A biodegradable acetic acid propylene emulsion and preparation method thereof
By using biodegradable vinegar-acrylic emulsion in paper-making coatings, the problem that paper-making coatings in the existing technology are difficult to meet biodegradation performance requirements is solved, and the water resistance, chemical resistance and efficient biodegradability of paper-making coatings are achieved, meeting the requirements meet the requirements of relevant standards.
Patent Information
- Application Number
- CN202310012637.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-05
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-01-05
Smart Images

Figure BDA0004039583900000121 
Figure BDA0004039583900000131 
Figure BDA0004039583900000132
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of papermaking coatings, and in particular to a bio-based degradable acetic acid-acrylic acid emulsion and a preparation method thereof. Background Art
[0002] Paper coating refers to a viscous liquid coated on the surface of paper or paperboard and can form a continuous film that is firmly attached to the paper or paperboard. It is usually mainly resin, oil, or emulsion, with or without pigments and fillers, and with corresponding additives, and is prepared with organic solvents or water. Since the update of the requirements for paper biodegradability, there are not many paper coatings involving the field of biodegradability, so it is not easy for paper sprayed with paper coating to meet the biodegradability requirements of the standard "GB / T 19277.1-2011 Definition, Classification, Marking and Degradability Requirements for Degradable Plastics".
[0003] It can be seen that the existing technology still needs to be improved and enhanced. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a bio-based degradable vinyl acetate acrylic emulsion and a preparation method thereof, so as to make the papermaking coating containing the bio-based degradable vinyl acetate acrylic emulsion have the biodegradability specified in the current standards.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] A bio-based degradable vinyl acetate emulsion comprises the following components in parts by weight: 36-38 parts of vinyl acetate, 2-4 parts of acrylic acid, 0.5-1.5 parts of vinyl siloxane, 4-6 parts of polyvinyl alcohol, 3-4 parts of cellulose, 1.5-2.5 parts of inorganic silicate, 0.4-0.6 parts of emulsifier, 0.45 parts or 0.55 parts of oxidation initiator, 0.35 parts or 0.45 parts of reduction initiator, 1.5-2.5 parts of pH regulator and 45 parts of deionized water.
[0007] In the bio-based degradable acetic acid acrylic emulsion, the vinyl siloxane includes one or more of vinyl triethoxy silane, vinyl trimethoxy silane and vinyl tripropoxy silane.
[0008] In the bio-based degradable acetic acid propylene emulsion, the inorganic silicate is one of potassium methyl silicate, sodium methyl silicate and lithium methyl silicate.
[0009] In the bio-based degradable acetoacrylate emulsion, the emulsifier is one or more of alkyl polyoxyethylene ether, fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether.
[0010] In the bio-based degradable acetic acid propylene emulsion, the oxidative initiator includes one or more of benzoyl peroxide, cumene hydroperoxide, hydrogen peroxide, and tert-butyl hydroperoxide; the reductive initiator includes one or more of N,N-dimethylaniline, N,N-diethylaniline, tartaric acid, and sodium glycolate sulfinate.
[0011] In the bio-based degradable acetic acid propylene emulsion, the pH regulator is sodium hydroxide or sodium bicarbonate.
[0012] The present invention also provides a method for preparing a bio-based degradable acetic acid propylene emulsion, comprising the following steps:
[0013] Step S001. At room temperature and pressure, 36 to 38 parts of vinyl acetate, 2 to 4 parts of acrylic acid and 0.5 to 1.5 parts of vinyl siloxane are sequentially added into a stirring container, and stirred for 30 minutes to obtain a monomer premix A;
[0014] Step S002. Add 25 parts of deionized water, 0.4-0.6 parts of emulsifier, 4-6 parts of polyvinyl alcohol and 3-4 parts of cellulose into the polymerization reactor in sequence, and stir evenly to obtain a base liquid B;
[0015] Step S003. 0.15 parts of the oxidizing initiator and 1.5 parts of deionized water are mixed and stirred to prepare an initiator solution C, 0.1 parts of the reducing initiator and 1 part of deionized water are mixed and stirred to prepare an initiator solution D, 0.3 parts of the oxidizing initiator and 6 parts of deionized water are mixed and stirred to prepare an initiator solution E, and 0.25 parts of the reducing initiator and 5.5 parts of deionized water are mixed and stirred to prepare an initiator solution F;
[0016] Step S004. Mix 1.5 to 2.5 parts of a pH regulator with 2 parts of deionized water to prepare a pH regulator solution G;
[0017] Step S005. Mix 1.5 to 2.5 parts of inorganic silicate with 2 parts of deionized water to prepare an inorganic silicate solution H;
[0018] Step S006. Raise the temperature in the polymerization reactor to 70°C to 75°C, and then simultaneously add initiator solution C and initiator solution D to the base solution B;
[0019] Step S007. After the initiator solution C and the initiator solution D are added dropwise, the initiator solution E, the initiator solution F and the monomer premixed solution A are added dropwise to the polymerization reactor at the same time, the adding time is controlled within 190 min to 270 min, and the mixture is kept warm for 30 min after the addition is completed;
[0020] Step S008. After the insulation of step S007 is completed, the temperature in the polymerization reactor is lowered to 43°C to 46°C, and the pH of the materials in the polymerization reactor is adjusted to 6 to 7 with the pH regulator solution G, and then the inorganic silicate solution H is added, and the materials in the polymerization reactor are stirred for 30 minutes. After the stirring is completed, a bio-based degradable acetic acid propylene emulsion is obtained.
