Battery-grade manganese phosphate and preparation method thereof, and lithium iron manganese phosphate positive electrode material

By subjecting feed-grade manganese sulfate to a secondary calcium removal treatment using dispersants and glycerol phosphate, the problem of removing calcium impurities in manganese phosphate is solved, the preparation of high-purity and high-yield manganese phosphate is achieved, and filtration difficulties and fluoride ions are avoided. The introduction reduces costs and meets the purity and yield requirements of battery materials.

CN116022761BActive Publication Date: 2024-10-18FOSHAN DYNANONIC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310164165.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-10-18
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

Existing technology is difficult to effectively remove calcium impurities in manganese phosphate, resulting in reduced battery capacity and poor electrochemical performance. In addition, poor filtration performance and the introduction of fluoride ions affect the reaction device.

Method used

By using feed-grade manganese sulfate as raw material, using dispersants and chemicals such as glyceryl phosphate for secondary calcium removal, calcium glycerophosphate is generated and slightly soluble in cold water, and combined with co-solvents to improve solubility, the preparation of high-purity manganese phosphate is achieved. Filtration difficulties and the introduction of fluoride ions are avoided.

Benefits of technology

The preparation of manganese phosphate with high purity (≥99.5%) and high yield (≥98%) is achieved. The calcium content is less than 50ppm, which meets the requirements of battery materials, avoids the problems of difficult filtration and introduction of fluoride ions, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004095302980000121
    Figure BDA0004095302980000121
  • Figure BDA0004095302980000171
    Figure BDA0004095302980000171
  • Figure BDA0004095302980000172
    Figure BDA0004095302980000172
Patent Text Reader

Abstract

The present invention relates to the technical field of preparation of manganese phosphate, and in particular to battery-grade manganese phosphate and its preparation method, and manganese iron phosphate lithium positive electrode material. The preparation method of battery-grade manganese phosphate comprises the following steps: (a) adding solution A and solution B to solution C in parallel for reaction, and collecting a solid crude product; (b) collecting a solid manganese phosphate product after mixing the solid crude product with solution D; the solution A is mainly prepared by mixing a dispersant, water and manganese sulfate raw materials; the solution B is mainly prepared by mixing (NH4)2HPO4, ammonia water, a dispersant and water; the solution C is mainly prepared by mixing a dispersant and water; the solution D is mainly prepared by mixing glycerophosphate, a cosolvent and water. The present invention can use feed-grade manganese sulfate as a raw material to obtain a manganese phosphate that meets the production requirements of battery materials with a yield of more than 98%, a calcium content of less than 50ppm, and a product purity of 99.5%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of preparation of manganese phosphate, and in particular to a battery-grade manganese phosphate and a preparation method thereof, and a lithium iron manganese phosphate positive electrode material. Background Art

[0002] With the rise of the new energy industry, the market demand for lithium iron manganese phosphate positive electrode materials continues to increase, and the price of its raw materials has also risen with market demand. Therefore, it is imperative to use low-cost raw materials to prepare high-quality positive electrode material raw materials.

[0003] In addition, as lithium-ion batteries have higher and higher requirements for the impurity content of raw materials, the content of each impurity is limited to a very low level. Since the relative atomic mass of calcium itself is higher than that of lithium, if the lithium iron phosphate positive electrode material contains a high amount of calcium, the calcium will exist in the form of calcium phosphate, without active Ca 2+ Replaced Li + , resulting in a decrease in battery capacity and a decrease in gram capacity. A small amount of calcium doping has the effect of increasing the cycle capacity, but too high a calcium content will lead to a low capacity of the entire battery. Since the radius of calcium ions is larger than that of lithium ions, this not only affects their transport in the electrode, but also easily causes some irreversible damage to the structure of the electrode material, leading to poor electrochemical performance.

[0004] At present, the industry usually uses chemical precipitation to remove calcium from manganese sulfate systems. By adding fluorides (such as sodium fluoride, ammonium fluoride, manganese fluoride, etc.) to react with calcium ions to form CaF2 precipitates, deep removal of calcium from manganese sulfate can be achieved; however, the resulting CaF2 precipitate has a small particle size, is difficult to settle, and has poor filtration performance, and will also introduce fluoride ions, which places higher requirements on the material of the reaction device. In order to improve the filtration performance, the researchers tried to improve its filtration performance by adding an appropriate amount of aluminum sulfate as a flocculant for CaF2, but the effect was not obvious, and aluminum ion impurities were also introduced.

