Modified magnesium-aluminum composite oxide carrier and preparation method thereof, catalyst and method for dry reforming of methane to produce synthesis gas
By preparing the modified magnesium-aluminum composite oxide support, an orderly mesoporous structure was formed, which solved the problem of poor stability of the catalyst at high temperature, improved the activity and anti-carbon properties of the methane dry reforming catalyst, and achieved high efficiency of the catalyst application.
Patent Information
- Application Number
- CN202111242639.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-25
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-25
AI Technical Summary
The existing methane dry reforming catalysts have poor stability under high temperature reaction conditions and are prone to carbonization, resulting in the migration of active metals and the increase in particle size, limiting the industrial application of the process.
Using a modified magnesium-aluminum composite oxide support, the magnesium-aluminum spindle with an orderly mesoporous structure is dried and calcined by mixing acid, aluminum oxide precursor, magnesium-aluminum precursor and modification additive precursor in a solvent. stone enhances the interaction between the support and the active metal, improves the stability of the catalyst and the resistance to carbon deposits.
It significantly improves the activity, stability and anti-carbon deposit performance of the catalyst, ensures the maintenance of the specific surface area of the carrier after high-temperature calcination, the size of metal particles is stable, and the catalytic activity is high, and it is suitable for methane dry reforming reaction.
Smart Images

Figure CN116020436B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalyst preparation, and in particular to a modified magnesium-aluminum composite oxide carrier and a preparation method thereof, and a catalyst and method for dry reforming methane to produce synthesis gas. Background Art
[0002] Methane is an important resource. It can be directly converted into methanol and formaldehyde; ethylene can be produced by coupling oxidation of methane; aromatic hydrocarbons and hydrogen can be produced from methane under anaerobic conditions. It is very difficult to produce acetylene by partial oxidation of methane; indirect conversion of methane into synthesis gas (H2 / CO) and subsequent preparation of high value-added intermediate chemicals and clean oil products through the Fischer-Tropsch synthesis process is an industrial route with great potential application significance. CO2 and methane are both greenhouse gases. In recent years, the demand for reducing greenhouse gas emissions has increased. Using CO2 and methane as raw materials for dry reforming reaction and preparing synthesis gas through catalysts is beneficial to alleviate the greenhouse effect caused by both and generate synthesis gas that is easy to process later. However, this process has not yet been industrialized. The reason is that the sintering and carbon deposition of the catalyst under high temperature reaction conditions are the main obstacles to the industrialization of this process. Therefore, the development of high-activity, high-selectivity and high-stability methane dry reforming catalysts is still the key to current research in this field.
[0003] At present, the main disadvantages of methane dry reforming catalysts reported in patents and literature are poor catalyst stability and easy deactivation due to carbonization. Nickel-based catalysts are cheap and have high activity, and are suitable active metal groups. Therefore, how to keep the active metals in nickel-based catalysts stable and prevent them from migrating and aggregating during high-temperature reactions and causing the metal particles to grow in size is the key to preparing highly active and highly stable nickel-based catalysts. Summary of the invention
[0004] The purpose of the present invention is to overcome the problems of low activity, small specific surface, easy occurrence of reverse water-gas reaction and poor stability of catalysts prepared with alumina and magnesium-aluminum spinel as carriers in the prior art, and to provide a modified magnesium-aluminum composite oxide carrier and a preparation method thereof, and a catalyst and method for dry reforming of methane to produce synthesis gas. The modified magnesium-aluminum composite oxide carrier has an ordered mesoporous structure, and the catalyst prepared using the carrier has high activity, stability and good anti-coking performance.
[0005] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a modified magnesium-aluminum composite oxide carrier, which includes a magnesium-aluminum composite oxide and a modification aid. Based on the total amount of the carrier, the content of the magnesium-aluminum composite oxide is 85-99.9% by weight, and the content of the modification aid is 0.1-15% by weight; based on the weight of the magnesium-aluminum composite oxide, the content of aluminum oxide is 60-99% by weight, and the content of magnesium oxide is 1-40% by weight; the modification aid is selected from at least one of alkaline earth metal oxides and rare earth metal oxides; the magnesium-aluminum composite oxide is an ordered mesoporous magnesium-aluminum spinel.
[0006] The second aspect of the present invention provides a method for preparing a modified magnesium-aluminum composite oxide carrier, the method comprising:
[0007] In the presence of a surfactant and a solvent, an acid, an aluminum oxide precursor, a magnesium oxide precursor and a modifying agent precursor are mixed, and then dried and calcined; the modifying agent is selected from at least one of an alkaline earth metal oxide and a rare earth metal oxide; the aluminum oxide precursor, the magnesium oxide precursor and the modifying agent precursor are used in such an amount that, in the prepared modified magnesium-aluminum composite oxide carrier, based on the total amount of the carrier, the content of the magnesium-aluminum composite oxide is 85-99.9% by weight, and the content of the modifying agent is 0.1-15% by weight; based on the total amount of the magnesium-aluminum composite oxide, the content of aluminum oxide is 60-99% by weight, and the content of magnesium oxide is 1-40% by weight.
[0008] The third aspect of the present invention provides a catalyst for dry reforming of methane to produce synthesis gas, the catalyst comprising a carrier and an active component, the carrier being the modified magnesium-aluminum composite oxide carrier described in the first aspect or the modified magnesium-aluminum composite oxide carrier prepared by the preparation method described in the second aspect.
[0009] A fourth aspect of the present invention provides a method for producing synthesis gas by dry reforming of methane, the method comprising: under conditions of dry reforming of methane to produce synthesis gas, contacting methane and carbon dioxide with a catalyst, wherein the catalyst is the catalyst for dry reforming of methane to produce synthesis gas as described in the third aspect.
[0010] The inventors discovered in their research that the carrier provided by the present invention has a large specific surface area and a strong ability to resist high-temperature sintering. After high-temperature calcination, the carrier phase transforms into a magnesium-aluminum spinel structure with ordered mesopores. After being made into a catalyst, the interaction force between the carrier and the active metal is strong, thereby greatly improving the stability of the carrier structure. After high-temperature calcination, the specific surface area of the carrier remains at a high level, and the carrier has a suitable pore size and pore volume.
