Porous metal with open skeleton and method for manufacturing the same

By opening the enclosed space of the hollow skeleton in the porous metal, the problem of its inability to utilize the internal space is solved, and the porosity and surface area are achieved, and the performance of batteries and catalysts is improved. It is suitable for batteries and catalysts and other fields.

CN116024619BActive Publication Date: 2024-11-15WUZHOU HGP ADVANCED MATERIALS TECH CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310014094.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-11-25
Filing Date
2023-01-05
Publication Date
2024-11-15
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

The closed space inside the hollow skeleton of the existing porous metal cannot be effectively utilized, resulting in the failure to fully utilize its potential performance, especially in battery and catalyst applications, which makes it difficult to improve battery capacity and catalytic activity.

Method used

Through directional conduction treatment and high-temperature reduction and sintering processes, porous metals with open frames are manufactured, opening up the enclosed space within the metal frames, increasing the effective porosity and surface area, so that it can be directly connected to the outside.

Benefits of technology

It improves the effective porosity and specific surface area of ​​porous metals, increases the filling amount of the electrolyte and electrode active substances of the battery, reduces the resistivity, improves the catalytic activity and heat exchange performance, and is suitable for a wider range of application fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116024619B_ABST
    Figure CN116024619B_ABST
Patent Text Reader

Abstract

The present invention discloses a porous metal with an open skeleton and a manufacturing method thereof, belonging to the technical field of porous metals. The porous metal is mainly or entirely composed of an open metal skeleton, and has a higher effective specific surface area and a higher effective porosity than the traditional porous metal with a hollow skeleton structure. It exhibits higher tensile strength, greater elongation, etc. in mechanical properties, and has higher thermal conductivity, filtration permeability, high loading capacity, etc. The manufacturing method of the porous metal is to first perform a directional conductive treatment, then remove the organic template material, and then reduce it to obtain a porous metal with an open structure, and further perform structural reinforcement and repair through secondary deposition. The porous metal can achieve roll-to-roll large-scale production. The porous metal can be used in the fields of ultra-thin liquid wicks of heat spreaders and heat spreaders, battery electrode materials, and electrolytic hydrogen production electrodes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous metals and relates to a porous metal with an open skeleton and a manufacturing method thereof. Background Art

[0002] Porous metal is a material composed of a metal skeleton and pores. Due to the presence of a large number of pores inside the material, compared with solid metal materials, it has the characteristics of low density, large specific surface area, high specific strength, excellent permeability, good electromagnetic shielding performance, and good energy and sound absorption performance. Due to its excellent physical, mechanical and mechanical properties, porous metal has become an excellent engineering material with dual attributes of function and structure. It has broad application prospects as a structural and functional material.

[0003] Because porous metals have high porosity and large specific surface area, they can be filled with more active substances, increasing the capacity of the battery and greatly reducing the real current density of the electrode. They are ideal materials for making various primary or secondary batteries such as nickel-cadmium batteries, nickel-hydrogen batteries, vanadium batteries, nickel-zinc batteries, sodium-ion batteries, lithium-ion batteries, as well as storage batteries, air batteries, fuel cells and solar cell electrodes, providing the possibility for the development of lightweight batteries with low internal consumption, long life and high specific energy. Porous metals have good electrical conductivity, certain self-supporting ability and large specific surface area to provide a wide interfacial electrochemical charge transfer space, thus becoming an excellent electrode material. Porous metal electrodes have extremely broad application prospects in the field of electrochemistry, and the research and application of porous metals has become an important development direction of electrode materials.

[0004] Nickel foam is a typical porous metal with a theoretical porosity of more than 90% and an effective porosity of 70% to 90%. It can be easily mass-produced and manufactured. It has been commercialized. It uses organic polymer porous materials (usually polyurethane foam materials) as templates, undergoes conductive treatment (through chemical plating, coating with conductive glue or vacuum vapor deposition), electrodeposition metal thickening, incineration to remove the organic polymer template, and then undergoes high-temperature reduction sintering process to obtain the product. Compared with powder sintered nickel matrix, nickel foam has the advantages of simple production process, low cost, high porosity, light weight, and easy active material filling. In the late 1980s, it replaced powder sintered nickel matrix as the electrode conductive matrix of nickel-cadmium and nickel-hydrogen batteries, thereby greatly improving the specific capacity and specific energy of the battery. As the current collecting material of the electrode matrix, nickel foam has the dual functions of carrying electrode active substances and collecting electrochemical reaction current. Therefore, the basic requirements for nickel foam are good mechanical and electrical properties, as well as a large porosity to fill more electrode active substances to increase the specific capacity of the battery.