[0005] Therefore, developing a process for preparing high-quality manganese phosphate, the raw material for positive electrode materials, using low-cost raw materials and ensuring that the calcium content meets industry requirements is of great significance for the development of lithium-powered batteries.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] One object of the present invention is to provide a method for preparing battery-grade manganese phosphate, which uses feed-grade manganese sulfate as a raw material and is treated by a certain process to achieve the effect of removing calcium impurities. The purity of the obtained manganese phosphate can meet industry requirements and the yield is high. In addition, the method does not require the introduction of fluoride ions and does not have the problem of filtration difficulty.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] A method for preparing battery-grade manganese phosphate comprises the following steps:

[0010] (a) adding solution A and solution B to solution C in parallel for reaction, and collecting the solid crude product;

[0011] (b) after the solid crude product is mixed with solution D, the solid manganese phosphate product is collected;

[0012] The solution A is mainly prepared by mixing a dispersant, water and a manganese sulfate raw material;

[0013] The solution B is mainly prepared by mixing (NH4)2HPO4, ammonia water, a dispersant and water;

[0014] The solution C is mainly prepared by mixing a dispersant and water;

[0015] The solution D is mainly prepared by mixing glycerophosphate, a co-solvent and water.

[0016] In a specific embodiment of the present invention, the manganese sulfate raw material includes feed-grade manganese sulfate monohydrate; the calcium content w(Ca) in the manganese sulfate raw material is ≤3000ppm.

[0017] In a specific embodiment of the present invention, the manganese phosphate product has a purity of ≥99.5% and a calcium content w(Ca) of <50ppm.

[0018] In a specific embodiment of the present invention, the concentrations of the dispersants in the solution A, the solution B and the solution C are the same.

[0019] In a specific embodiment of the present invention, in the solution A, the solution B and the solution C, the concentration of the dispersant is 10 to 50 mg / L.

[0020] In a specific embodiment of the present invention, the dispersant includes at least one of MA / AA, HDTMPA, AA / HPA, AA / AMPS and PASP.

[0021] In a specific embodiment of the present invention, the co-solvent includes at least one of an organic acid and a salt thereof. Further, the co-solvent includes at least one of ammonium citrate, tartaric acid, citric acid and lactic acid.

[0022] In a specific embodiment of the present invention, in the solution A, the concentration of manganese sulfate is 1-1.5 mol / L.

[0023] In a specific embodiment of the present invention, in the solution B, the concentration of (NH4)2HPO4 is 1 to 2 mol / L.

[0024] In a specific embodiment of the present invention, based on the Mn in the solution A and the P in the solution B, the mass ratio of Mn / P in the solution A and the solution B is 2.2 to 2.66.

[0025] In a specific embodiment of the present invention, the amount of ammonia water in the solution B (calculated as ammonia water solution) is 25% to 30% of the mass of the manganese sulfate raw material.

[0026] In a specific embodiment of the present invention, the volume ratio of the solution B to the solution C is 3:(1-2).

[0027] In a specific embodiment of the present invention, in step (a), the reaction temperature is 40-50°C.

[0028] In a specific embodiment of the present invention, in step (a), the time for adding the solution A and the solution B in parallel is 30 to 60 minutes. Further, after the addition is completed, the reaction is continued for 10 to 20 minutes.

[0029] In a specific embodiment of the present invention, in step (a), collecting the crude solid product comprises: filtering the material obtained after the reaction, and then washing the filter cake.

[0030] In a specific embodiment of the present invention, in the solution D, the mass concentration of the glycerophosphate is 5% to 20%, and the mass concentration of the cosolvent is 0.5% to 1.5%. If the concentration and amount of the added glycerophosphate are high, the viscosity of the solution D will be high, and it will be difficult to separate, and the cost will also increase accordingly.

[0031] In a specific embodiment of the present invention, in step (b), the mass ratio of the solid crude product to the solution D is 1:(5-10).

[0032] In a specific embodiment of the present invention, in step (b), the temperature of the mixing treatment is 10 to 30° C.; and the time of the mixing treatment is 20 to 60 minutes.

[0033] In a specific embodiment of the present invention, in step (b), collecting the solid manganese phosphate product includes: filtering the mixed material and then washing the filter cake.

[0034] In a specific embodiment of the present invention, step (b) further comprises: collecting the filtrate after the mixing treatment, heating and boiling it, filtering it while hot, and collecting the filtrate for recycling.

[0035] Another object of the present invention is to provide a battery-grade manganese phosphate prepared according to any one of the above-mentioned methods for preparing battery-grade manganese phosphate.

[0036] Another object of the present invention is to provide a lithium iron manganese phosphate positive electrode material, which is mainly made from the battery-grade manganese phosphate prepared by any of the above methods, or mainly made from any of the above-mentioned battery-grade manganese phosphates.