[0021] In the method for preparing the bio-based degradable acetic acid propylene emulsion, in step S008, after the heat preservation is completed, initiator solution I and initiator solution J are simultaneously added dropwise, and the dropping time is controlled to 30 minutes. After the dropping is completed, the temperature in the polymerization reactor is lowered to 43° C. to 46° C.;
[0022] The initiator solution I includes 0.1 parts of an oxidizing initiator and 1 part of deionized water; the initiator solution J includes 0.1 parts of a reducing initiator and 1 part of deionized water.
[0023] Beneficial effects:
[0024] The present invention provides a bio-based degradable acetoacetic acid acrylic emulsion and a preparation method thereof. The acetoacetic acid acrylic emulsion is generated by polymerizing acrylic acid, vinyl siloxane and ethyl acetate, thereby giving a paper coating good film-forming properties, and making the paper coating coating have certain water resistance and chemical resistance; by using polyvinyl alcohol and cellulose as bio-based protective colloids of the acetoacetic acid acrylic emulsion, the acetoacetic acid acrylic emulsion can maintain good stability, thereby providing a guarantee for the water resistance and chemical resistance of the paper coating coating; in addition, inorganic silicate can improve the water resistance and chemical resistance of the acetoacetic acid acrylic emulsion system. Since the polyvinyl alcohol and cellulose in the acetoacetic acid acrylic emulsion can be biodegraded, and the polyenol chain segments remaining from the hydrolysis of the polymerization product of acrylic acid, vinyl siloxane and ethyl acetate can also be biofermented and degraded, the bio-based degradable acetoacetic acid acrylic emulsion provided by the present invention can not only enhance the water resistance and chemical resistance of paper sprayed with paper coating, but also make the paper coating and paper meet the biodegradability specified in the standard "GB / T 19277.1-2011 Definition, Classification, Marking and Degradability Requirements of Degradable Plastics". The coating containing the bio-based degradable acetic acid acrylic emulsion of the present invention is sprayed on paper, and the relative biodegradation efficiency of the paper is measured according to the standard "GB / T19277.1-2011 Final aerobic biodegradability of materials under controlled composting conditions". The test results show that the relative biodegradation efficiency of the paper can reach ≥90%. DETAILED DESCRIPTION
[0025] The present invention provides a bio-based biodegradable acetic acid propylene emulsion and a preparation method thereof. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the following examples. It should be understood that the specific examples described herein are only used to explain the present invention and are not intended to limit the present invention.
[0026] The invention provides a bio-based degradable vinyl acetate acrylic emulsion, comprising the following components in parts by weight: 36-38 parts of vinyl acetate, 2-4 parts of acrylic acid, 0.5-1.5 parts of vinyl siloxane, 4-6 parts of polyvinyl alcohol, 3-4 parts of cellulose, 1.5-2.5 parts of inorganic silicate, 0.4-0.6 parts of emulsifier, 0.45 parts or 0.55 parts of oxidation initiator, 0.35 parts or 0.45 parts of reduction initiator, 1.5-2.5 parts of pH regulator and 45 parts of deionized water.
