rpm, etc.; the stirring time is 1-30min, for example, 5min, 10min, 15min, 20min, 25min, 30min, etc.
[0023] Preferably, the power of the ultrasound is 60-360 W, for example, 60 W, 100 W, 150 W, 200 W, 300 W, etc.; the time of the ultrasound is 1-30 min, for example, 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, etc.
[0024] Preferably, the reaction temperature in step (1) is 80-150°C, for example 80°C, 90°C, 100°C, 120°C, 130°C, 150°C, etc.; the reaction time is 12-72h, for example 12h, 18h, 24h, 36h, 48h, 60h, 72h, etc.
[0025] Other specific point values within the above numerical ranges can be selected and will not be described in detail here.
[0026] Preferably, after the reaction in step (1) is completed, post-treatment is performed, and the post-treatment includes: cooling the reaction solution, centrifuging, washing the precipitate, and drying.
[0027] The cooling refers to cooling to 15-35°C, such as 15°C, 20°C, 25°C, 30°C, 35°C, etc.
[0028] The washing can be exemplarily performed by washing with N,N-dimethylformamide and methanol in sequence, and the number of washing times is 2-8 times.
[0029] The drying can be carried out in the form of baking, and the drying temperature is 60-140°C, for example, 60°C, 70°C, 80°C, 100°C, 120°C, etc.; the drying time is more than 5h, for example, 5h, 6h, 7h, 8h, 9h, 10h, etc.
[0030] Other specific point values within the above numerical ranges can be selected and will not be described in detail here.
[0031] Preferably, the solvent in step (2) comprises any one of N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone, or a combination of at least two thereof.
[0032] Preferably, the concentration of the metal organic layer precursor in the solvent in step (2) is 1-10 g / L, for example, 1 g / L, 2 g / L, 3 g / L, 4 g / L, 5 g / L, 6 g / L, 7 g / L, 8 g / L, 10 g / L, etc.
[0033] Preferably, the mass ratio of the metal organic layer precursor to the porphine compound is 1:(0.3-4), for example, 1:0.3, 1:0.5, 1:1, 1:1.5, 1:2, 1:3, 1:4, etc.
[0034] Preferably, ultrasonic treatment is performed before the reaction in step (2).
[0035] Preferably, the power of the ultrasound is 60-360 W, for example, 60 W, 100 W, 150 W, 200 W, 300 W, etc.; the time of the ultrasound is 1-30 min, for example, 5 min, 10 min, 15 min, 20 min, 25 min, 30 min, etc.
[0036] Preferably, the reaction temperature in step (2) is 60-140°C, for example 60°C, 70°C, 80°C, 100°C, 120°C, etc.; the reaction time is 5-20h, for example 5h, 8h, 10h, 12h, 15h, 20h, etc.
[0037] Other specific point values within the above numerical ranges can be selected and will not be described in detail here.
[0038] Preferably, after the reaction in step (2) is completed, post-treatment is performed, and the post-treatment includes: cooling the reaction solution, centrifuging, washing the precipitate, and drying.
[0039] The cooling refers to cooling to 15-35°C, such as 15°C, 20°C, 25°C, 30°C, 35°C, etc.
[0040] The washing can be exemplarily performed by washing with N,N-dimethylformamide and acetone in sequence, and the number of washing times is 2-8 times.
[0041] The drying can be carried out in the form of baking, and the drying temperature is 60-140°C, for example, 60°C, 70°C, 80°C, 100°C, 120°C, etc.; the drying time is more than 5h, for example, 5h, 6h, 7h, 8h, 9h, 10h, etc.
[0042] Other specific point values within the above numerical ranges can be selected and will not be described in detail here.
[0043] In a second aspect, the present invention provides a modified metal organic adsorbent for precious metal recovery prepared according to the preparation method described in the first aspect.
[0044] In a third aspect, the present invention provides use of the modified metal organic adsorbent for precious metal recovery according to the second aspect in recovering precious metals.
[0045] Preferably, the modified metal organic adsorbent is used to recover precious metals from waste liquid.
[0046] Preferably, the treatment device used in the application comprises a regulating unit, an adsorption unit, a separation and recovery unit and an auxiliary monitoring unit; the regulating unit, the adsorption unit and the separation and recovery unit are connected in sequence;
[0047] The regulating unit includes an acid-base dosing pump and a regulating tank;
[0048] The adsorption unit includes a fixed bed reactor;
[0049] The separation and recovery unit includes a regulating tank, a dosing pump, a cyclone separator and a rotary kiln;
[0050] The auxiliary monitoring unit includes a water quantity detection module and a water quality monitoring module. The water quantity detection module includes an electromagnetic flowmeter, and the water quality monitoring module includes a pH detector and a precious metal online analyzer.