[0011] The special ordered structure and magnesium-aluminum spinel phase can significantly improve the dispersion ability of the metal, thereby obtaining smaller metal clusters, and under harsh reaction conditions, the metal has better high-temperature sintering resistance and maintains a smaller size after the reaction. When the modified magnesium-aluminum oxide composite carrier and catalyst prepared by the present invention are used in dry reforming reactions, compared with similar catalysts, the catalytic activity is higher, and the anti-coking ability and the anti-sintering ability of active metals are significantly enhanced. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is the wide-angle XRD pattern of Example 1 of the present invention and Comparative Example 1 at 5-75°;
[0013] Figure 2 is the small-angle XRD pattern of Example 1 of the present invention and Comparative Example 1 at 0-5°;
[0014] Figure 3 is a curve diagram of the reaction performance of methane dry reforming catalyzed by the catalyst in Example 1;
[0015] Figure 4 This is a performance curve of the methane dry reforming reaction catalyzed by the catalyst in Comparative Example 1. DETAILED DESCRIPTION
[0016] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0017] The first aspect of the present invention provides a modified magnesium-aluminum composite oxide carrier, which includes a magnesium-aluminum composite oxide and a modification aid. Based on the total amount of the carrier, the content of the magnesium-aluminum composite oxide is 85-99.9% by weight, and the content of the modification aid is 0.1-15% by weight; based on the total amount of the magnesium-aluminum composite oxide, the content of aluminum oxide is 60-99% by weight, and the content of magnesium oxide is 1-40% by weight; the modification aid is selected from at least one of alkaline earth metal oxides and rare earth metal oxides; the magnesium-aluminum composite oxide is an ordered mesoporous magnesium-aluminum spinel.
[0018] The ordered mesoporous structure of the magnesium-aluminum composite oxide described in the present invention is characterized by small-angle XRD.
[0019] In a preferred embodiment, based on the total amount of the carrier, the content of the magnesium-aluminum composite oxide is 90-98% by weight, and the content of the modification aid is 2-10% by weight.
[0020] In a preferred embodiment, based on the total amount of the magnesium-aluminum composite oxide, the content of aluminum oxide is 69-97% by weight, and the content of magnesium oxide is 3-31% by weight.
[0021] In a preferred embodiment, the modification aid is selected from at least one of the alkaline earth metal elements Be, Ca, Mg, Ba and Sr.
[0022] In a preferred embodiment, the modification aid is selected from at least one of the rare earth metal elements La, Y, Ce, Pr, Nd and Sm.
[0023] In a specific embodiment, the modification aid is selected from at least one of Be, Ca, Mg, Ba, Sr, La, Y, Ce, Pr, Nd and Sm.
[0024] In a specific embodiment, the modification aid is selected from at least one of CaO, La2O3, CeO2 and Y2O3, more preferably La2O3 and CeO2, and more preferably, the mass ratio of CeO2 to La2O3 is 0.1-4:1, preferably 0.1-2:1. The advantages of adopting this preferred embodiment are that the active component nickel grains are smaller, the nickel dispersion is higher, and the reaction activity is higher.
[0025] In the present invention, the metal content is measured by ICP method.
[0026] In the present invention, preferably, the specific surface area of the carrier is 3-250m 2 / g, pore volume is 0.2-0.7cm 3 / g, the average pore size is 9-25nm, and more preferably, the specific surface area of the carrier is 60-250m 2 / g, pore volume is 0.25-0.7cm 3 / g, and the average pore size is 9-20nm.
[0027] The carrier provided by the present invention has a large specific surface area, suitable pore volume and average pore diameter, so that the carrier has the advantages of uniform dispersion of the active component nickel and smaller crystal grains.
[0028] In the present invention, the specific surface area, pore volume and average pore diameter of the carrier can be characterized and measured by nitrogen adsorption method.
[0029] The second aspect of the present invention provides a method for preparing a modified magnesium-aluminum oxide composite carrier, which comprises: in the presence of a surfactant and a solvent, an acid, an aluminum oxide precursor, a magnesium oxide precursor and a modification aid precursor are mixed, and then dried and calcined; the modification aid is selected from at least one of an alkaline earth metal oxide and a rare earth metal oxide; the amount of the aluminum oxide precursor, the magnesium oxide precursor and the modification aid precursor is such that in the prepared modified magnesium-aluminum composite oxide carrier, based on the total amount of the carrier, the content of the magnesium-aluminum composite oxide is 85-99.9% by weight, and the content of the modification aid is 0.1-15% by weight; based on the total amount of the magnesium-aluminum composite oxide, the content of aluminum oxide is 60-99% by weight, and the content of magnesium oxide is 1-40% by weight.
[0030] In a preferred case, the amounts of the aluminum oxide precursor, the magnesium oxide precursor and the modifying agent precursor are such that in the prepared modified magnesium-aluminum composite oxide carrier, based on the total amount of the carrier, the content of the magnesium-aluminum composite oxide is 90-98 weight %, and the content of the modifying agent is 2-10 weight %; based on the total amount of the magnesium-aluminum composite oxide, the content of aluminum oxide is 69-97 weight %, and the content of magnesium oxide is 3-31 weight %.
[0031] According to the method of the present invention, preferably, the modification aid is selected from at least one of the alkaline earth metal elements Be, Ca, Mg, Ba and Sr.
[0032] In a preferred embodiment, the modification aid is selected from at least one of the rare earth metal elements La, Y, Ce, Pr, Nd and Sm.
[0033] In a specific embodiment, the modification aid is selected from at least one of Be, Ca, Mg, Ba, Sr, La, Y, Ce, Pr, Nd and Sm.
[0034] In a specific embodiment, the modification aid is selected from at least one of CaO, La2O3, CeO2 and Y2O3, more preferably La2O3 and CeO2.
[0035] In a preferred embodiment, the mass ratio of CeO2 and La2O3 is 0.1-4:1, preferably 0.1-2:1. In this preferred embodiment, the use of CeO2 and La2O3 in combination is more conducive to improving the activity, selectivity, stability and anti-carbon deposition ability of the catalyst prepared by the carrier in the methane dry reforming reaction.
[0036] According to the method of the present invention, in order to uniformly mix the surfactant, solvent, acid oxygen, aluminum oxide precursor, magnesium oxide precursor and modification aid precursor, the mixing preferably comprises the following steps:
[0037] (1) first mixing a surfactant, a solvent, an acid and an alumina precursor;
[0038] (2) Adding a magnesium oxide precursor and a modification aid precursor to the first mixed material.
[0039] According to the method of the present invention, preferably, in step (1), the first mixing is performed under stirring conditions, and stirring is performed to make the mixing of the surfactant, solvent, acid and alumina precursor more uniform.