[0027] In the above composition, the functional monomers acrylic acid and vinyl siloxane can undergo polymerization reaction with vinyl acetate to obtain an acetoacetic acid emulsion, and the acetoacetic acid emulsion is used in papermaking coatings to give the papermaking coatings better film-forming properties, and can enhance the water resistance and chemical resistance of paper sprayed with the papermaking coatings; the polyvinyl alcohol and cellulose can be biodegradable, and can be used as bio-based protective colloids while making the papermaking coatings biodegradable, and can wrap and protect the emulsion particles, so that the acetoacetic acid emulsion has better stability, and the water resistance and chemical resistance of the paper can also be maintained at a higher level; the inorganic silicate can improve the water resistance and chemical resistance of the acetoacetic acid emulsion system. After the papermaking coating containing the acetoacetic acid emulsion is sprayed on the paper, during the drying process of the coating, the latex particles fuse, the inorganic silicate will contact the surface of the coating, and gradually establish a network structure with the vinyl siloxane and cellulose, so that a dense coating can be formed on the surface of the paper, so that the surface layer of the coating becomes hard, and the water resistance and chemical resistance of the coating and the paper are more prominent.
[0028] Furthermore, the vinyl siloxane includes one or more of vinyl triethoxy silane, vinyl trimethoxy silane and vinyl tripropoxy silane.
[0029] Furthermore, the inorganic silicate is one of potassium methyl silicate, sodium methyl silicate and lithium methyl silicate. The above inorganic silicates are all inorganic substances, which can enhance the water resistance and chemical resistance of the papermaking coating without affecting the biodegradability of the paper sprayed with the papermaking coating.
[0030] Furthermore, the emulsifier is one or more of alkyl polyoxyethylene ether, fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether. The above emulsifier is a non-ionic emulsifier with high chemical stability, acid and alkali resistance, strong emulsification ability, and can greatly improve the stability of the system.
[0031] Furthermore, the oxidation initiator includes one or more of benzoyl peroxide, cumene hydroperoxide, hydrogen peroxide, and tert-butyl hydroperoxide; the reduction initiator includes one or more of N,N-dimethylaniline, N,N-diethylaniline, tartaric acid, and sodium glycolate sulfinate.
[0032] Furthermore, the pH adjuster is sodium hydroxide or sodium bicarbonate.
[0033] In the bio-based degradable acetoacetic acid-propylene emulsion provided by the present invention, acrylic acid, vinyl siloxane and ethyl acetate are polymerized to generate acetoacetic acid-propylene emulsion, thereby giving the papermaking coating good film-forming properties, so that the papermaking coating coating has certain water resistance and chemical resistance; and polyvinyl alcohol and cellulose as bio-based protective colloids of the acetoacetic acid-propylene emulsion can keep the acetoacetic acid-propylene emulsion in a good stability, thereby providing a guarantee for the water resistance and chemical resistance of the papermaking coating coating; in addition, inorganic silicate can improve the water resistance and chemical resistance of the acetoacetic acid-propylene emulsion system. Because polyvinyl alcohol and cellulose in the acetoacetic acid-propylene emulsion can be biodegraded, and the polyenol chain segments remaining from the hydrolysis of the polymerization product of acrylic acid, vinyl siloxane and ethyl acetate can also be biofermented and degraded, the bio-based degradable acetoacetic acid-propylene emulsion provided by the present invention can not only enhance the water resistance and chemical resistance of paper sprayed with papermaking coating, but also make the papermaking coating and paper meet the biodegradability specified in the standard "GB / T 19277.1-2011 Definition, Classification, Marking and Degradability Requirements for Degradable Plastics". The coating containing the bio-based degradable acetic acid acrylic emulsion of the present invention is sprayed on paper, and the relative biodegradation efficiency of the paper is measured according to the standard "GB / T 19277.1-2011 Final aerobic biodegradability of materials under controlled composting conditions". The test results show that the relative biodegradation efficiency of the paper can reach ≥90%.