[0051] Preferably, the wastewater contains precious metal ions at a concentration of 1-4000 mg / L (e.g., 200 mg / L, 500 mg / L, 1000 mg / L, 2000 mg / L, 3000 mg / L, etc.), and the pH of the wastewater is in the range of 0-9 (e.g., pH=2, pH=4, pH=7, pH=9).
[0052] Preferably, the mass volume ratio of the modified metal organic adsorbent to wastewater is 0.05-200 mg / mL, for example 0.1 mg / mL, 1 mg / mL, 10 mg / mL, 50 mg / mL, 100 mg / mL, 150 mg / mL, 200 mg / mL, etc.
[0053] The precious metals involved in the present invention include gold, platinum, palladium, rhodium, iridium and the like.
[0054] Other specific point values within the above numerical ranges can be selected and will not be described in detail here.
[0055] Compared with the prior art, the present invention has the following beneficial effects:
[0056] The preparation method involved in the present invention adopts low-cost production raw materials, simple process, and is convenient for industrial mass production. The multi-porphin compound can be in-situ loaded on the surface of the metal organic layer precursor, effectively improving the loading effect; at the same time, the active sites such as unsaturated zirconium atoms on the surface of the metal organic layer precursor can also participate in the loading reaction, further enhancing the stability of the adsorbent; and the metal organic layer precursor has a large specific surface area, which can increase the loading ratio of the multi-porphin compound, and finally increase the adsorption capacity.
[0057] The prepared modified metal organic adsorbent can adsorb precious metal ions through multiple effects such as coordination adsorption between NH- and N- functional groups contained on the surface of the adsorbent and precious metal ions, electrostatic adsorption between porphyrin rings in porphyrin compounds and precious metal ions, and reduction adsorption, and has high selectivity, high adsorption rate and high adsorption capacity for precious metals. At the same time, the modified metal organic adsorbent has flexible characteristics, which can change the fluid state on the surface of the adsorbent, thereby increasing the contact opportunity between the precious metal ions in the waste liquid and the modified metal organic adsorbent, thereby enhancing the adsorption rate. Moreover, the modified metal organic adsorbent has a wide suitable pH range, and can achieve selective and rapid adsorption of precious metal ions in the pH range of 0-9. In addition, the modified metal organic adsorbent is suitable for sequencing batch and continuous flow operation modes, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0058] Figure 1 is a scanning electron microscope image of the modified metal organic adsorbent prepared in Example 1;
[0059] Figure 2 is a scanning electron microscope image of the modified metal organic adsorbent prepared in Comparative Example 1;
[0060] Figure 3 is a graph showing the gold adsorption amount of the modified metal organic adsorbent prepared in Example 1 and the metal organic layer precursor adsorbent prepared in Comparative Example 1;
[0061] Figure 4 is a statistical diagram of the competitive ion test results of the modified metal organic adsorbent prepared in Example 1;
[0062] Figure 5 is a transmission electron microscope image of gold particles distributed on the surface of the modified metal organic adsorbent obtained in Example 1 after adsorption;
[0063] Figure 6 is a graph showing the gold adsorption amount of the modified metal organic adsorbent prepared in Example 1 at different pH values;
[0064] Figure 7 The present invention is a flowchart of the application process of the modified metal organic adsorbent for efficiently adsorbing and recovering precious metals in wastewater. DETAILED DESCRIPTION
[0065] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0066] Example 1
[0067] This embodiment provides a modified metal organic adsorbent for precious metal recovery, and the preparation method is as follows:
[0068] (1) Weigh 200 mg of 1,3,5-tris(4-carboxyphenyl)benzene and 162 mg of zirconium chloride into a 100 mL polytetrafluoroethylene reactor, add 80 mL of N,N-dimethylformamide, add a magnetic rotor to stir for 15 min, then add 16 mL of formic acid and 1 mL of water;
[0069] (2) The obtained solid-liquid mixture was stirred for 15 minutes, then placed in an ultrasonic instrument for 10 minutes at a power of 180 W, heated to 120° C. and reacted for 48 hours to obtain a metal organic layer precursor mixture;