[0005] As an electroformed replica of organic foam plastics, nickel foam basically maintains the structural morphology of the original foam plastics. The skeletons that make up nickel foam are crisscrossed, and each node is generally formed by 3-5 skeletons crossing each other. After removing the organic foam matrix, these metal skeletons will form tiny hollow cavities inside the skeleton. The tiny hollow cavities are the spaces left after the original organic foam plastics disappear. Therefore, the skeletons are all closed hollow rib structures. The tiny hollow cavities inside the skeletons are also part of the overall porosity of nickel foam, accounting for about 2% to 20% of the porosity of the entire nickel foam. These holes inside the skeletons have too small pore sizes, which not only makes it difficult to fill active substances inside them, but also increases the resistivity of the battery. If these micropores can be utilized during the battery manufacturing process, the amount of electrolyte filled in the battery or the amount of electrode active substances can be increased, thereby improving the overall performance of the battery.

[0006] A monograph entitled "Introduction to Porous Materials" (Liu Peisheng. Introduction to Porous Materials [M]. Tsinghua University Press, 2004) discloses a porous metal prepared by electrodeposition in Chapter 3.3.4 on page 193, and its process includes substrate pretreatment, conductive treatment, electroplating and reduction sintering. At the same time, page 196 of this chapter points out that the porous body obtained after reduction sintering is a three-dimensional network composed of hollow metal ribs.

[0007] The porous metal with hollow ribs is produced by depositing metal on an organic porous template and then undergoing a sintering reduction process. Its skeleton has a tiny hollow cavity, and the inner wall of the hollow cavity also has a large surface area. However, since it is enclosed inside the skeleton, this part of the surface area is difficult to use. If there is a way to expose this part of the surface, when this type of porous metal is used as a battery current collector, the electrolyte or electrode active material can have a larger contact area with the current collector, which can greatly improve the current collection capacity and improve the overall performance of the battery; when this type of porous metal is used as a catalyst carrier, the synthesized catalyst will have a larger catalytic area and catalytic sites, and its catalytic activity becomes higher.

[0008] A journal article titled "Forced Convection of Hollow Skeleton Open-Cell Metal Foam" (Feng Shangsheng, Jin Dongfan, Lu Tianjian. Forced Convection of Hollow Skeleton Open-Cell Metal Foam [C] / / 2009 Academic Conference of the Chinese Society of Mechanics. 2009) compared the forced convection heat transfer capacity and flow resistance performance of solid rod racks and hollow rod rack open-cell metal foams, and concluded that: ① Under the same porosity, whether air or water is used as the cooling medium, the metal foam Nu number decreases with the increase of the rod rack hollowness; ② Under the same relative density, the piezoresistance ratio of hollow rod and solid rod metal foams is greater than 1, and increases rapidly with the increase of the rod rack hollowness. When the rod rack hollowness reaches 60%, the flow resistance of the hollow rod metal foam is 47% higher than that of the solid rod foam. It can be seen that the forced convection heat transfer capacity of hollow rod metal is weaker than that of solid rod metal foam.

[0009] Open-cell metal foam has a high specific surface area and heat exchange coefficient. At the same time, its complex solid skeleton structure can promote fluid disturbance. These characteristics make metal foam have excellent heat transfer performance. The effective heat exchange coefficient of metal foam with a hollow rib structure is lower than that of metal foam with a solid rib structure. Therefore, by opening the hollow rib structure of the skeleton, its heat exchange coefficient can be effectively improved.

[0010] The production process of hollow rib porous metal obtained by depositing metal on an organic porous template and then sintering and reducing it has the characteristics of convenient large-scale continuous production, lower cost and better consistency compared with other processes for manufacturing porous metals, which is unmatched by other processes for manufacturing porous metals. However, the disadvantage of the porous metal prepared by this template method is that the metal skeleton is hollow, and the hollow cavity inside the skeleton occupies a large amount of space but is almost unusable, making it difficult to fully utilize the advantages of this type of porous metal. Therefore, it is necessary to open the closed hollow rib structure and utilize the space and surface area it occupies to improve the performance of this type of porous metal so that it can play a better role in more fields. Summary of the invention

[0011] The purpose of the present invention is to provide a porous metal with an open skeleton and a method for manufacturing the same. The porous metal with an open skeleton provided by the present invention can open most or all of the enclosed spaces in the hollow skeleton of the porous metal, increase the surface area, reduce the density, and improve the effective porosity, so that the potential performance of the porous metal is further released. The effective porosity refers to the proportion of pores that can play a function (filling electrode active materials, filling catalysts, absorbing liquids, serving as liquid channels, etc.) to all pores. The purpose of the present invention is achieved by the following technical solutions.