[0037] Compared with the prior art, the present invention has the following beneficial effects:

[0038] The preparation method of battery-grade manganese phosphate of the present invention comprises the following steps: adding solution A and solution B to solution C in parallel for reaction, using a dispersant to reduce the particle size of calcium phosphate particles and disperse them, so that the calcium phosphate precipitate can be separated from the product by filtering, washing and other treatments during the filtration process. Then, the crude product is mixed with solution D, and glycerophosphate is reacted with calcium phosphate to generate glycerophosphate calcium, which is slightly soluble in cold water, and a cosolvent is used to appropriately increase the solubility of glycerophosphate calcium to further reduce the calcium content. By performing a secondary decalcification treatment on the process of preparing manganese phosphate from manganese sulfate, manganese phosphate that meets the production requirements of battery materials and has a yield of more than 98%, a calcium content of less than 50 ppm, and a product purity of 99.5% can be obtained using feed-grade manganese sulfate as a raw material. DETAILED DESCRIPTION

[0039] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but it will be appreciated by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work, all belong to the scope of protection of the present invention. If specific conditions are not indicated in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0040] A method for preparing battery-grade manganese phosphate comprises the following steps:

[0041] (a) adding solution A and solution B to solution C in parallel for reaction, and collecting the solid crude product;

[0042] (b) after the solid crude product is mixed with solution D, the solid manganese phosphate product is collected;

[0043] The solution A is mainly prepared by mixing a dispersant, water and a manganese sulfate raw material;

[0044] The solution B is mainly prepared by mixing (NH4)2HPO4, ammonia water, a dispersant and water;

[0045] The solution C is mainly prepared by mixing a dispersant and water;

[0046] The solution D is mainly prepared by mixing glycerophosphate, a co-solvent and water.

[0047] The preparation method of battery-grade manganese phosphate of the present invention comprises the following steps: adding solution A and solution B to solution C in parallel for reaction, using a dispersant to reduce the particle size of calcium phosphate particles and disperse them, so that the calcium phosphate precipitate can be separated from the product by filtering, washing and other treatments during the filtration process. Then, the crude product is mixed with solution D, and glycerophosphate is reacted with calcium phosphate to generate glycerophosphate calcium, which is slightly soluble in cold water, and a cosolvent is used to appropriately increase the solubility of glycerophosphate calcium to further reduce the calcium content. By performing a secondary decalcification treatment on the process of preparing manganese phosphate from manganese sulfate, manganese phosphate that meets the production requirements of battery materials and has a yield of more than 98%, a calcium content of less than 50 ppm, and a product purity of 99.5% can be obtained using feed-grade manganese sulfate as a raw material.

[0048] Furthermore, the present invention can make the precipitate generated by the reaction more uniform by adding the precipitate into another solution in parallel, thereby avoiding the phenomenon of wrapping and local over-concentration.

[0049] In a specific embodiment of the present invention, the preparation of the solution A comprises: mixing a dispersant and water to obtain an aqueous solution of the dispersant; then dissolving a manganese sulfate monohydrate raw material in the aqueous solution of the dispersant, filtering, and collecting the filtrate. In the process of preparing the solution A, the manganese sulfate monohydrate raw material is dissolved in the aqueous solution of the dispersant, and the insoluble impurities are initially removed by filtering to obtain a clear solution A containing manganese sulfate.

[0050] In a specific embodiment of the present invention, the preparation of the solution B includes: mixing (NH4)2HPO4, ammonia water, a dispersant and water in proportion, and mixing well to obtain the solution B.

[0051] In a specific embodiment of the present invention, the preparation of the solution C includes: mixing a dispersant and water in proportion, and mixing well to obtain the solution C.

[0052] In a specific embodiment of the present invention, the preparation of the solution D comprises: mixing glycerophosphate, a cosolvent and water in proportion, and mixing well to obtain the solution D.

[0053] In a specific embodiment of the present invention, the manganese sulfate raw material includes feed-grade manganese sulfate; the calcium content w(Ca) in the manganese sulfate raw material is ≤3000ppm.

[0054] For example, in different embodiments, the calcium content w (Ca) in the feed-grade manganese sulfate monohydrate raw material used in the present invention can be 3000ppm, 2800ppm, 2500ppm, 2200ppm, 2000ppm, etc. When feed-grade manganese sulfate monohydrate with a relatively high calcium content is used as a raw material, the calcium content in the manganese phosphate product obtained after treatment can still be less than 50ppm, meeting the requirements of battery-grade manganese phosphate.

[0055] In a specific embodiment of the present invention, the manganese phosphate product has a purity of ≥99.5% and a calcium content w(Ca) of <50ppm.

[0056] As in a specific embodiment, in the manganese phosphate product, the calcium content w (Ca) can be illustratively 48ppm, 45ppm, 42ppm, 40ppm, 38ppm, 35ppm, 32ppm, 30ppm, 28ppm, 25ppm, 22ppm, 20ppm, 18ppm, 15ppm, 12ppm, 10ppm, 5ppm, etc.

[0057] In a specific embodiment of the present invention, the concentration of the dispersant in the solution A, the solution B and the solution C is the same.