[0070] (3) The obtained metal organic layer mixed solution was centrifuged at a speed of 8000 rpm for 10 min, the supernatant was removed and the precipitate was collected; then the precipitate was washed with N,N-dimethylformamide, centrifuged again for 10 min after washing, and the supernatant was removed, and this was repeated 3 times; then the precipitate was washed with methanol, centrifuged again for 10 min after washing, and the supernatant was removed, and this was repeated 3 times; finally, the centrifuged precipitate was placed in a drying oven and dried at 100° C. for 24 h to obtain a metal organic layer precursor powder;
[0071] (4) Weigh 200 mg of the obtained metal organic layer precursor powder into a 50 mL polytetrafluoroethylene reactor, add 40 mL of N,N-dimethylformamide, add a magnetic rotor and stir for 15 min, then add 174 mg of meso-tetrakis(4-carboxyphenyl)porphine, and continue stirring for 10 min;
[0072] (5) placing the obtained solid-liquid mixture into an ultrasonic device and ultrasonicating it at a power of 240 W for 10 min, heating it to 100° C. and reacting it for 12 h to obtain a modified metal organic layer mixture;
[0073] (6) The obtained modified polymer mixture was centrifuged at a speed of 6000 rpm for 5 minutes, the supernatant was removed and the precipitate was collected; then the precipitate was washed with N,N-dimethylformamide, centrifuged again for 5 minutes after washing, and the supernatant was removed, and this process was repeated 3 times; then the precipitate was washed with acetone, centrifuged again for 5 minutes after washing, and the supernatant was removed, and this process was repeated 3 times; finally, the precipitate after centrifugation was placed in a drying oven and dried at 80°C for 12 hours to obtain a modified metal organic adsorbent.
[0074] The scanning electron microscopy image of the prepared modified metal organic adsorbent is shown in Figure 1 As shown, electron microscopy results show that the modified metal organic adsorbent has a flower-like structure composed of ultra-thin layers crossing each other.
[0075] Comparative Example 1
[0076] This comparative example provides a metal organic adsorbent for precious metal recovery. The preparation method is different from that of Example 1 only in that steps (4) to (6) are not performed, and steps (1) to (3) are completely the same to obtain a metal organic layer precursor powder.
[0077] The scanning electron microscopy image of the prepared metal organic adsorbent is shown in Figure 2 As shown, the electron microscopy results show that the morphology of the modified metal organic adsorbent prepared in Example 1 is similar.
[0078] Test Example 1
[0079] This test example evaluates the adsorption performance of the adsorbents prepared in Example 1 and Comparative Example 1 on gold in wastewater:
[0080] (1) Test method:
[0081] Wastewater was prepared with precious metals and multiple coexisting heavy metal ions (gold, manganese, mercury, beryllium, cadmium, copper, lead, zinc, cobalt, nickel, sodium, potassium, calcium, magnesium and multiple metal ions) to test the concentration of each metal ion before adsorption. The detection method is shown in GB / T 30902-2014. Among them, the concentration of gold is 0.1 mg / L. The static adsorption method is used, that is, 10 mg of adsorbent is accurately weighed into 50 mL of wastewater to be tested, and the magnetic rotor is stirred at a speed of 500 rpm. Water samples are taken at fixed intervals, and the concentration of each metal ion in the supernatant after adsorption is tested by the same method.
[0082] (2) Test results:
[0083] The adsorption amount of gold in wastewater with a pH of 2 at different concentrations of the adsorbents prepared in Example 1 and Comparative Example 1 is shown in the figure below: Figure 3As shown in the figure, it can be seen that the adsorption amount of the modified metal organic adsorbent obtained in Example 1 is significantly higher than that of the unmodified metal organic layer precursor adsorbent in Comparative Example 1. The maximum adsorption capacity of the modified metal organic adsorbent can reach 2400 mg Au / g, while the maximum adsorption capacity of the unmodified metal organic layer precursor adsorbent in Comparative Example 1 is 1000 mg Au / g.
[0084] The recovery rate of each metal ion in wastewater with a pH of 2 using the adsorbent prepared in Example 1 with a concentration of 0.2 mg / ml is as follows: Figure 4 As shown in the figure, it can be seen that the modified metal organic adsorbent obtained in Example 1 has high selectivity for precious metals, the gold recovery rate reaches more than 95%, and has no adsorption for other coexisting heavy metal ions.
[0085] The modified metal organic adsorbent of Example 1 after adsorbing the precious metal was observed by transmission electron microscopy. Figure 5 As shown, there are a large number of gold nanoparticles on the surface of the modified metal organic adsorbent after adsorption, indicating that the adsorption process is accompanied by the reduction of gold to a single substance.