[0034] The present invention also provides a method for preparing a bio-based degradable acetic acid propylene emulsion, comprising the following steps:
[0035] Step S001. At room temperature and pressure, 36 to 38 parts of vinyl acetate, 2 to 4 parts of acrylic acid and 0.5 to 1.5 parts of vinyl siloxane are sequentially added into a stirring container, and stirred for 30 minutes to obtain a monomer premix A;
[0036] Step S002. Add 25 parts of deionized water, 0.4-0.6 parts of emulsifier, 4-6 parts of polyvinyl alcohol and 3-4 parts of cellulose into the polymerization reactor in sequence, and stir evenly to obtain a base liquid B;
[0037] Step S003. 0.15 parts of the oxidizing initiator and 1.5 parts of deionized water are mixed and stirred to prepare an initiator solution C, 0.1 parts of the reducing initiator and 1 part of deionized water are mixed and stirred to prepare an initiator solution D, 0.3 parts of the oxidizing initiator and 6 parts of deionized water are mixed and stirred to prepare an initiator solution E, and 0.25 parts of the reducing initiator and 5.5 parts of deionized water are mixed and stirred to prepare an initiator solution F;
[0038] Step S004. Mix 1.5 to 2.5 parts of a pH regulator with 2 parts of deionized water to prepare a pH regulator solution G;
[0039] Step S005. Mix 1.5 to 2.5 parts of inorganic silicate with 2 parts of deionized water to prepare an inorganic silicate solution H;
[0040] Step S006. Raise the temperature in the polymerization reactor to 70°C to 75°C, and then simultaneously add initiator solution C and initiator solution D to the base solution B;
[0041] Step S007. After the initiator solution C and the initiator solution D are added dropwise, the initiator solution E, the initiator solution F and the monomer premixed solution A are added dropwise to the polymerization reactor at the same time, the adding time is controlled within 190 min to 270 min, and the mixture is kept warm for 30 min after the addition is completed;
[0042] Step S008. After the insulation of step S007 is completed, the temperature in the polymerization reactor is lowered to 43°C to 46°C, and the pH of the materials in the polymerization reactor is adjusted to 6 to 7 with the pH regulator solution G, and then the inorganic silicate solution H is added, and the materials in the polymerization reactor are stirred for 30 minutes. After the stirring is completed, a bio-based degradable acetic acid propylene emulsion is obtained.
[0043] Furthermore, in step S008, after the insulation is completed, initiator solution I and initiator solution J are added dropwise at the same time, and the addition time is controlled at 30 minutes. After the addition is completed, the temperature in the polymerization reactor is lowered to 43°C to 46°C; wherein, initiator solution I includes 0.1 parts of oxidizing initiator and 1 part of deionized water; initiator solution J includes 0.1 parts of reducing initiator and 1 part of deionized water. The initiator solution I and initiator solution J can be used to treat the residual monomers in the emulsion, respectively, which can improve the conversion efficiency of the monomers, eliminate irritating odors, reduce the odor of the acetic acid propylene emulsion, and improve the health of the construction workers while being environmentally friendly.
[0044] Furthermore, in step S006, the initiator solution C and the initiator solution D are added dropwise so that the monomers in the monomer pre-emulsion A can react quickly after the monomer pre-emulsion A is added, thereby increasing the yield of the acetic acid propylene emulsion.
[0045] Furthermore, in step S006, the temperature in the polymerization reactor cannot be too low. If the temperature in the reactor is too low, the monomers in the reactor will reach the reaction conditions, while if the temperature in the reactor is too high, ethyl acetate will easily volatilize. Therefore, a better reaction temperature can ensure that the yield of ethyl acetate emulsion will not decrease. Preferably, in step S006, the temperature in the polymerization reactor is 70°C to 75°C.
[0046] Furthermore, in step S008, adjusting the pH of the materials in the polymerization reactor to 6-7 with the pH adjusting agent solution G helps to improve the storage stability of the acetic acid propylene emulsion. At the same time, when using the acetic acid propylene emulsion, it will not cause harm to the construction workers due to the excessive acidity or alkalinity of the emulsion.
[0047] In order to further illustrate the bio-based degradable acetic acid propylene emulsion and the preparation method thereof provided by the present invention, the following examples and comparative examples are provided.
[0048] Example 1
[0049] The invention provides a bio-based degradable vinyl acetate emulsion, which comprises the following components in parts by weight: 36 parts of vinyl acetate, 2 parts of acrylic acid, 0.5 parts of vinyl triethoxy silane, 4 parts of polyvinyl alcohol, 3 parts of cellulose, 1.5 parts of potassium methyl silicate, 0.4 parts of alkyl polyoxyethylene ether, 0.45 parts of benzoyl peroxide, 0.35 parts of N,N-dimethylaniline, 1.5 parts of sodium hydroxide, 45 parts of deionized water, 0.1 parts of tert-butyl hydroperoxide and 0.1 parts of sodium hydroxyacetic acid sulfinate.