[0058] In actual operation, when the concentrations of the dispersants in the solution A, the solution B and the solution C are the same, during the parallel feeding process, it can be ensured that the concentration of the dispersant does not change due to volume changes, which can further ensure the stability of the reaction process, so that the particle size of the calcium phosphate particles in the system is uniform and small without affecting the manganese phosphate. During the filtration process, the calcium phosphate can pass through the filter medium (such as filter paper / filter membrane, etc.), while the manganese phosphate does not pass through the filter medium, thereby ensuring that the calcium phosphate precipitate is separated from the crude product through filtration and washing during the filtration process.

[0059] In a specific embodiment of the present invention, in the solution A, the solution B and the solution C, the concentration of the dispersant is 10 to 50 mg / L.

[0060] For example, in different embodiments, the concentration of the dispersant in the solution A, the solution B and the solution C may be independently 10 mg / L, 15 mg / L, 20 mg / L, 25 mg / L, 30 mg / L, 35 mg / L, 40 mg / L, 45 mg / L, 50 mg / L, etc.

[0061] In a specific embodiment of the present invention, the dispersant includes at least one of MA / AA, HDTMPA, AA / HPA, AA / AMPS and PASP. Among them, MA / AA refers to a low molecular weight polyelectrolyte obtained by copolymerization of maleic acid and acrylic acid in a certain ratio; HDTMPA is hexamethylenediaminetetramethylenephosphonic acid; AA / HPA is acrylic acid-hydroxypropyl acrylate copolymer; AA / AMPS is a copolymer of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid; PASP is polyaspartic acid (sodium).

[0062] In a specific embodiment of the present invention, the co-solvent includes at least one of an organic acid and a salt thereof. Further, the co-solvent includes at least one of ammonium citrate, tartaric acid, citric acid and lactic acid.

[0063] In a specific embodiment of the present invention, in the solution A, the concentration of manganese sulfate is 1-1.5 mol / L.

[0064] For example, in different embodiments, in the solution A, the concentration of manganese sulfate can be illustratively 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.5 mol / L, etc.

[0065] In a specific embodiment of the present invention, in the solution B, the concentration of (NH4)2HPO4 is 1 to 2 mol / L, such as 1.5 mol / L.

[0066] For example, in different embodiments, in the solution B, the concentration of (NH4)2HPO4 can be illustratively 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.5 mol / L, 1.6 mol / L, 1.8 mol / L, 2 mol / L, etc.

[0067] In a specific embodiment of the present invention, based on the Mn in the solution A and the P in the solution B, the mass ratio of Mn / P in the solution A and the solution B is 2.2 to 2.66.

[0068] The mass ratio is within the above range, which ensures that manganese phosphate is completely generated and the cost is appropriate. When the mass ratio is too large, manganese phosphate is not completely generated; when the mass ratio is too small, although manganese phosphate can be completely generated, the dosage of the reagent is excessive, the cost is too high, and it is not economically efficient.

[0069] The manganese sulfate and (NH4)2HPO4 in the solution A and the solution B are calculated as Mn and P, respectively, and the Mn / P mass ratio of the two can be exemplified as 2.2, 2.25, 2.3, 2.35, 2.4, 2.45, 2.5, 2.55, 2.6, 2.65, 2.66, etc.

[0070] In a specific embodiment of the present invention, the amount of ammonia water in the solution B (calculated as ammonia water solution) is 25% to 30% of the mass of the manganese sulfate raw material, wherein the mass fraction of ammonia water solution is 25% to 28%.

[0071] For example, in different embodiments, the amount of ammonia water in the solution B can be illustratively 25%, 26%, 27%, 28%, 29%, 30%, etc., of the mass of the manganese sulfate raw material.

[0072] In a specific embodiment of the present invention, the volume ratio of the solution B to the solution C is 3:(1-2).

[0073] For example, in different embodiments, the volume ratio of the solution B to the solution C can be exemplified as 3:1, 3:1.2, 3:1.5, 3:1.8, 3:2, etc.

[0074] In a specific embodiment of the present invention, in step (a), the reaction temperature is 40-50°C.

[0075] In actual operation, the temperature of solution C is first adjusted to maintain at 40-50°C, and then solution A and solution B are added in parallel. During the addition process, the temperature of solution C is controlled to maintain at 40-50°C until the reaction is completed. When solution A and solution B are added in parallel, stirring is performed. Solution A and solution B can be added dropwise.

[0076] In a specific embodiment of the present invention, in step (a), the time for adding the solution A and the solution B in parallel is 30 to 60 minutes. Further, after the addition is completed, the reaction is continued for 10 to 20 minutes.

[0077] For example, in different embodiments, the feeding time may be illustratively 30 min, 35 min, 40 min, 45 min, 50 min, 55 min, 60 min, etc.

[0078] The addition time is regulated within the above range to further improve the uniformity of the reaction; after the addition is completed, the reaction is continued for a period of time to make the reaction more complete.