[0040] In the present invention, the stirring and mixing conditions can be selected in a wide range. Preferably, the first mixing time is 2-10 hours, and more preferably, the time is 4-6 hours.
[0041] According to the method of the present invention, the order of adding the surfactant, solvent, acid and alumina precursor in step (1) is not specifically limited, as long as the four are mixed evenly. Preferably, the surfactant is dissolved in a solvent, and then the acid and alumina precursor are added and mixed.
[0042] According to the method of the present invention, there is no particular limitation on the type of surfactant in step (1), and those skilled in the art can select it according to actual needs. Preferably, the surfactant is selected from at least one of P123, F127 and CTAB, and more preferably P123. The advantage of adopting this preferred embodiment is that a special hexagonal pore structure is formed to promote the dispersion of nickel, so that the catalyst has higher activity.
[0043] In a preferred case, the acid is at least one of nitric acid, sulfuric acid and hydrochloric acid, preferably nitric acid. The advantage of adopting this preferred embodiment is that other elements will not be introduced after calcination, thereby affecting the properties of the carrier.
[0044] In a preferred embodiment, the solvent is selected from at least one of ethanol, H2O and methanol, preferably ethanol.
[0045] In a preferred case, the aluminum oxide precursor is aluminum isopropoxide and / or aluminum nitrate, preferably aluminum isopropoxide. The advantage of adopting this preferred embodiment is that the surface potential of the carrier prepared by aluminum isopropoxide is different, which is more conducive to the loading and dispersion of active metals.
[0046] In a preferred embodiment, the magnesium oxide precursor is magnesium nitrate and / or magnesium chloride, preferably magnesium nitrate.
[0047] According to the method of the present invention, the amount of the surfactant used in step (1) is not specifically limited. Preferably, the molar ratio of the surfactant to the aluminum oxide precursor calculated as the aluminum element is 0.005-0.05:1; more preferably 0.01-0.03:1; and even more preferably 0.015-0.025:1. The purpose of adopting this preferred embodiment is to make the pore structure of the carrier more orderly and improve the catalyst activity.
[0048] According to the method of the present invention, the amount of acid used in step (1) is not specifically limited. Preferably, the molar ratio of the acid to the aluminum oxide precursor calculated as aluminum element is 1-5:1; more preferably 1.5-3:1; and even more preferably 1.95-2.45:1.
[0049] According to the method of the present invention, the amount of the solvent used in step (1) is not specifically limited. Preferably, the molar ratio of the solvent to the aluminum oxide precursor calculated as aluminum element is 30-40:1, more preferably 32-37:1, and even more preferably 34.5-36.5:1.
[0050] According to the method of the present invention, the order of adding the magnesium oxide precursor and the modification aid precursor in step (2) is not particularly limited. Preferably, the magnesium oxide precursor (preferably magnesium nitrate) and the modification aid precursor are added in sequence. The advantage of adopting this preferred embodiment is that the support structure is better.
[0051] In a preferred embodiment, the modification aid precursor is selected from at least one of cerium nitrate, lanthanum nitrate and yttrium nitrate.
[0052] The method according to the present invention further comprises drying and calcining after step (2).
[0053] According to the method of the present invention, the drying conditions can be selected in a wide range. Preferably, the drying temperature is 50-70°C and the drying time is 42-54 hours.
[0054] According to the method of the present invention, the range of roasting conditions is relatively wide. Preferably, the target roasting temperature is 600-1200°C, more preferably 700-1100°C, and the target roasting time is 6-18 hours, more preferably 10-16 hours.
[0055] In a preferred embodiment, the calcination is divided into two stages, which include: heating to 350-450°C at a heating rate of 0.8-1.2°C / min, keeping the temperature for 2-8 hours, preferably 3-5 hours, and then heating to the target calcination temperature of 600-1200°C, preferably 700-1100°C, at a rate of 1-5°C / min. By adopting a two-stage calcination method, the purpose of the first stage calcination is to remove the surfactant in the carrier, and the advantage is to form a hexagonal mesoporous structure; the purpose of the second stage calcination is to make the carrier maintain the structural characteristics of the ordered mesopores. A suitable calcination procedure is conducive to maintaining the ordered mesoporous channels, and the channels will not collapse due to heat.
[0056] The third aspect of the present invention provides a catalyst for preparing synthesis gas by dry reforming of methane, the catalyst comprising a carrier and an active component, the carrier being the modified magnesium-aluminum composite oxide carrier described in the first aspect or the modified magnesium-aluminum composite oxide carrier prepared by the preparation method described in the second aspect.
[0057] According to the method of the present invention, there is no specific limitation on the preparation method of the catalyst. For example, it can be prepared by an impregnation method, specifically, it can be prepared by the following preparation method: the carrier prepared above is dissolved in deionized water and stirred, the precursor solution containing the active component is impregnated in the carrier and allowed to stand, and then placed on a rotary evaporator for vacuum drying, and then dried, and then the dried product is roasted to obtain a catalyst. Wherein, the compound of the active component is selected from a water-soluble active component compound, for example, a nitrate containing an active component.
[0058] According to the method of the present invention, the stirring conditions can be selected in a wide range, as long as the precursor containing the active component can be dissolved.
[0059] According to the method of the present invention, the drying conditions can be selected in a wide range. Preferably, the drying temperature is 80-140°C and the drying time is 4-7 hours.
[0060] According to the method of the present invention, the range of selection of calcination conditions is relatively wide. Preferably, the calcination temperature is 500-700°C and the calcination time is 4-8h.
[0061] According to the method of the present invention, in order to improve the performance of the catalyst in the methane dry reforming reaction, preferably, the active component is selected from at least one of Ni, Co, Fe and a noble metal, and the noble metal can be one of Au, Rh, Pt, Pd, Ir, Ru, and more preferably Ni.
[0062] According to the method of the present invention, in order to further improve the performance of the catalyst in the methane dry reforming reaction, preferably, the content of the active component is 2-10 wt % based on the total amount of the catalyst.
[0063] According to the method of the present invention, preferably, the dispersion of the active components measured by hydrogen chemical adsorption method is 4-28%, and more preferably 12-23%. The catalyst of the present invention has good dispersion, while the dispersion of the active components of existing similar catalysts is usually less than 10%. The dispersion of the catalyst of the present invention is much better than the dispersion of the active components of similar catalysts.
[0064] In a preferred embodiment, the average particle size of the active component is 2-14 nm, preferably 4-9 nm. The catalytic metal provided by the present invention is uniformly dispersed, so that a smaller metal particle size can be obtained.