[0050] This embodiment also provides a method for preparing a bio-based degradable acetic acid propylene emulsion, comprising the following steps:
[0051] Step S001. At room temperature and pressure, 36 parts of vinyl acetate, 2 parts of acrylic acid and 0.5 parts of vinyl triethoxysilane are added into a stirring container in sequence, and the mixture is stirred for 30 minutes to obtain a monomer premix A;
[0052] Step S002. Add 25 parts of deionized water, 0.4 parts of alkyl polyoxyethylene ether, 4 parts of polyvinyl alcohol and 3 parts of cellulose into the polymerization reactor in sequence, and stir evenly to obtain a base liquid B;
[0053] Step S003. 0.15 parts of benzoyl peroxide and 1.5 parts of deionized water are mixed and stirred to prepare initiator solution C, 0.1 parts of N, N-dimethylaniline and 1 part of deionized water are mixed and stirred to prepare initiator solution D, 0.3 parts of benzoyl peroxide and 6 parts of deionized water are mixed and stirred to prepare initiator solution E, and 0.25 parts of N, N-dimethylaniline and 5.5 parts of deionized water are mixed and stirred to prepare initiator solution F;
[0054] Step S004. Mix 1.5 parts of sodium hydroxide and 2 parts of deionized water and stir to prepare a pH regulator solution G;
[0055] Step S005. Mix 1.5 parts of potassium methyl silicate and 2 parts of deionized water and stir to prepare an inorganic silicate solution H;
[0056] Step S006. Raise the temperature in the polymerization reactor to 70°C to 75°C, and then simultaneously add initiator solution C and initiator solution D to the base solution B;
[0057] Step S007. After the initiator solution C and the initiator solution D are added dropwise, the initiator solution E, the initiator solution F and the monomer premixed solution A are added dropwise to the polymerization reactor at the same time. The adding time is controlled within 190 minutes. After the adding is completed, the mixture is kept warm for 30 minutes.
[0058] Step S008. After the insulation of step S007 is completed, initiator solution I and initiator solution J are added dropwise at the same time, and the dropping time is controlled at 30 minutes. After the dropping is completed, the temperature in the polymerization reactor is lowered to 43°C to 46°C, and the pH of the material in the polymerization reactor is adjusted to 6 to 7 with the pH regulator solution G, and then the inorganic silicate solution H is added, and the material in the polymerization reactor is stirred for 30 minutes. After the stirring is completed, a bio-based degradable acetic acid propylene emulsion is obtained.
[0059] Among them, the initiator solution I includes 0.1 parts of oxidizing initiator and 1 part of deionized water; the initiator solution J includes 0.1 parts of reducing initiator and 1 part of deionized water.
[0060] Example 2
[0061] A bio-based degradable vinyl acetate emulsion comprises the following components in parts by weight: 37 parts of vinyl acetate, 3 parts of acrylic acid, 1 part of vinyl trimethoxy silane, 2 parts of polyvinyl alcohol, 3.5 parts of cellulose, 2 parts of sodium methyl silicate, 0.5 parts of fatty alcohol polyoxyethylene ether, 0.45 parts of isopropylbenzene hydroperoxide, 0.35 parts of N,N-diethylaniline, 2 parts of sodium hydroxide, 45 parts of deionized water, 0.1 parts of tert-butyl hydroperoxide and 0.1 parts of sodium hydroxyacetic acid sulfinate.
[0062] This embodiment also provides a method for preparing a bio-based degradable acetic acid propylene emulsion, comprising the following steps:
[0063] Step S001. At room temperature and pressure, 37 parts of vinyl acetate, 3 parts of acrylic acid and 1 part of vinyl trimethoxy silane were added into a stirring container in sequence, and the mixture was stirred for 30 minutes to obtain a monomer premix A;
[0064] Step S002. Add 25 parts of deionized water, 0.5 parts of fatty alcohol polyoxyethylene ether, 5 parts of polyvinyl alcohol and 3.5 parts of cellulose into the polymerization reactor in sequence, and stir evenly to obtain a base liquid B;
[0065] Step S003. 0.15 parts of cumene hydroperoxide and 1.5 parts of deionized water are mixed and stirred to prepare initiator solution C, 0.1 parts of N, N-diethylaniline and 1 part of deionized water are mixed and stirred to prepare initiator solution D, 0.3 parts of cumene hydroperoxide and 6 parts of deionized water are mixed and stirred to prepare initiator solution E, and 0.25 parts of N, N-diethylaniline and 5.5 parts of deionized water are mixed and stirred to prepare initiator solution F;
[0066] Step S004. Mix 2 parts of sodium hydroxide and 2 parts of deionized water and stir to prepare a pH regulator solution G;
[0067] Step S005. Mix 2 parts of sodium methyl silicate and 2 parts of deionized water and stir to prepare an inorganic silicate solution H;
[0068] Step S006, step S007 and step S008 are the same as those in the first embodiment.