[0079] In a specific embodiment of the present invention, in step (a), collecting the solid crude product includes: filtering the reacted material, and then washing the filter cake with water to obtain a solid crude product, namely crude manganese phosphate. The filter cake can be washed with deionized water in small amounts and multiple times. The residual liquid and fine calcium phosphate precipitates attached to the surface of the manganese phosphate are washed away by washing with deionized water in small amounts and multiple times.

[0080] In a specific embodiment of the present invention, in the solution D, the mass concentration of the glycerophosphate is 5% to 20%, and the mass concentration of the co-solvent is 0.5% to 1.5%.

[0081] For example, in different embodiments, in the solution D, the mass concentration of the glycerophosphate can be exemplarily 5%, 6%, 8%, 10%, 12%, 14%, 15%, 16%, 18%, 20%, etc.; the mass concentration of the co-solvent can be exemplarily 0.5%, 0.6%, 0.8%, 1%, 1.2%, 1.4%, 1.5%, etc.

[0082] By using the solution D with the above ratio, it is further ensured that the calcium phosphate in the crude manganese phosphate is converted into glycerophosphate, and the glycerophosphate is dissolved in water and separated from the manganese phosphate, thereby achieving the effect of calcium removal.

[0083] In a specific embodiment of the present invention, in step (b), the mass ratio of the solid crude product to the solution D is 1:(5-10).

[0084] For example, in different embodiments, the mass ratio of the solid crude product to the solution D can be exemplified as 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, etc.

[0085] In order to convert calcium phosphate in the crude manganese phosphate product into calcium glycerophosphate as much as possible, the amount of glycerophosphate ester needs to be excessive. However, the actual consumption of glycerophosphate ester is in a molar ratio with calcium ions, and the remaining glycerophosphate ester can be recycled, so the overall cost is low.

[0086] In a specific embodiment of the present invention, in step (b), the temperature of the mixing treatment is 10 to 30° C.; and the time of the mixing treatment is 20 to 60 minutes.

[0087] For example, in different embodiments, the temperature of the mixing treatment can be exemplified as 10°C, 15°C, 20°C, 25°C, 30°C, etc.; the time of the mixing treatment can be exemplified as 20min, 25min, 30min, 35min, 40min, 45min, 50min, 55min, 60min, etc.

[0088] In actual operation, in step (b), the mixing process can be carried out at room temperature.

[0089] In a specific embodiment of the present invention, in step (b), collecting the solid manganese phosphate product includes: filtering the mixed material, and then washing the filter cake with water to obtain the solid manganese phosphate product. The filter cake can be washed with deionized water in small amounts and multiple times to rinse the residual liquid attached to the surface of the manganese phosphate.

[0090] In actual operation, the solid manganese phosphate product collected after washing is dried to obtain battery-grade manganese phosphate, wherein the drying temperature can be adjusted according to actual conditions, such as 60-70°C.

[0091] In a specific embodiment of the present invention, step (b) further comprises: collecting the filtrate after the mixing treatment, heating and boiling it, filtering it while hot, and collecting the filtrate for recycling.

[0092] Glycerol phosphate can react with calcium phosphate to form glycerol calcium phosphate. Glycerol calcium phosphate is slightly soluble in cold water. Adding a small amount of cosolvent can increase the solubility of glycerol calcium phosphate. As the temperature rises, the solubility of glycerol calcium phosphate decreases. At 100°C, glycerol calcium phosphate is almost completely precipitated. The treated filtrate is heated and boiled to precipitate glycerol calcium phosphate. After hot filtration, the glycerol phosphate ester solution after calcium separation can be obtained, which can be recycled to reduce costs.

[0093] The present invention also provides a battery-grade manganese phosphate, which is prepared according to any one of the above-mentioned methods for preparing the battery-grade manganese phosphate.

[0094] The present invention also provides a lithium iron manganese phosphate positive electrode material, which is mainly prepared from the battery-grade manganese phosphate prepared by any one of the above methods, or is mainly prepared from any one of the above battery-grade manganese phosphates.

[0095] Example 1

[0096] This embodiment provides a method for preparing battery-grade manganese phosphate, comprising the following steps:

[0097] (1) Weigh 15.76 mg of dispersant AA / AMPS, dissolve it in deionized water, and dilute it to 1000 mL to obtain an aqueous solution of the dispersant; weigh 100 g of feed-grade manganese sulfate monohydrate raw material, then take 250 mL of the aqueous solution of the dispersant to dissolve the feed-grade manganese sulfate monohydrate raw material, and then filter and collect the filtrate; add deionized water to the filtrate to dilute it to obtain a solution A with a manganese sulfate concentration of 1.5 mol / L and a dispersant concentration of 10 mg / L.