[0086] At the same time, the adsorption of gold in wastewater by the adsorbent prepared in Example 1 at different pH values was investigated over time. Figure 6 As shown in the figure, it can be seen that the slope of the change curve can represent the adsorption rate. The adsorption rate of the modified metal organic adsorbent obtained in Example 1 is the largest under acidic conditions. The modified metal organic adsorbent obtained in Example 1 is applicable to wastewater with a pH of 2-9 and strongly acidic wastewater. In addition, the modified metal organic adsorbent obtained in Example 1 has a faster adsorption rate, and gold is basically completely adsorbed after 1 minute.
[0087] Example 2
[0088] This embodiment provides a modified metal organic adsorbent for precious metal recovery, and the preparation method is as follows:
[0089] (1) Weigh 200 mg of 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine, 100 mg of zirconium nitrate, and 62 mg of zirconium oxychloride into a 100 mL polytetrafluoroethylene reactor, add 60 mL of N,N-dimethylformamide, add a magnetic rotor and stir for 10 min, then add 8 mL of formic acid and 2 mL of water;
[0090] (2) stirring the obtained solid-liquid mixture for 15 minutes, then placing it in an ultrasonic instrument and ultrasonicating it at a power of 120 W for 10 minutes, heating it to 140° C. and reacting it for 36 hours to obtain a metal organic layer precursor mixture;
[0091] (3) The obtained metal organic layer mixed solution was centrifuged at a speed of 8000 rpm for 10 min, the supernatant was removed and the precipitate was collected; then the precipitate was washed with N,N-dimethylformamide, centrifuged again for 10 min after washing, and the supernatant was removed, and this was repeated 3 times; then the precipitate was washed with methanol, centrifuged again for 10 min after washing, and the supernatant was removed, and this was repeated 3 times; finally, the centrifuged precipitate was placed in a drying oven and dried at 100° C. for 24 h to obtain a metal organic layer precursor powder;
[0092] (4) Weigh 200 mg of the obtained metal organic layer precursor powder into a 50 mL polytetrafluoroethylene reactor, add 20 mL of N,N-dimethylformamide, add a magnetic rotor and stir for 15 min, then add 160 mg of 5,10,15,20-tetrakis(4-carboxymethoxyphenyl)-21H,23H-porphine, and continue stirring for 10 min;
[0093] (5) placing the obtained solid-liquid mixture into an ultrasonic device and ultrasonicating it at a power of 180 W for 5 min, heating it to 120° C. and reacting it for 8 h to obtain a modified metal organic layer mixture;
[0094] (6) The obtained modified polymer mixture was centrifuged at a speed of 8000 rpm for 10 min, the supernatant was removed and the precipitate was collected; then the precipitate was washed with N,N-dimethylformamide, centrifuged again for 10 min after washing, and the supernatant was removed, and this process was repeated 3 times; then the precipitate was washed with acetone, centrifuged again for 10 min after washing, and the supernatant was removed, and this process was repeated 3 times; finally, the precipitate after centrifugation was placed in a drying oven and dried at 100°C for 12 h to obtain a modified metal organic adsorbent.
[0095] Test Example 2
[0096] This test example evaluates the adsorption performance of the adsorbent prepared in Example 2 on platinum in wastewater:
[0097] Test method: Select precious metals and multiple coexisting heavy metal ions (platinum, manganese, mercury, beryllium, cadmium, copper, lead, zinc, cobalt, nickel, sodium, potassium, calcium, magnesium and multiple metal ions) to prepare wastewater with a pH of 2, and test the concentration of each metal ion before adsorption. The detection method is shown in GB / T 30902-2014, where the concentration of platinum is 10 mg / L. The static adsorption method is used, that is, 10 mg of adsorbent is accurately weighed into 50 mL of the wastewater to be tested, and the magnetic rotor is stirred at a speed of 500 rpm.
[0098] Test results: After 5 minutes, the platinum recovery rate reached 99.5%, which was basically completely adsorbed, and there was no adsorption of other coexisting ions. At the same time, the obtained modified metal organic adsorbent is applicable to wastewater with a pH of 2-9 and strongly acidic wastewater.