[0069] Example 3
[0070] The invention provides a bio-based degradable vinyl acetate emulsion, comprising the following components in parts by weight: 38 parts of vinyl acetate, 4 parts of acrylic acid, 1.5 parts of vinyl tripropoxy silane, 6 parts of polyvinyl alcohol, 4 parts of cellulose, 2.5 parts of lithium methyl silicate, 0.6 parts of alkylphenol polyoxyethylene ether, 0.45 parts of hydrogen peroxide, 0.35 parts of tartaric acid, 2.5 parts of sodium bicarbonate and 45 parts of deionized water.
[0071] This embodiment also provides a method for preparing a bio-based degradable acetic acid propylene emulsion, comprising the following steps:
[0072] Step S001. At room temperature and pressure, 38 parts of vinyl acetate, 4 parts of acrylic acid and 1.5 parts of vinyltripropoxysilane were added into a stirring container in sequence, and the mixture was stirred for 30 minutes to obtain a monomer premix A;
[0073] Step S002. Add 25 parts of deionized water, 0.6 parts of alkylphenol polyoxyethylene ether, 6 parts of polyvinyl alcohol and 4 parts of cellulose into the polymerization reactor in sequence, and stir evenly to obtain a base liquid B;
[0074] Step S003. 0.15 parts of hydrogen peroxide and 1.5 parts of deionized water are mixed and stirred to prepare initiator solution C, 0.1 parts of tartaric acid and 1 part of deionized water are mixed and stirred to prepare initiator solution D, 0.3 parts of hydrogen peroxide and 6 parts of deionized water are mixed and stirred to prepare initiator solution E, and 0.25 parts of tartaric acid and 5.5 parts of deionized water are mixed and stirred to prepare initiator solution F;
[0075] Step S004. Mix 2.5 parts of sodium bicarbonate and 2 parts of deionized water and stir to prepare a pH regulator solution G;
[0076] Step S005. Mix 2.5 parts of lithium methyl silicate and 2 parts of deionized water and stir to prepare an inorganic silicate solution H;
[0077] Step S006, step S007 and step S008 are the same as those in the first embodiment.
[0078] Comparative Example 1
[0079] A bio-based degradable vinyl acetate emulsion comprises the following components in parts by weight: 37 parts of vinyl acetate, 3 parts of acrylic acid, 1 part of vinyl trimethoxy silane, 2 parts of polyvinyl alcohol, 3.5 parts of cellulose, 0.5 parts of fatty alcohol polyoxyethylene ether, 0.45 parts of isopropylbenzene hydroperoxide, 0.35 parts of N,N-diethylaniline, 2 parts of sodium hydroxide, 45 parts of deionized water, 0.1 parts of tert-butyl hydroperoxide and 0.1 parts of sodium hydroxyacetic acid sulfinate.
[0080] This comparative example also provides a method for preparing a bio-based degradable acetic acid propylene emulsion. Compared with Example 2, the method for preparing the bio-based degradable acetic acid propylene emulsion does not include step S005 in Example 2.
[0081] Comparative Example 2
[0082] A bio-based degradable vinyl acetate emulsion comprises the following components in parts by weight: 37 parts of vinyl acetate, 3 parts of acrylic acid, 1 part of vinyl trimethoxy silane, 2 parts of polyvinyl alcohol, 3.5 parts of cellulose, 0.5 part of sodium methyl silicate, 0.5 part of fatty alcohol polyoxyethylene ether, 0.45 part of isopropylbenzene hydroperoxide, 0.35 part of N,N-diethylaniline, 2 parts of sodium hydroxide, 45 parts of deionized water, 0.1 part of tert-butyl hydroperoxide and 0.1 part of sodium hydroxyacetic acid sulfinate.