[0065] In the present invention, the dispersion of the active components is measured by H2 chemical adsorption method using a Micromeritics (ASAP-2010C) chemical adsorption instrument. Specifically, 0.2 g of the sample is first degassed at 300°C for 1 hour, then heated to 700°C for reduction for 2 hours, and then cooled to 40°C for H2 chemical adsorption operation.
[0066] The active component dispersion and the average particle size d of the active component particles were calculated using the following formula based on the amount of chemically adsorbed H2.
[0067] Dispersion of active ingredients D:
[0068]
[0069] Average particle size d of active component particles:
[0070]
[0071] Where V ad It refers to the monolayer adsorption of H2 under standard conditions, in mL; W s is the sample mass in g; FW Me is the molar mass of metal Me such as Ni, in g / mol; F Me is the metal loading in the catalyst, expressed in %; V m SA is the molar gas volume in the index state, in mL / mol; Me is the specific surface area of metal Me, in m 2 / gcat;ρ Me is the metal density of Me in g / cm 3 .
[0072] The catalyst prepared by the present invention is particularly suitable for the reaction of producing synthesis gas by dry reforming of methane, and has high activity, selectivity and stability when used in the reaction process of producing synthesis gas by reforming methane.
[0073] A fourth aspect of the present invention provides a method for producing synthesis gas by dry reforming of methane, the method comprising: under conditions of methane dry reforming to produce synthesis gas, contacting methane and carbon dioxide with a catalyst, wherein the catalyst is the catalyst for producing synthesis gas by dry reforming of methane as described in the third aspect.
[0074] The present invention has no particular limitation on the contact method, which can be a conventional method in the art. For example, the catalyst, methane and carbon dioxide can be contacted by feeding methane and carbon dioxide into a reactor separately and contacting with the catalyst at the same time, or methane and carbon dioxide can be formed into a mixture and then contacted with the catalyst. Preferably, methane and carbon dioxide are formed into a mixture and then contacted with the catalyst.
[0075] According to the method of the present invention, there is no particular limitation on the conditions for producing synthesis gas by dry reforming of methane. Preferably, the conditions for producing synthesis gas by dry reforming of methane include: a molar ratio of carbon dioxide to methane of 1-1.2:1, more preferably 1-1.1:1; a reaction temperature of 600-850°C, more preferably 650-800°C; a pressure of 0-3MPa, more preferably 0-1MPa; a total space velocity of the raw gas of 2000-120000mL·g -1 ·h -1 , more preferably 60000-120000mL·g -1 ·h -1 .
[0076] According to the method of the present invention, before use, the catalyst is reduced and activated by a mixed gas of hydrogen and nitrogen. Preferably, the reduction and activation conditions are as follows: the molar ratio of hydrogen and nitrogen is 1-2:1, the reduction temperature can be 600-800°C, preferably 650-750°C, and the reduction time can be 2-6h, preferably 3-4h.
[0077] In the present invention, XRD is used to detect the physical phase and crystal structure of the carrier in the embodiments and comparative examples.
[0078] The present invention will be described in detail below by way of examples. Unless otherwise specified, the raw materials used in the following examples are commercially available.
[0079] Example 1
[0080] (1) Preparation of catalyst carrier
[0081] Weigh 4g P123 and dissolve it in 80ml anhydrous ethanol, stir vigorously until P123 is completely dissolved, weigh 8g aluminum isopropoxide and 6ml concentrated nitric acid and dissolve them in the anhydrous ethanol solution of P123, stir for 4h, add 2.5g Mg(NO3)2·6H2O and 0.4g Ce(NO3)3·6H2O, dry for 48h, heat to 400℃ at 1℃ / min, keep warm for 5h, then heat to 900℃ at 4℃ / min, keep warm for 2h, and obtain a magnesium aluminum composite oxide carrier. The composition of the carrier is listed in Table 1, and the XRD spectrum is shown as follows Figure 1 and Figure 2 As shown, it is shown that the support is a spinel phase containing ordered mesopores, and the specific surface area, pore volume and average pore size of the support are determined and the data are recorded in Table 2.
[0082] (2) Preparation of Catalyst
[0083] Weigh 0.530g of Ni(NO3)2·6H2O and dissolve it in 5ml of deionized water, stir and dissolve it, impregnate the impregnation liquid into 2g of the above-mentioned magnesium aluminum composite oxide and let it stand for 1h, then place it on a rotary evaporator for vacuum drying, and then place it in an oven for drying at 120℃ for 5h. The dried sample is then placed in a muffle furnace and calcined at 600℃ for 3h. The obtained catalyst is recorded as Ni / Mg-Al-Ce, and the composition of the catalyst is listed in Table 3. The dispersion of the active component of the catalyst measured by hydrogen chemical adsorption method is 19%, and the average particle size of the active component is 4.5nm.
[0084] (3) Catalyst evaluation
[0085] Weigh 0.1 g of Ni / Mg-Al-Ce catalyst, dilute it to 3 ml with quartz sand of 40-60 mesh, load it into a quartz tube reactor with an inner diameter of 8 mm, and reduce it at 700 ° C for 3 h in an atmosphere of hydrogen and nitrogen (1:1) under normal pressure. After the reduction is completed, heat it to 750 ° C in a hydrogen atmosphere, switch the raw gas (CH4 / CO2 / N2 molar ratio = 1.5:1.5:7) to react, and the reaction space velocity is 120000 ml g -1 ·h -1 , the reaction pressure is normal pressure. After the reaction is stable for 120h, the tail gas composition is analyzed by online gas chromatography. The calculation results are: XCH4 = 92.5%, XCO2 = 91.4%, H2 / CO = 1.11.
[0086] The stability evaluation results of the catalyst obtained in Example 1 are shown in Figure 3 , the specific reaction time is 260 hours of the catalytic methane dry reforming reaction performance. Figure 3 It can be seen that the reaction performance of the catalyst is very stable.
[0087] Example 2
[0088] (1) Preparation of catalyst carrier
[0089] Weigh 4g P123 and dissolve it in 80ml anhydrous ethanol, stir vigorously until P123 is completely dissolved, weigh 8g aluminum isopropoxide and 6ml concentrated nitric acid and dissolve it in the anhydrous ethanol solution of P123, stir for 4h, add 2.5g Mg(NO3)2·6H2O and 0.4g Ce(NO3)3·6H2O, dry for 48h, heat to 400℃ at 1℃ / min, keep warm for 5h, then heat to 700℃ at 4℃ / min, keep warm for 2h, and prepare the magnesium aluminum composite oxide carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore size of the carrier are measured and the data are recorded in Table 2.