[0099] Example 3
[0100] This embodiment provides a modified metal organic adsorbent for precious metal recovery, and the preparation method is as follows:
[0101] (1) Weigh 200 mg of 1,3,5-tris(4-carboxyphenyl)benzene, 120 mg of zirconium bromide, and 40 mg of zirconium chloride in a 100 mL polytetrafluoroethylene reactor, add 60 mL of N,N-dimethylformamide, add a magnetic rotor and stir for 5 min, then add 12 mL of formic acid and 0.8 mL of water;
[0102] (2) stirring the obtained solid-liquid mixture for 10 min, heating it to 125° C. and reacting it for 32 h to obtain a metal organic layer precursor mixture;
[0103] (3) The obtained metal organic layer mixed solution was centrifuged at a speed of 7500 rpm for 3 minutes, the supernatant was removed and the precipitate was collected; then the precipitate was washed with N,N-dimethylformamide, centrifuged again for 3 minutes after washing, and the supernatant was removed, and this was repeated 3 times; then the precipitate was washed with methanol, centrifuged again for 3 minutes after washing, and the supernatant was removed, and this was repeated 3 times; finally, the precipitate after centrifugation was placed in a drying oven and dried at 105°C for 16 hours to obtain a metal organic layer precursor powder;
[0104] (4) Weigh 170 mg of the obtained metal organic layer precursor powder into a 50 mL polytetrafluoroethylene reactor, add 10 mL of N,N-dimethylformamide, add a magnetic rotor and stir for 8 min, then add 70 mg of 5-(4-methoxycarbonylphenyl)-10,15,2-triphenylporphine and continue stirring for 3 min;
[0105] (5) placing the obtained solid-liquid mixture into an ultrasonic instrument and ultrasonicating it at a power of 240 W for 20 min, heating it to 135° C. and reacting it for 6 h to obtain a modified metal organic layer mixture;
[0106] (6) The obtained modified polymer mixture was centrifuged at a speed of 7000 rpm for 5 minutes, the supernatant was removed and the precipitate was collected; then the precipitate was washed with N,N-dimethylacetamide, centrifuged again for 5 minutes after washing, and the supernatant was removed, and this was repeated 3 times; then the precipitate was washed with ethanol, centrifuged again for 5 minutes after washing, and the supernatant was removed, and this was repeated 3 times; finally, the precipitate after centrifugation was placed in a drying oven and dried at 110°C for 10 hours to obtain a modified metal organic adsorbent.
[0107] Test Example 3
[0108] This test example evaluates the adsorption performance of the adsorbent prepared in Example 3 on palladium in wastewater:
[0109] Test method: Select precious metals and multiple coexisting heavy metal ions (palladium, manganese, mercury, beryllium, cadmium, copper, lead, zinc, cobalt, nickel, sodium, potassium, calcium, magnesium and multiple metal ions) to prepare wastewater with a pH of 3, and test the concentration of each metal ion before adsorption. The detection method is shown in GB / T 30902-2014, where the concentration of palladium is 8 mg / L. The static adsorption method is used, that is, 10 mg of adsorbent is accurately weighed into 50 mL of the wastewater to be tested, and the magnetic rotor is stirred at a speed of 500 rpm.
[0110] Test results: After 5 minutes, the platinum recovery rate reached 99.0%, and the platinum was basically completely adsorbed, and there was no adsorption of other coexisting ions. At the same time, the obtained modified metal organic adsorbent is applicable to wastewater with a pH of 2-9 and strongly acidic wastewater.
[0111] Example 4
[0112] This embodiment provides a modified metal organic adsorbent for precious metal recovery, and the preparation method is as follows:
[0113] (1) Weigh 200 mg of 1,3,5-tris(4-carboxyphenylethynyl)benzene, 100 mg of zirconium nitrate, and 62 mg of zirconium oxychloride into a 100 mL polytetrafluoroethylene reactor, add 60 mL of N,N-dimethylformamide, add a magnetic rotor and stir for 10 min, then add 8 mL of formic acid and 2 mL of water;
[0114] (2) The obtained solid-liquid mixture was stirred for 15 minutes, then placed in an ultrasonicator for 10 minutes at 120W, and heated to 140°C for 36 hours to obtain a metal organic layer precursor mixture;
[0115] (3) The obtained metal organic layer mixed solution was centrifuged at a speed of 8000 rpm for 10 min, the supernatant was removed and the precipitate was collected; then the precipitate was washed with N,N-dimethylformamide, centrifuged again for 10 min after washing, and the supernatant was removed, and this was repeated 3 times; then the precipitate was washed with methanol, centrifuged again for 10 min after washing, and the supernatant was removed, and this was repeated 3 times; finally, the centrifuged precipitate was placed in a drying oven and dried at 100° C. for 24 h to obtain a metal organic layer precursor powder;
[0116] (4) Weigh 200 mg of the obtained metal organic layer precursor powder into a 50 mL polytetrafluoroethylene reactor, add 20 mL of N,N-dimethylformamide, add a magnetic rotor to stir for 15 min, then add 160 mg of 5,10,15,20-tetrakis(2,6-dichlorophenyl)porphine, and continue stirring for 5 min;
[0117] (5) placing the obtained solid-liquid mixture into an ultrasonic device and ultrasonicating it at a power of 180 W for 5 min, heating it to 120° C. and reacting it for 8 h to obtain a modified metal organic layer mixture;
[0118] (6) The obtained modified polymer mixture was centrifuged at a speed of 8000 rpm for 10 min, the supernatant was removed and the precipitate was collected; then the precipitate was washed with N,N-dimethylformamide, centrifuged again for 10 min after washing, and the supernatant was removed, and this process was repeated 3 times; then the precipitate was washed with acetone, centrifuged again for 10 min after washing, and the supernatant was removed, and this process was repeated 3 times; finally, the precipitate after centrifugation was placed in a drying oven and dried at 100°C for 12 h to obtain a modified metal organic adsorbent.