[0098] (2) (NH4)2HPO4 was weighed according to the mass ratio of Mn to P in solution A being 2.66, and an ammonia solution (calculated as an ammonia solution) was weighed according to 25% of the mass of manganese sulfate in solution A. (NH4)2HPO4, ammonia solution and dispersant water were prepared to obtain 300 mL of solution B, in which the concentration of dispersant in solution B was 10 mg / L.

[0099] (3) Mixing the dispersant with water to prepare 100 mL of solution C with a dispersant concentration of 10 mg / L, and keeping the temperature at 40° C. Under stirring conditions, adding solution A and solution B in step (1) and step (2) in parallel, dropwise adding them into solution C, and controlling the adding time to be 30 min. After the adding is completed, the reaction is continued for 15 min, and the material is filtered and separated. The filter cake is washed with deionized water in small amounts for multiple times to obtain crude manganese phosphate.

[0100] (4) Glycerol phosphate, co-solvent ammonium citrate and water are mixed in proportion to obtain solution D, wherein the mass concentration of glycerol phosphate is 10% and the mass concentration of co-solvent is 1%. Then crude manganese phosphate is added to solution D, the mass ratio of crude manganese phosphate to solution D is 1:5, and the mixture is reacted at room temperature for 30 minutes; after the reaction, the material is filtered and separated, the filter cake is washed with deionized water in small amounts for multiple times, and then the filter cake is dried at 70°C to obtain battery-grade manganese phosphate. The filtrate obtained by filtration and separation is heated to boil and filtered while hot, and then the filtrate is collected and recycled.

[0101] The composition analysis of the feed-grade manganese sulfate raw material used in this example is shown in Table 1.

[0102] Table 1 Composition analysis of feed grade manganese sulfate raw materials

[0103]

[0104] Example 2

[0105] This embodiment provides a method for preparing battery-grade manganese phosphate, comprising the following steps:

[0106] (1) Weigh 39.4 mg of dispersant AA / HPA, dissolve it in deionized water and dilute it to 1000 mL to obtain an aqueous solution of the dispersant; weigh 100 g of feed-grade manganese sulfate monohydrate raw material, then take 250 mL of the aqueous solution of the dispersant to dissolve the feed-grade manganese sulfate monohydrate raw material, and then filter and collect the filtrate; add deionized water to the filtrate to dilute it to obtain a solution A with a manganese sulfate concentration of 1.5 mol / L and a dispersant concentration of 25 mg / L.

[0107] (2) (NH4)2HPO4 was weighed according to the mass ratio of Mn to P in solution A being 2.20, and ammonia water was weighed according to 30% of the mass of manganese sulfate in solution A. (NH4)2HPO4, ammonia water and dispersant water were prepared to obtain 300 mL of solution B, in which the concentration of dispersant in solution B was 25 mg / L.

[0108] (3) Mixing the dispersant with water to prepare 100 mL of solution C with a dispersant concentration of 25 mg / L, and keeping the temperature at 40° C. Under stirring conditions, adding solution A and solution B in step (1) and step (2) in parallel, dropwise adding them into solution C, and controlling the adding time to be 60 min. After the adding is completed, the reaction is continued for 15 min, and the material is filtered and separated. The filter cake is washed with deionized water in small amounts for multiple times to obtain crude manganese phosphate.

[0109] (4) Glycerol phosphate, co-solvent citric acid and water are mixed in proportion to obtain solution D, wherein the mass concentration of glycerol phosphate is 5% and the mass concentration of co-solvent is 1%. Then crude manganese phosphate is added to solution D, the mass ratio of crude manganese phosphate to solution D is 1:10, and the mixture is reacted at room temperature for 30 minutes; after the reaction, the material is filtered and separated, the filter cake is washed with deionized water in small amounts for multiple times, and then the filter cake is dried at 70°C to obtain battery-grade manganese phosphate. The filtrate obtained by filtration and separation is heated to boil and filtered while hot, and then the filtrate is collected and recycled.

[0110] The composition of the feed-grade manganese sulfate raw material used in this embodiment is the same as that in Example 1.

[0111] Example 3

[0112] This embodiment provides a method for preparing battery-grade manganese phosphate, comprising the following steps:

[0113] (1) Weigh 78.8 mg of a dispersant HDTMPA, dissolve it in deionized water, and dilute it to 1000 mL to obtain an aqueous solution of the dispersant; weigh 100 g of a feed-grade manganese sulfate monohydrate raw material, then take 250 mL of the aqueous solution of the dispersant to dissolve the feed-grade manganese sulfate monohydrate raw material, and then filter and collect the filtrate; add deionized water to the filtrate to dilute it to obtain a solution A with a manganese sulfate concentration of 1.5 mol / L and a dispersant concentration of 50 mg / L.

[0114] (2) (NH4)2HPO4 was weighed according to the mass ratio of Mn to P in solution A being 2.43, and ammonia water was weighed according to 28% of the mass of manganese sulfate in solution A. (NH4)2HPO4, ammonia water and dispersant water were prepared to obtain 300 mL of solution B, in which the concentration of dispersant in solution B was 50 mg / L.