[0090] (2) Preparation of Catalyst
[0091] Weigh 0.530g of Ni(NO3)2·6H2O and dissolve it in 5ml of deionized water, stir and dissolve it, impregnate the impregnation liquid into 2g of the above-mentioned magnesium aluminum composite oxide and let it stand for 1h, then place it on a rotary evaporator for vacuum drying, and then place it in an oven for drying at 120℃ for 5h. The dried sample is then placed in a muffle furnace and calcined at 600℃ for 3h. The obtained catalyst is recorded as Ni / Mg-Al-Ce, and the composition of the catalyst is listed in Table 3. The dispersion of the active component of the catalyst measured by hydrogen chemical adsorption method is 17%, and the average particle size of the active component is 5.2nm.
[0092] (3) Catalyst evaluation
[0093] Weigh 0.1 g of Ni / Mg-Al-Ce catalyst, dilute it to 3 ml with quartz sand of 40-60 mesh, load it into a quartz tube reactor with an inner diameter of 8 mm, and reduce it at 700 ° C for 3 h in an atmosphere of hydrogen and nitrogen (1:1) under normal pressure. After the reduction is completed, heat it to 750 ° C in a hydrogen atmosphere, switch the raw gas (CH4 / CO2 / N2 molar ratio = 1.5:1.5:7) to react, and the reaction space velocity is 120000 ml g -1 ·h -1 , the reaction pressure is normal pressure. After the reaction is stable for 120h, the tail gas composition is analyzed by online gas chromatography. The calculation results are: XCH4 = 89.8%, XCO2 = 89.2%, H2 / CO = 1.19.
[0094] Example 3
[0095] (1) Preparation of catalyst carrier
[0096] Weigh 4g P123 and dissolve it in 80ml anhydrous ethanol, stir vigorously until P123 is completely dissolved, weigh 8g aluminum isopropoxide and 6ml concentrated nitric acid and dissolve it in the anhydrous ethanol solution of P123, stir for 4h, add 2.5g Mg(NO3)2·6H2O and 0.4g Ce(NO3)3·6H2O, dry for 48h, heat to 400℃ at 1℃ / min, keep warm for 5h, then heat to 1100℃ at 4℃ / min, keep warm for 2h, and prepare magnesium aluminum composite oxide carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore size of the carrier are measured and recorded in Table 2, and the composition of the catalyst is listed in Table 3.
[0097] (2) Preparation of Catalyst
[0098] Weigh 0.530g of Ni(NO3)2·6H2O and dissolve it in 5ml of deionized water, stir and dissolve it, and then immerse the impregnation liquid in 2g of the above-mentioned magnesium-aluminum composite oxide and let it stand for 1h, then place it on a rotary evaporator for vacuum drying, and then place it in an oven for drying at 120℃ for 5h. The dried sample is then placed in a muffle furnace and calcined at 600℃ for 3h. The obtained catalyst is recorded as Ni / Mg-Al-Ce. The dispersion of the catalyst active component measured by hydrogen chemical adsorption method is 12%, and the average particle size of the active component is 6.8nm.
[0099] (3) Catalyst evaluation
[0100] Weigh 0.1 g of Ni / Mg-Al-Ce catalyst, dilute it to 3 ml with quartz sand of 40-60 mesh, load it into a quartz tube reactor with an inner diameter of 8 mm, and reduce it at 700 ° C for 3 h in an atmosphere of hydrogen and nitrogen (1:1) under normal pressure. After the reduction is completed, heat it to 750 ° C in a hydrogen atmosphere, switch the raw gas (CH4 / CO2 / N2 molar ratio = 1.5:1.5:7) to react, and the reaction space velocity is 120000 ml g -1 ·h -1 , the reaction pressure is normal pressure. After the reaction is stable for 120h, the tail gas composition is analyzed by online gas chromatography. The calculation results are: XCH4 = 88.7%, XCO2 = 87.6%, H2 / CO = 1.18.
[0101] Example 4
[0102] The method of Example 1 was followed, except that 2.5 g of Mg(NO3)2·6H2O was replaced by 1.5 g of Mg(NO3)2·6H2O to prepare a carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the carrier were measured and recorded in Table 2. The obtained catalyst was recorded as Ni / Mg-Al-Ce, and the composition of the catalyst was listed in Table 3.
[0103] The catalyst was evaluated according to the catalyst evaluation method in Example 1. The dispersion of the catalyst active component measured by hydrogen chemical adsorption method was 18%, and the average particle size of the active component was 6.8 nm. After the reaction was stable for 120 hours, the tail gas composition was analyzed by online gas chromatography, and the calculation results showed that: XCH4 = 91.7%, XCO2 = 90.8%, H2 / CO = 1.13.
[0104] Example 5
[0105] The method of Example 1 was followed, except that 2.5 g of Mg(NO3)2·6H2O was replaced by 0.5 g of Mg(NO3)2·6H2O to prepare a carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the carrier were measured and recorded in Table 2. The obtained catalyst was recorded as Ni / Mg-Al-Ce, and the composition of the catalyst was listed in Table 3.
[0106] The catalyst was evaluated according to the evaluation method of Example 1. The dispersion of the active components of the catalyst measured by hydrogen chemical adsorption method was 17%, and the average particle size of the active components was 7.6 nm. After the reaction was stable for 120 hours, the tail gas composition was analyzed by online gas chromatography and calculated as follows: XCH4 = 91.4%, XCO2 = 90.4%, H2 / CO = 1.15.
[0107] Example 6
[0108] The method of Example 1 was followed, except that 2.5 g of Mg(NO3)2·6H2O was replaced by 5.5 g of Mg(NO3)2·6H2O to prepare a carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the carrier were measured and recorded in Table 2. The obtained catalyst was recorded as Ni / Mg-Al-Ce, and the composition of the catalyst was listed in Table 3.
[0109] The catalyst was evaluated according to the evaluation method of Example 1. The dispersion of the active components of the catalyst measured by hydrogen chemical adsorption method was 15%, and the average particle size of the active components was 8.7 nm. After the reaction was stable for 120 hours, the tail gas composition was analyzed by online gas chromatography and calculated as follows: XCH4 = 90.2%, XCO2 = 89.1%, H2 / CO = 1.19.