[0119] Test Example 4
[0120] This test example evaluates the adsorption performance of the adsorbent prepared in Example 4 on rhodium in wastewater:
[0121] Test method: Select precious metals and multiple coexisting heavy metal ions (rhodium, manganese, mercury, beryllium, cadmium, copper, lead, zinc, cobalt, nickel, sodium, potassium, calcium, magnesium and multiple metal ions) to prepare wastewater with a pH of 2, and test the concentration of each metal ion before adsorption. The detection method is shown in GB / T 30902-2014, where the concentration of rhodium is 7 mg / L. The static adsorption method is used, that is, 10 mg of adsorbent is accurately weighed into 50 mL of wastewater to be tested, and the magnetic rotor is stirred at a speed of 500 rpm.
[0122] Test results: After 5 minutes, the rhodium recovery rate reached 98.8%, which was basically completely adsorbed, and there was no adsorption of other coexisting ions. At the same time, the obtained modified metal organic adsorbent is applicable to wastewater with a pH of 2-9 and strongly acidic wastewater.
[0123] Example 5
[0124] This embodiment provides a modified metal organic adsorbent for precious metal recovery, and the preparation method is as follows:
[0125] (1) Weigh 220 mg of 1,3,5-tris(4-carboxyphenylethynyl)benzene and 200 mg of zirconium oxychloride into a 100 mL polytetrafluoroethylene reactor, add 70 mL of N,N-dimethylformamide, add a magnetic rotor to stir for 5 min, then add 12 mL of formic acid and 0.4 mL of water;
[0126] (2) stirring the obtained solid-liquid mixture for 5 min, then placing it in an ultrasonicator and ultrasonicating it at 180 W for 5 min, heating it to 135° C. and reacting it for 30 h to obtain a metal organic layer precursor mixture;
[0127] (3) The obtained metal organic layer mixed solution is centrifuged at a speed of 3000 rpm for 15 minutes, the supernatant is removed and the precipitate is collected; then the precipitate is washed with N,N-dimethylacetamide, centrifuged again for 15 minutes after washing, and the supernatant is removed, and this is repeated 3 times; then the precipitate is washed with ethanol, centrifuged again for 15 minutes after washing, and the supernatant is removed, and this is repeated 3 times; finally, the centrifuged precipitate is placed in a drying oven and dried at 120° C. for 20 hours to obtain a metal organic layer precursor powder;
[0128] (4) Weigh 150 mg of the obtained metal organic layer precursor powder into a 50 mL polytetrafluoroethylene reactor, add 20 mL of N,N-dimethylacetamide, add a magnetic rotor and stir for 8 min, then add 135 mg of 5,10,15,20-tetrakis(4-carboxymethoxyphenyl)-21H,23H-porphine, and continue stirring for 8 min;
[0129] (5) placing the obtained solid-liquid mixture into an ultrasonic instrument and ultrasonicating it at a power of 360 W for 20 min, heating it to 135° C. and reacting it for 8 h to obtain a modified metal organic layer mixture;
[0130] (6) The obtained modified polymer mixture was centrifuged at 3000 rpm for 15 min, the supernatant was removed and the precipitate was collected; then the precipitate was washed with N,N-dimethylacetamide, centrifuged again for 15 min after washing, and the supernatant was removed, and this process was repeated 3 times; then the precipitate was washed with ethanol, centrifuged again for 15 min after washing, and the supernatant was removed, and this process was repeated 3 times; finally, the precipitate after centrifugation was placed in a drying oven and dried at 120°C for 8 h to obtain a modified metal organic adsorbent.