[0115] (3) Mixing the dispersant with water to prepare 100 mL of solution C with a dispersant concentration of 50 mg / L, and keeping the temperature at 50° C. Under stirring conditions, adding solution A and solution B in step (1) and step (2) in parallel, dropwise adding them into solution C, and controlling the adding time to be 45 min. After the addition is completed, the reaction is continued for 15 min, and the material is filtered and separated. The filter cake is washed with deionized water in small amounts for multiple times to obtain crude manganese phosphate.

[0116] (4) Glycerol phosphate, co-solvent lactic acid and water are mixed in proportion to obtain solution D, wherein the mass concentration of glycerol phosphate is 20% and the mass concentration of co-solvent is 1.5%. Then crude manganese phosphate is added to solution D, the mass ratio of crude manganese phosphate to solution D is 1:8, and the mixture is reacted at room temperature for 30 minutes; after the reaction, the material is filtered and separated, the filter cake is washed with deionized water in small amounts for multiple times, and then the filter cake is dried at 70°C to obtain battery-grade manganese phosphate. The filtrate obtained by filtration and separation is heated to boil and filtered while hot, and then the filtrate is collected and recycled.

[0117] The composition of the feed-grade manganese sulfate raw material used in this embodiment is the same as that in Example 1.

[0118] Comparative Example 1

[0119] Comparative Example 1 refers to the preparation method of Example 1, except that the dispersant used in Example 1 is replaced by an equal mass of polyethylene glycol 4000.

[0120] Comparative Example 2

[0121] Comparative Example 2 refers to the preparation method of Example 1, except that the concentration of the dispersant in solution A, solution B and solution C is 8 mg / L, and the rest remains unchanged.

[0122] Comparative Example 3

[0123] Comparative Example 3 refers to the preparation method of Example 1, except that the concentration of the dispersant in solution A, solution B and solution C is 60 mg / L, and the rest remains unchanged.

[0124] Comparative Example 4

[0125] Comparative Example 4 The preparation method of Example 1 is referred to, except that in step (2), an ammonia solution is weighed according to 20% of the mass of manganese sulfate in solution A (calculated as ammonia solution).

[0126] Comparative Example 5

[0127] Comparative Example 5 The preparation method of Reference Example 1 is different only in that: in step (2), an ammonia solution is weighed according to 35% of the mass of manganese sulfate in solution A (calculated as ammonia solution).

[0128] Comparative Example 6

[0129] Comparative Example 6 refers to the preparation method of Example 1, with the only difference being that in the solution B prepared in step (2), the concentration of (NH4)2HPO4 is 2 mol / L.

[0130] Comparative Example 7

[0131] Comparative Example 7 refers to the preparation method of Example 1, except that in step (4), the mass concentration of glycerophosphate in solution D is 3%.

[0132] Comparative Example 8

[0133] Comparative Example 8 refers to the preparation method of Example 1, except that in step (4), the mass concentration of glycerophosphate in solution D is 25%.

[0134] Comparative Example 9

[0135] Comparative Example 9 refers to the preparation method of Example 1, except that in step (4), the mass concentration of the co-solvent in solution D is 2%.

[0136] Comparative Example 10

[0137] Comparative Example 10 provides a method for preparing manganese phosphate, comprising the following steps:

[0138] (1) Weigh 15.76 mg of dispersant AA / AMPS, dissolve it in deionized water, and dilute it to 1000 mL to obtain an aqueous solution of the dispersant; weigh 100 g of feed-grade manganese sulfate monohydrate raw material, then take 250 mL of the aqueous solution of the dispersant to dissolve the feed-grade manganese sulfate monohydrate raw material, and then filter and collect the filtrate; add deionized water to the filtrate to dilute it to obtain a solution A with a manganese sulfate concentration of 1.5 mol / L and a dispersant concentration of 10 mg / L.

[0139] (2) (NH4)2HPO4 was weighed according to the mass ratio of Mn to P in solution A being 2.66, and an ammonia solution (calculated as an ammonia solution) was weighed according to 25% of the mass of manganese sulfate in solution A. (NH4)2HPO4, ammonia solution and dispersant water were prepared to obtain 300 mL of solution B, in which the concentration of dispersant in solution B was 10 mg / L.

[0140] (3) Mixing the dispersant with water to prepare 100 mL of solution C with a dispersant concentration of 10 mg / L, and keeping the temperature at 40° C. Under stirring conditions, adding solution A and solution B in step (1) and step (2) in parallel, dropwise adding them into solution C, and controlling the adding time to be 30 min. After the adding is completed, the reaction is continued for 15 min, and the material is filtered and separated. The filter cake is washed with deionized water in small amounts for multiple times to obtain crude manganese phosphate.