[0110] Example 7
[0111] The method of Example 1 was followed, except that 0.4 g of Ce(NO3)3·6H2O was replaced by 0.38 g of La(NO3)3·6H2O to prepare a carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the carrier were measured and recorded in Table 2. The obtained catalyst was recorded as Ni / Mg-Al-La, and the composition of the catalyst was listed in Table 3.
[0112] The catalyst was evaluated according to the evaluation method of Example 1. The dispersion of the active components of the catalyst measured by hydrogen chemical adsorption method was 17%, and the average particle size of the active components was 5.6 nm. After the reaction was stable for 120 hours, the tail gas composition was analyzed by online gas chromatography and calculated as follows: XCH4 = 91.2%, XCO2 = 90.3%, H2 / CO = 1.14.
[0113] Example 8
[0114] The method of Example 1 was followed, except that 0.4 g of Ce(NO3)3·6H2O was replaced by 0.53 g of Y(NO3)3·6H2O to prepare a carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the carrier were measured and recorded in Table 2. The obtained catalyst was recorded as Ni / Mg-Al-Y, and the composition of the catalyst was listed in Table 3.
[0115] The catalyst was evaluated according to the evaluation method of Example 1. The dispersion of the active components of the catalyst measured by hydrogen chemical adsorption method was 16%, and the average particle size of the active components was 5.9 nm. After the reaction was stable for 120 hours, the tail gas composition was analyzed by online gas chromatography and calculated as follows: XCH4 = 90.8%, XCO2 = 90.1%, H2 / CO = 1.15.
[0116] Example 9
[0117] The method of Example 1 was followed, except that 0.38 g of La(NO3)3·6H2O was added after 0.4 g of Ce(NO3)3·6H2O to prepare a carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the carrier were measured and recorded in Table 2. The obtained catalyst was recorded as Ni / Mg-Al-Ce-La, and the composition of the catalyst was listed in Table 3.
[0118] The catalyst was evaluated according to the evaluation method of Example 1. The dispersion of the active components of the catalyst measured by hydrogen chemical adsorption method was 21%, and the average particle size of the active components was 4.1 nm. After the reaction was stable for 120 hours, the tail gas composition was analyzed by online gas chromatography and calculated as follows: XCH4 = 92.8%, XCO2 = 91.8%, H2 / CO = 1.09.
[0119] Example 10
[0120] The method of Example 1 was followed, except that 0.53 g of Y(NO3)3·6H2O was added after 0.4 g of Ce(NO3)3·6H2O to prepare a carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the carrier were measured and recorded in Table 2. The obtained catalyst was recorded as Ni / Mg-Al-Ce-Y, and the composition of the catalyst was listed in Table 3.
[0121] The catalyst was evaluated according to the evaluation method of Example 1. The dispersion of the active components of the catalyst measured by hydrogen chemical adsorption method was 20%, and the average particle size of the active components was 4.3 nm. After the reaction was stable for 120 hours, the tail gas composition was analyzed by online gas chromatography and calculated as follows: XCH4 = 92.6%, XCO2 = 91.6%, H2 / CO = 1.10.
[0122] Embodiment 11
[0123] The method of Example 1 was followed, except that the calcination conditions were to raise the temperature to 900°C for 3 hours and keep the temperature for 3 hours to prepare a carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the carrier are measured and recorded in Table 2. The obtained catalyst is recorded as Ni / Mg-Al-Ce, and the composition of the catalyst is listed in Table 3.
[0124] The catalyst was evaluated according to the evaluation method of Example 1. The dispersion of the catalyst active component measured by hydrogen chemical adsorption method was 5.8%, and the average particle size of the active component was 24.7 nm. After the reaction was stable for 120 hours, the tail gas composition was analyzed by online gas chromatography, and the calculation results showed that: XCH4 = 55.4%, XCO2 = 52.9%, H2 / CO = 1.19.
[0125] Comparative Example 1
[0126] The method of Example 1 was followed, except that P123 was not used, to prepare a carrier. The composition of the carrier is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the carrier were measured and the data were recorded in Table 2. The prepared catalyst was recorded as Ni / Mg-Al-Ce, the composition of the catalyst was listed in Table 3, and the XRD spectrum was shown in Table 3. Figure 1 and Figure 2 .Depend on Figure 2 From the small-angle XRD spectrum, it can be seen that comparative example 1 has no diffraction peaks at 0.75° and 1.5°, so it does not have an ordered mesoporous structure.
[0127] The catalyst was evaluated according to the evaluation method of Example 1. The dispersion of the catalyst active component measured by hydrogen chemical adsorption method was 3.7%, and the average particle size of the active component was 28.1 nm. After the reaction was stable for 60 hours, the tail gas composition was analyzed by online gas chromatography and calculated as follows: XCH4 = 45.6%, XCO2 = 41.3%, H2 / CO = 1.20.
[0128] The stability evaluation results of the catalyst obtained in Comparative Example 1 are shown in Figure 4 , the specific reaction time is 60 hours of the catalytic methane dry reforming reaction performance. Figure 4 It can be seen that the reaction performance stability of the catalyst is poor.
[0129] Comparative Example 2
[0130] The method of Example 1 was followed, except that the magnesium oxide precursor was not added, to prepare a support. The composition of the support is listed in Table 1, and the specific surface area, pore volume and average pore diameter of the support were measured and the data were recorded in Table 2. The prepared catalyst was recorded as Ni / Al-Ce, and the composition of the catalyst was listed in Table 3.
[0131] The catalyst was evaluated according to the evaluation method of Example 1. The dispersion of the catalyst active component measured by hydrogen chemical adsorption method was 4.7%, and the average particle size of the active component was 26.1 nm. After the reaction was stable for 120 hours, the tail gas composition was analyzed by online gas chromatography, and the calculation results showed that: XCH4 = 52.4%, XCO2 = 49.9%, H2 / CO = 1.18.