[0083] This embodiment also provides a method for preparing a bio-based degradable acetic acid propylene emulsion, specifically:
[0084] Steps S001 to S004 are the same as those in Example 2;
[0085] Step S005. Mix 0.5 parts of sodium methyl silicate and 2 parts of deionized water and stir to prepare an inorganic silicate solution H;
[0086] Step S006, step S007 and step S008 are the same as those in the second embodiment.
[0087] Comparative Example 3
[0088] A bio-based degradable vinyl acetate emulsion comprises the following components in parts by weight: 37 parts of vinyl acetate, 3 parts of acrylic acid, 1 part of vinyl trimethoxy silane, 2 parts of polyvinyl alcohol, 3.5 parts of cellulose, 1 part of sodium methyl silicate, 0.5 parts of fatty alcohol polyoxyethylene ether, 0.45 parts of isopropylbenzene hydroperoxide, 0.35 parts of N,N-diethylaniline, 2 parts of sodium hydroxide, 45 parts of deionized water, 0.1 parts of tert-butyl hydroperoxide and 0.1 parts of sodium hydroxyacetic acid sulfinate.
[0089] This embodiment also provides a method for preparing a bio-based degradable acetic acid propylene emulsion, specifically:
[0090] Steps S001 to S004 are the same as those in Example 2;
[0091] Step S005. Mix 0.5 parts of sodium methyl silicate and 2 parts of deionized water and stir to prepare an inorganic silicate solution H;
[0092] Step S006, step S007 and step S008 are the same as those in the second embodiment.
[0093] Comparative Example 4
[0094] A bio-based degradable vinyl acetate emulsion comprises the following components in parts by weight: 37 parts of vinyl acetate, 3 parts of acrylic acid, 1 part of vinyl trimethoxy silane, 2 parts of polyvinyl alcohol, 3.5 parts of cellulose, 4 parts of sodium methyl silicate, 0.5 parts of fatty alcohol polyoxyethylene ether, 0.45 parts of isopropylbenzene hydroperoxide, 0.35 parts of N,N-diethylaniline, 2 parts of sodium hydroxide, 45 parts of deionized water, 0.1 parts of tert-butyl hydroperoxide and 0.1 parts of sodium hydroxyacetic acid sulfinate.
[0095] This embodiment also provides a method for preparing a bio-based degradable acetic acid propylene emulsion, specifically:
[0096] Steps S001 to S004 are the same as those in Example 2;
[0097] Step S005. Mix 4 parts of sodium methyl silicate and 2 parts of deionized water and stir to prepare an inorganic silicate solution H;
[0098] Step S006, step S007 and step S008 are the same as those in the second embodiment.
[0099] The acetic acid acrylic emulsions prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were formulated into papermaking coatings according to the papermaking coating formula shown in Table 1 below, and then the formulated papermaking coatings were sprayed on paper. After the coating was dried, water was dripped on the coating surface for 10 minutes, and the coating condition was observed. The observation results are shown in Table 2 below.
[0100] Table 1:
[0101]
[0102]
[0103] Table 2:
[0104]
[0105] It can be seen from the observation results in Table 2 that the papermaking coatings containing the acetic acid acrylate emulsions prepared in Examples 1 to 3 can enhance the water resistance of the paper after being sprayed on the paper; while the acetic acid acrylate emulsion of Comparative Example 1 does not use inorganic silicate, and after the papermaking coating containing the acetic acid acrylate emulsion is sprayed on the paper, the water resistance of the paper is poor; Comparative Example 4 uses too much inorganic silicate, which easily leads to poor stability of the acetic acid acrylate emulsion and cannot be used normally; Compared with Comparative Example 1, the water resistance of the paper in Comparative Examples 2 and 3 is improved, but the optimal effect is still not achieved.
[0106] It is understandable that those skilled in the art can make equivalent substitutions or changes based on the technical solution and inventive concept of the present invention, and all these changes or substitutions should fall within the protection scope of the claims attached to the present invention.