[0131] Test Example 5
[0132] This test example evaluates the adsorption performance of the adsorbent prepared in Example 5 on iridium in wastewater:
[0133] Test method: Select precious metals and multiple coexisting heavy metal ions (iridium, manganese, mercury, beryllium, cadmium, copper, lead, zinc, cobalt, nickel, sodium, potassium, calcium, magnesium and multiple metal ions) to prepare wastewater with a pH of 4, and test the concentration of each metal ion before adsorption. The detection method is shown in GB / T 30902-2014, where the concentration of iridium is 9 mg / L. The static adsorption method is used, that is, 10 mg of adsorbent is accurately weighed into 50 mL of wastewater to be tested, and the magnetic rotor is stirred at a speed of 500 rpm.
[0134] Test results: After 5 minutes, the iridium recovery rate reached 99.2%, which was basically completely adsorbed, and there was no adsorption of other coexisting ions. At the same time, the obtained modified metal organic adsorbent is applicable to wastewater with a pH of 2-9 and strongly acidic wastewater.
[0135] Application Example 1
[0136] This application example provides the application of the adsorbent prepared in Example 1 to adsorb and recover precious metals in circuit board waste liquid:
[0137] (1) Selecting a certain type of waste circuit board after soaking in a 5 mol / L sodium hydroxide aqueous solution and aqua regia (nitric acid / hydrochloric acid = 1 / 3) as the circuit board waste liquid to be treated, the metal in the circuit board is dissolved in the solution in the form of ions (including gold, copper, aluminum, nickel, cesium, iron, and manganese);
[0138] (2) Use Figure 7 The treatment device shown in the figure is used for treatment. First, the circuit board waste liquid is transported into the regulating tank, and the pH value of the waste water in the regulating tank is monitored by a pH detector, and the dosing pump switch is fed back in real time and controlled to adjust the pH value of the waste water to 2. After the adjustment, the circuit board waste liquid enters the adsorption unit;
[0139] (3) According to the influent precious metal ion concentration fed back by the precious metal online analyzer and the influent water volume fed back by the electromagnetic flowmeter, the hydraulic retention time of the waste liquid in the adsorption unit is controlled to be 2 h, the separated solid adsorbent is passed into the separation and recovery unit, and the effluent is sent to the downstream treatment module;
[0140] (4) After the solid adsorbent separated by the adsorption unit enters the separation and recovery unit, it is first transported to the regulating tank. The pH value in the regulating tank is monitored using a pH detector, and the dosing pump switch is controlled in real time to adjust the pH value to 12. The residence time is 2 hours. The effluent passes through a solid-liquid cyclone separator, and the solid enters a rotary kiln at a temperature of 1000°C and a residence time of 4 hours. The obtained solid is a solid precious metal with a purity of more than 90%. The concentration (mg / L) of the precious metal in the effluent is analyzed by a precious metal online analyzer. The test results are shown in Table 1.
[0141] Table 1
[0142] index gold copper aluminum nickel cesium iron manganese Before treatment 7 800 200 50 7.0 6.3 3.5 After treatment 0.01 800 200 50 7.0 6.3 3.5 Removal rate 99.9% 0% 0% 0% 0% 0% 0%
[0143] From the data results in Table 1, it can be seen that the modified metal organic adsorbent involved in the present invention has adsorption performance with high selectivity, high adsorption rate and high adsorption capacity for precious metals, and has good application prospects.
[0144] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate a modified metal organic adsorbent for precious metal recovery and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
[0145] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0146] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
Claims
1. A method for preparing a modified metal organic adsorbent for precious metal recovery, characterized in that: The preparation method comprises the following steps: (1) mixing a zirconium salt, an aromatic acid organic compound and a solvent, and reacting them to obtain a metal organic layer precursor; the aromatic acid organic compound includes any one of 1,3,5-tris(4-carboxyphenyl)benzene, 2,4,6-tris(4-carboxyphenyl)-1,3,5-triazine or 1,3,5-tris(4-carboxyphenylethynyl)benzene, or a combination of at least two thereof; (2) mixing a metal organic layer precursor, a porphine compound and a solvent, and reacting them to obtain the modified metal organic adsorbent; the porphine compound contains a porphyrin ring, including meso-tetraphenylporphine, 5,10,15,20-tetrakis(2,6-dichlorophenyl)porphine, meso-tetrakis(4-carboxyphenyl)porphine, meso-tetrakis(isobenzoic acid)porphine, 5,10,15,20- Any one of tetrakis(4-carboxyphenyl)porphine tetramethyl ester, racemic-tetrakis(N-methyl-3-pyridyl)porphine tetrachloride, 5,10,15,20-tetrakis(4-carboxymethoxyphenyl)-21H,23H-porphine, 5-(4-methoxycarbonylphenyl)-10,15,2-triphenylporphine or 5,10,15,20-tetrakis(4-pyridyl)porphine, or a combination of at least two thereof.