[0132] Table 1 Composition of carrier
[0133] Carrier composition (weight %) Example 1 <![CDATA[5.1%Ce-79.3%Al2O3-15.6%MgO]]> Example 2 <![CDATA[5.1%Ce-79.3%Al2O3-15.6%MgO]]> Example 3 <![CDATA[5.1%Ce-79.3%Al2O3-15.6%MgO]]> Example 4 <![CDATA[5.5%Ce-84.5%Al2O3-10.0%MgO]]> Example 5 <![CDATA[5.9%Ce-90.5%Al2O3-4.6%MgO]]> Example 6 <![CDATA[4.3%Ce-66.8%Al2O3-28.9%MgO]]> Example 7 <![CDATA[4.9%La-79.5%Al2O3-15.6%MgO]]> Example 8 <![CDATA[4.9%Y-79.5%Al2O3-15.6%MgO]]> Example 9 <![CDATA[4.9%Ce-4.6%La-75.6%Al2O3-14.9%MgO]]> Example 10 <![CDATA[4.9%Ce-4.6%Y2O3-75.6%Al2O3-14.9%MgO]]> Embodiment 11 <![CDATA[5.1%Ce-79.3%Al2O3-15.6%MgO]]> Comparative Example 1 <![CDATA[5.1%Ce-79.3%Al2O3-15.6%MgO]]> Comparative Example 2 <![CDATA[6.1%Ce-93.9%Al2O3]]>
[0134] Table 2 Characteristic parameters of carrier
[0135]
[0136]
[0137] Table 3 Catalyst composition
[0138] Catalyst composition (weight %) Example 1 <![CDATA[5.0%Ni-4.9%CeO2-75.3%Al2O3-14.8%MgO]]> Example 2 <![CDATA[5.0%Ni-4.9%CeO2-75.3%Al2O3-14.8%MgO]]> Example 3 <![CDATA[5.0%Ni-4.9%CeO2-75.3%Al2O3-14.8%MgO]]> Example 4 <![CDATA[5.0%Ni-5.2%CeO2-80.2%Al2O3-9.6%MgO]]> Example 5 <![CDATA[5.0%Ni-5.6%CeO2-86.0%Al2O3-4.4%MgO]]> Example 6 <![CDATA[5.0%Ni-4.1%CeO2-63.4%Al2O3-27.5%MgO]]> Example 7 <![CDATA[5.0%Ni-4.7%La2O3-75.5%Al2O3-14.8%MgO]]> Example 8 <![CDATA[5.0%Ni-4.7%Y2O3-75.5%Al2O3-14.8%MgO]]> Example 9 <![CDATA[5.0%Ni-4.7%CeO2-4.6%La2O3-71.7%Al2O3-14.0%MgO]]> Example 10 <![CDATA[5.0%Ni-4.7%CeO2-4.6%Y2O3-71.7%Al2O3-14.0%MgO]]> Embodiment 11 <![CDATA[5.0%Ni-4.9%CeO2-75.3%Al2O3-14.8%MgO]]> Comparative Example 1 <![CDATA[5.0%Ni-4.9%CeO2-75.3%Al2O3-14.8%MgO]]> Comparative Example 2 <![CDATA[5.0%Ni-5.8%CeO2-89.2%Al2O3]]>
[0139] It can be seen from the data of the above embodiments and the data in Table 2 that the carrier provided by the present invention has a larger specific surface area, and the active metal loaded on these carriers can obtain a higher active metal dispersion, and the average particle size of the metal particles is also relatively small. Therefore, the prepared catalyst has better reaction activity and stability and anti-carbon deposition performance, and can operate continuously and stably for a long period of time.
[0140] By comparing Example 1 with Examples 2-8, it can be found that the optimal calcination temperature is 900°C, and the catalyst prepared using a single modification agent cerium has better performance; by comparing Example 9 with Example 10, it can be found that the catalyst prepared using a double modification agent of lanthanum and cerium has the best performance.
[0141] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A modified magnesium-aluminum composite oxide carrier, the carrier comprising magnesium-aluminum composite oxide and a modification aid, wherein the content of magnesium-aluminum composite oxide is 85-99.9% by weight, and the content of modification aid is 0.1-15% by weight based on the total amount of the carrier; the content of aluminum oxide is 60-99% by weight, and the content of magnesium oxide is 1-40% by weight based on the total amount of the magnesium-aluminum composite oxide; The modification aid is selected from at least one of rare earth metal oxides; The magnesium-aluminum composite oxide is an ordered mesoporous magnesium-aluminum spinel; The modified magnesium-aluminum composite oxide carrier is prepared by the following method: In the presence of a surfactant and a solvent, an acid, an aluminum oxide precursor, a magnesium oxide precursor and a modification aid precursor are mixed, and then dried and calcined.
2. The modified magnesium-aluminum composite oxide support according to claim 1, wherein Based on the total amount of the carrier, the content of the magnesium-aluminum composite oxide is 90-98% by weight, and the content of the modification aid is 2-10% by weight.
3. The modified magnesium-aluminum composite oxide support according to claim 2, wherein Based on the total amount of magnesium-aluminum composite oxide, the content of aluminum oxide is 69-97% by weight, and the content of magnesium oxide is 3-31% by weight.
4. The modified magnesium-aluminum composite oxide support according to any one of claims 1 to 3, wherein: The modification aid is selected from at least one of La2O3, CeO2 and Y2O3.
5. The modified magnesium-aluminum composite oxide support according to claim 4, wherein The modification aid is selected from La2O3 and CeO2.
6. The modified magnesium-aluminum composite oxide support according to claim 5, wherein The mass ratio of CeO2 and La2O3 is 0.1-4:
1.
7. The modified magnesium-aluminum composite oxide support according to claim 6, wherein The mass ratio of CeO2 and La2O3 is 0.1-2:
1.
8. The modified magnesium-aluminum composite oxide support according to any one of claims 1 to 3, wherein: The specific surface area of the carrier is 3-250m 2 / g, pore volume is 0.2-0.7cm 3 / g, and the average pore size is 9-25nm.
9. A method for preparing a modified magnesium-aluminum composite oxide carrier, the method comprising: In the presence of a surfactant and a solvent, an acid, an aluminum oxide precursor, a magnesium oxide precursor and a modification aid precursor are mixed, and then dried and calcined; The modification aid is selected from at least one of rare earth metal oxides; The amounts of the aluminum oxide precursor, magnesium oxide precursor and modification aid precursor are such that in the prepared modified magnesium aluminum composite oxide carrier, based on the total amount of the carrier, the content of magnesium aluminum composite oxide is 85-99.9% by weight, and the content of the modification aid is 0.1-15% by weight; based on the total amount of the magnesium aluminum composite oxide, the content of aluminum oxide is 60-99% by weight, and the content of magnesium oxide is 1-40% by weight.
10. The preparation method according to claim 9, wherein: The amounts of the aluminum oxide precursor, magnesium oxide precursor and modification aid precursor are such that in the prepared modified magnesium aluminum composite oxide carrier, based on the total amount of the carrier, the content of magnesium aluminum composite oxide is 90-98% by weight, and the content of the modification aid is 2-10% by weight; based on the total amount of the magnesium aluminum composite oxide, the content of aluminum oxide is 69-97% by weight, and the content of magnesium oxide is 3-31% by weight.