Claims
1. A bio-based biodegradable acetic acid propylene emulsion, It is characterized in that The invention comprises the following components in parts by weight: 36-38 parts of vinyl acetate, 2-4 parts of acrylic acid, 0.5-1.5 parts of vinyl siloxane, 4-6 parts of polyvinyl alcohol, 3-4 parts of cellulose, 1.5-2.5 parts of inorganic silicate, 0.4-0.6 parts of emulsifier, 0.55 parts of oxidation initiator, 0.45 parts of reduction initiator, 1.5-2.5 parts of pH regulator and 45 parts of deionized water; The vinyl siloxane includes one or more of vinyl triethoxysilane, vinyl trimethoxysilane and vinyl tripropoxysilane; The inorganic silicate is one of potassium methyl silicate, sodium methyl silicate and lithium methyl silicate; The method for preparing the bio-based degradable acetic acid propylene emulsion comprises the following steps: Step S001. At room temperature and pressure, 36 to 38 parts of vinyl acetate, 2 to 4 parts of acrylic acid and 0.5 to 1.5 parts of vinyl siloxane are sequentially added into a stirring container, and stirred for 30 minutes to obtain a monomer premix A; Step S002. Add 25 parts of deionized water, 0.4-0.6 parts of emulsifier, 4-6 parts of polyvinyl alcohol and 3-4 parts of cellulose into the polymerization reactor in sequence, and stir evenly to obtain a base liquid B; Step S003. 0.15 parts of the oxidizing initiator and 1.5 parts of deionized water are mixed and stirred to prepare an initiator solution C, 0.1 parts of the reducing initiator and 1 part of deionized water are mixed and stirred to prepare an initiator solution D, 0.3 parts of the oxidizing initiator and 6 parts of deionized water are mixed and stirred to prepare an initiator solution E, and 0.25 parts of the reducing initiator and 5.5 parts of deionized water are mixed and stirred to prepare an initiator solution F; Step S004. Mix 1.5 to 2.5 parts of a pH regulator with 2 parts of deionized water to prepare a pH regulator solution G; Step S005. Mix 1.5 to 2.5 parts of inorganic silicate with 2 parts of deionized water to prepare an inorganic silicate solution H; Step S006. Raise the temperature in the polymerization reactor to 70°C to 75°C, and then simultaneously add initiator solution C and initiator solution D to the base solution B; Step S007. After the initiator solution C and the initiator solution D are added dropwise, the initiator solution E, the initiator solution F and the monomer premixed solution A are added dropwise to the polymerization reactor at the same time, the adding time is controlled within 190 min to 270 min, and the mixture is kept warm for 30 min after the addition is completed; Step S008. After the heat preservation of step S007 is completed, initiator solution I and initiator solution J are added dropwise at the same time, and the dropping time is controlled to be 30 minutes. After the dropping is completed, the temperature in the polymerization reactor is lowered to 43° C. to 46° C., and the pH of the materials in the polymerization reactor is adjusted to 6 to 7 with pH regulator solution G, and then the inorganic silicate solution H is added, and the materials in the polymerization reactor are stirred for 30 minutes. After the stirring is completed, a bio-based degradable acetic acid propylene emulsion is obtained; The initiator solution I includes 0.1 parts of an oxidizing initiator and 1 part of deionized water; the initiator solution J includes 0.1 parts of a reducing initiator and 1 part of deionized water.
2. The biodegradable acetoacrylate emulsion according to claim 1, It is characterized in that The emulsifier is one or more of alkyl polyoxyethylene ether, fatty alcohol polyoxyethylene ether and alkylphenol polyoxyethylene ether.
3. The biodegradable acetoacrylate emulsion according to claim 1, It is characterized in that The oxidation initiator includes one or more of benzoyl peroxide, cumene hydroperoxide, hydrogen peroxide, and tert-butyl hydroperoxide; the reduction initiator includes one or more of N,N-dimethylaniline, N,N-diethylaniline, tartaric acid, and sodium glycolate sulfinate.
4. The biodegradable acetoacrylate emulsion according to claim 1, It is characterized in that The pH regulator is sodium hydroxide or sodium bicarbonate.
Citation Information
Patent Citations
Composite high-power waterproof silica gel paint and preparation method thereof
CN103468040A
High-water-resistance modified polyvinyl acetate emulsion adhesive for pencils, and preparation method for adhesive
CN105038658A
Organosilicon vinyl acetate-acrylic emulsion and preparation method thereof and redispersible emulsion powder prepared from organosilicon vinyl acetate-acrylic emulsion
CN106496399A
Modified inorganic silicate compounded stain-resistant anti-freezing emulsion and preparation method thereof
CN112851867A
Inorganic coating base material system, inorganic coating system, interior wall inorganic coating and application
CN115216166A