2. The preparation method according to claim 1, characterized in that: The zirconium salt includes any one of zirconium chloride, zirconium oxychloride, zirconium nitrate or zirconium bromide, or a combination of at least two thereof.
3. The preparation method according to claim 1, characterized in that: The molar ratio of the zirconium salt to the aromatic acid organic compound in step (1) is 1:(0.1-10).
4. The preparation method according to claim 1, characterized in that: The solvent in step (1) is a mixed solvent of an organic solvent, a carboxylic acid and water.
5. The preparation method according to claim 4, characterized in that: The organic solvent includes any one of N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone, or a combination of at least two thereof.
6. The preparation method according to claim 4, characterized in that: The carboxylic acid includes any one of formic acid, acetic acid, propionic acid or trifluoroacetic acid, or a combination of at least two thereof.
7. The preparation method according to claim 4, characterized in that: The volume ratio of the organic solvent, carboxylic acid and water in the mixed solvent is 8:(0.1-2):(0.1-2).
8. The preparation method according to claim 1, characterized in that: The molar volume ratio of the aromatic acid organic compound to the organic solvent is 0.1-5 mol / L.
9. The preparation method according to claim 1, characterized in that: Before the reaction in step (1), stirring and / or ultrasonic treatment is performed.
10. The preparation method according to claim 9, characterized in that: The stirring speed is 100-600 rpm, and the stirring time is 1-30 min.
11. The preparation method according to claim 9, characterized in that: The power of the ultrasound is 60-360W, and the time of the ultrasound is 1-30min.
12. The preparation method according to claim 1, characterized in that: The reaction temperature of step (1) is 80-150° C., and the reaction time is 12-72 hours.
13. The preparation method according to claim 1, characterized in that: After the reaction in step (1) is completed, post-treatment is performed, and the post-treatment includes: cooling the reaction solution, centrifuging, washing the precipitate, and drying.
14. The preparation method according to claim 1, characterized in that: The solvent in step (2) includes any one of N,N-dimethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone, or a combination of at least two thereof.
15. The preparation method according to claim 1, characterized in that: In step (2), the concentration of the metal organic layer precursor in the solvent is 1-10 g / L.
16. The preparation method according to claim 1, characterized in that: The mass ratio of the metal organic layer precursor to the porphine compound is 1:(0.3-4).
17. The preparation method according to claim 1, characterized in that: The reaction in step (2) is also preceded by ultrasonic treatment.
18. The preparation method according to claim 17, characterized in that: The power of the ultrasound is 60-360W, and the time of the ultrasound is 1-30min.
19. The preparation method according to claim 1, characterized in that: The reaction temperature of step (2) is 60-140° C., and the reaction time is 5-20 h.
20. The preparation method according to claim 1, characterized in that: After the reaction in step (2) is completed, post-treatment is performed, and the post-treatment includes: cooling the reaction solution, centrifuging, washing the precipitate, and drying.
21. A modified metal organic adsorbent for precious metal recovery obtained by the preparation method according to any one of claims 1 to 20.
22. Use of the modified metal organic adsorbent for precious metal recovery according to claim 21 in recovering precious metals.
23. The use according to claim 22, characterized in that The modified metal organic adsorbent is used for recovering precious metals from waste liquid.
24. The use according to claim 23, characterized in that The treatment device used in the application comprises a regulating unit, an adsorption unit, a separation and recovery unit and an auxiliary monitoring unit; the regulating unit, the adsorption unit and the separation and recovery unit are connected in sequence; The regulating unit includes an acid-base dosing pump and a regulating tank; The adsorption unit includes a fixed bed reactor; The separation and recovery unit includes a regulating tank, a dosing pump, a cyclone separator and a rotary kiln; The auxiliary monitoring unit includes a water quantity detection module and a water quality monitoring module. The water quantity detection module includes an electromagnetic flowmeter, and the water quality monitoring module includes a pH detector and a precious metal online analyzer.
25. The use according to claim 23, characterized in that The waste liquid contains precious metal ions at a concentration of 1-4000 mg / L, and the pH of the waste liquid is in the range of 0-9.
26. The use according to claim 23, characterized in that The mass volume ratio of the modified metal organic adsorbent to the waste liquid is 0.05-200 mg / mL.
Citation Information
Patent Citations
Tetrathiol-porphyrin compound as well as preparation method and application thereof
CN107759803A
Treatment method for selectively adsorbing and recycling precious metal ions in wastewater by using modified polymer adsorbent