11. The preparation method according to claim 10, wherein: The modification aid is selected from at least one of La2O3, CeO2 and Y2O3.
12. The preparation method according to claim 11, wherein: The modification aids are La2O3 and CeO2.
13. The preparation method according to claim 12, wherein: The mass ratio of CeO2 and La2O3 is 0.1-2:
1.
14. The preparation method according to claim 13, wherein: The mass ratio of CeO2 and La2O3 is 0.1-4:
1.
15. The preparation method according to claim 9, wherein: The mixing comprises the following steps: (1) first mixing a surfactant, a solvent, an acid and an alumina precursor; (2) Adding a magnesium oxide precursor and a modification aid precursor to the first mixed material.
16. The preparation method according to claim 15, wherein: The first mixing is performed under stirring conditions.
17. The preparation method according to claim 15, wherein: The first mixing time is 2-10 hours.
18. The preparation method according to claim 17, wherein: The first mixing time is 4-6 hours.
19. The preparation method according to any one of claims 9 to 18, wherein: The surfactant is selected from at least one of P123, F127 and CTAB.
20. The preparation method according to claim 19, wherein: The surfactant is P123.
21. The preparation method according to any one of claims 9 to 18, wherein: The acid is at least one of nitric acid, sulfuric acid and hydrochloric acid.
22. The preparation method according to claim 21, wherein The acid is nitric acid.
23. The preparation method according to any one of claims 9 to 18, wherein: The solvent is selected from at least one of ethanol, H2O and methanol.
24. The preparation method according to claim 23, wherein: The solvent is ethanol.
25. The preparation method according to any one of claims 9 to 18, wherein: The aluminum oxide precursor is aluminum isopropoxide and / or aluminum nitrate.
26. The preparation method according to claim 25, wherein: The aluminum oxide precursor is aluminum isopropoxide.
27. The preparation method according to claim 26, wherein: The magnesium oxide precursor is magnesium nitrate and / or magnesium chloride.
28. The preparation method according to claim 27, wherein The magnesium oxide precursor is magnesium nitrate and / or magnesium chloride.
29. The preparation method according to any one of claims 9 to 18, wherein: The molar ratio of the surfactant to the aluminum oxide precursor calculated as the aluminum element is 0.005-0.05:
1.
30. The preparation method according to claim 29, wherein: The molar ratio of the surfactant to the aluminum oxide precursor calculated as the aluminum element is 0.01-0.03:
1.
31. The preparation method according to claim 30, wherein: The molar ratio of the surfactant to the aluminum oxide precursor calculated as the aluminum element is 0.015-0.025:
1.
32. The preparation method according to any one of claims 9 to 18, wherein: The molar ratio of the acid to the aluminum oxide precursor calculated as the aluminum element is 1-5:
1.
33. The preparation method according to claim 32, wherein: The molar ratio of the acid to the aluminum oxide precursor calculated as aluminum element is 1.5-3:
1.
34. The preparation method according to claim 33, wherein: The molar ratio of the acid to the aluminum oxide precursor calculated as aluminum element is 1.95-2.45:
1.
35. The preparation method according to any one of claims 9 to 18, wherein: The molar ratio of the solvent to the aluminum oxide precursor calculated as aluminum element is 30-40:
1.
36. The preparation method according to claim 35, wherein: The molar ratio of the solvent to the aluminum oxide precursor calculated as aluminum element is 32-37:
1.
37. The preparation method according to claim 36, wherein The molar ratio of the solvent to the aluminum oxide precursor calculated as the aluminum element is 34.5-36.5:
1.
38. The preparation method according to any one of claims 9 to 18, wherein: The target calcination temperature is 600-1200°C, and the target calcination time is 6-18 hours.
39. The preparation method according to claim 38, wherein The target calcination temperature is 700-1100°C, and the target calcination time is 10-16 hours.
40. The preparation method according to claim 38, wherein The calcination comprises: heating to 350-450° C. at a heating rate of 0.8-1.2° C. / min, keeping the temperature for 2-8 hours, and then heating to a target calcination temperature of 600-1200° C. at a heating rate of 1-5° C. / min.
41. The preparation method according to claim 40, wherein The calcination comprises: heating to 350-450° C. at a heating rate of 0.8-1.2° C. / min, keeping the temperature for 3-5 hours, and then heating to a target calcination temperature of 700-1100° C. at a heating rate of 1-5° C. / min.
42. A catalyst for producing synthesis gas by dry reforming of methane, the catalyst comprising a carrier and an active component, the carrier being a modified magnesium-aluminum composite oxide carrier as described in any one of claims 1 to 8 or a modified magnesium-aluminum composite oxide carrier prepared by the preparation method as described in any one of claims 9 to 41.
43. The catalyst according to claim 42, wherein The active component is selected from at least one of Ni, Co, Fe and precious metals.
44. The catalyst according to claim 43, wherein The active component is Ni.
45. The catalyst according to any one of claims 42 to 44, wherein Based on the total amount of the catalyst, the content of the active component is 2-10% by weight in terms of element count.
46. The catalyst according to any one of claims 42 to 44, wherein The dispersion of the active components measured by hydrogen chemical adsorption method is 4-28%, and the average particle size of the active components is 2-14 nm.
47. The catalyst according to any one of claims 42 to 44, wherein The dispersion of the active components measured by hydrogen chemical adsorption method is 12-23%; the average particle size of the active components is 4-9 nm.
48. A method for preparing synthesis gas by dry reforming of methane, the method comprising: Under conditions of methane dry reforming to produce synthesis gas, methane and carbon dioxide are contacted with a catalyst, wherein the catalyst is the catalyst for methane dry reforming to produce synthesis gas as described in any one of claims 42 to 47.
49. The method of claim 48, wherein: The conditions for producing synthesis gas by dry reforming of methane include: the molar ratio of carbon dioxide to methane is 1-1.2:1, the reaction temperature is 600-850℃, the pressure is 0-3MPa, and the total space velocity of the raw gas is 2000-120000mL•g -1 •h -1 .
50. The method of claim 49, wherein: The conditions for producing synthesis gas by dry reforming of methane include: the molar ratio of carbon dioxide to methane is 1-1.1:1; the reaction temperature is 650-800℃; the pressure is 0-1MPa; the total space velocity of the raw gas is 60000-120000mL•g -1 •h -1 .