[0141] The composition of the feed-grade manganese sulfate monohydrate raw material used in Comparative Example 10 is the same as that in Example 1.

[0142] Experimental Example 1

[0143] In order to compare and illustrate the differences in the components of the manganese phosphate products obtained in different embodiments and comparative examples, the components of the manganese phosphate products obtained in different embodiments and comparative examples were analyzed. The analysis results are shown in Table 2.

[0144] Table 2 Composition analysis of different manganese phosphate products

[0145]

[0146] Experimental Example 2

[0147] The purity of the manganese phosphate products obtained in different embodiments and comparative examples and the yield of the preparation method were tested and settled. The results are shown in Table 3.

[0148] The yield is calculated as follows:

[0149] η=M(manganese phosphate)*w2(Mn) / [M(feed grade manganese sulfate)*w1(Mn)].

[0150] Table 3 Purity and yield of different embodiments and comparative examples

[0151]

[0152]

[0153] From the above test results, it can be seen that the preparation method of battery-grade manganese phosphate of the present invention can use feed-grade manganese sulfate as raw material to obtain manganese phosphate with a yield of more than 98%, a calcium content of less than 50ppm, and a product purity of 99.5%, which meets the production requirements of battery materials. In addition, the method of the present invention does not require the pre-purification and removal of calcium in the manganese sulfate solution, and does not require the introduction of F - There is no difficulty in filtering and the problem that colloidal precipitation cannot be filtered, and the effect of removing calcium impurities can be achieved. The amount of reagents used is small, and it can be recycled, the overall cost is low, and it is easy to realize industrialization.

[0154] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing battery-grade manganese phosphate, characterized in that: The steps include: (a) adding solution A and solution B to solution C in parallel for reaction, and collecting the solid crude product; (b) after the solid crude product is mixed with solution D, the solid manganese phosphate product is collected; The solution A is mainly prepared by mixing a dispersant, water and a manganese sulfate raw material; The solution B is mainly prepared by mixing (NH4)2HPO4, ammonia water, a dispersant and water; The solution C is mainly prepared by mixing a dispersant and water; The solution D is mainly prepared by mixing glycerophosphate, a cosolvent and water; The manganese sulfate raw material includes feed-grade manganese sulfate; The dispersant includes at least one of a copolymer of maleic acid and acrylic acid, hexamethylenediaminetetramethylenephosphonic acid, an acrylic acid-hydroxypropyl acrylate copolymer, a copolymer of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid, and polyaspartic acid (sodium); The cosolvent comprises at least one of ammonium citrate, tartaric acid, citric acid and lactic acid; The calcium content w(Ca) in the manganese sulfate raw material is ≤3000ppm; The amount of ammonia water in the solution B is 25% to 30% of the mass of the manganese sulfate raw material; In step (a), collecting the crude solid product comprises filtering the material obtained after the reaction.

2. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: The manganese phosphate product has a purity of ≥99.5% and a calcium content w(Ca) of <50ppm.

3. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: The concentrations of the dispersants in the solution A, the solution B, and the solution C are the same.

4. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: In the solution A, the solution B and the solution C, the concentration of the dispersant is 10-50 mg / L.

5. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: It has at least one of the following technical features: (1) In the solution A, the concentration of manganese sulfate is 1-1.5 mol / L; (2) In the solution B, the concentration of (NH4)2HPO4 is 1-2 mol / L; (3) Based on the Mn in the solution A and the P in the solution B, the mass ratio of Mn / P in the solution A and the solution B is 2.2 to 2.66; (4) The volume ratio of the solution B to the solution C is 3:(1~2).

6. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: In step (a), the reaction temperature is 40-50°C.

7. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: In step (a), the time for adding the solution A and the solution B in parallel is 30 to 60 minutes.

8. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: In step (a), collecting the crude solid product comprises: filtering the material obtained after the reaction, and then washing the filter cake.

9. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: In the solution D, the mass concentration of the glycerophosphate is 5% to 20%.

10. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: The mass concentration of the co-solvent is 0.5% to 1.5%.

11. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: The mass ratio of the solid crude product to the solution D is 1:(5-10).

12. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: In step (b), the temperature of the mixing treatment is 10-30° C.; and the time of the mixing treatment is 20-60 min.

13. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: In step (b), collecting the solid manganese phosphate product includes filtering the mixed material and then washing the filter cake.

14. The method for preparing battery-grade manganese phosphate according to claim 1, characterized in that: Step (b) also includes: collecting the filtrate after the mixing treatment, heating and boiling it, filtering it while it is hot, and collecting the filtrate for recycling.

Citation Information

Patent Citations

  • Method for producing positive electrode active material for lithium ion secondary battery

    CN112689918A

  • Method for preparing co-precipitate, and method for producing lithium-containing compound oxide

    JP2015147689A