[0012] A porous metal with an open skeleton, wherein the porous metal is composed of a metal skeleton and pores, wherein the metal skeleton is obtained by depositing metal on the surface of an organic polymer porous material and then removing the organic polymer porous material; the metal skeletons are all open skeletons or a mixture of open skeletons and hollow skeletons; the open skeleton includes the space left after the metal deposition layer and the organic polymer porous material are removed, and the space left is not completely surrounded by the metal deposition layer and can be directly connected to the external space; the hollow skeleton includes the space left after the metal deposition layer and the organic polymer porous material are removed, and the space left is completely surrounded by the metal deposition layer and cannot be directly connected to the external space.

[0013] Furthermore, the ratio of the open frame to the total metal frame is 20% to 100%, preferably 60% to 100%.

[0014] The proportion of the open skeleton described in the present invention to the total metal skeleton can be measured by the following method: take a piece of porous metal, encapsulate it in a resin (such as epoxy resin), and then grind and polish the test surface. The test surface can select any one of the four surfaces parallel to the direction of the directional deposition metal. After the test surface is grinded and polished, select a test area on the test surface with a width equal to the thickness of the porous metal and a length equal to twice the thickness of the porous metal. Calculate the number of open skeletons in the test area and the number of all metal skeletons. If a part of the open skeleton or hollow skeleton is included in the test area, it will be counted as one open skeleton or hollow skeleton for accumulation.

[0015] The ratio of open frames to all metal frames = the total number of open frames in the test area / the total number of metal frames in the test area × 100%

[0016] In some specific embodiments, the porous metal is a two-dimensional porous metal, and its metal skeleton is a continuous solid and arranged in a polygonal two-dimensional shape; accordingly, the pores are columnar and separated between the metal skeletons.

[0017] In some specific embodiments, the porous metal is a three-dimensional porous metal, whose metal skeleton is a continuous solid and presents a three-dimensional network structure, and the pores between the metal skeletons are interconnected.

[0018] In some specific embodiments, the average pore size of the pores is 0.05-5 mm.

[0019] In some specific embodiments, the thickness of the metal layer of the metal skeleton is 1-1000 μm.

[0020] In some specific embodiments, the thickness of the porous metal is 0.005-65 mm.

[0021] In some specific embodiments, the metal deposition layer is a bimodal metal deposition layer composed of grains of two different sizes or a multimodal metal deposition layer composed of grains of multiple different sizes.

[0022] In some specific embodiments, the metal deposition layer is a single metal material formed by any one of iron, nickel, copper, iron, aluminum, chromium, cadmium, germanium, tin, lead, zinc, gold, silver, titanium, cobalt, vanadium, niobium, hafnium, tantalum, bismuth, molybdenum, tungsten, manganese, platinum, palladium, ruthenium, rhodium, iridium, and osmium, or a multilayer metal material or alloy material formed by two or more of the above metals.

[0023] The method for manufacturing the porous metal of the present invention comprises the following steps:

[0024] (1) Directed conductive treatment: Using an organic polymer porous material as a template, the outer surface of the template is partially conductive by a method of directed deposition or directed coating of a conductive layer, so that the outer surface of the template is not completely surrounded by the conductive layer. During the process of directed deposition or directed coating of a conductive layer, the metal or its compound to be deposited or coated is attached to part of the surface of the organic polymer porous material along a preset track; the rest of the surface of the organic polymer porous material is in the shadow of the preset track, and the required metal or its compound cannot be attached to this area, thereby achieving partial conductivity on the surface of the organic polymer porous material.

[0025] (2) removing the template to obtain a semi-finished product that does not contain organic polymer porous materials;

[0026] (3) High-temperature reduction sintering: The semi-finished product obtained in step (2) is placed in a reducing or protective atmosphere for treatment at a temperature of 400-1500°C for a time of 20-200 minutes to obtain a porous metal product.

[0027] The present invention provides a method for manufacturing a porous metal with an open skeleton, which is to use an organic polymer porous material as a template, undergo a directional conductive treatment, remove the organic polymer template, and then undergo a high-temperature reduction sintering process to obtain a product. During the directional conductive treatment, a method of directional deposition or directional coating of a conductive layer is used to make the outer surface of the polymer template partially conductive, that is, the conductive layer does not completely surround the skeleton surface of the organic polymer porous material. After the deposited metal layer reaches a sufficient thickness, more than 20% of the skeleton surface of the organic polymer porous material is not completely surrounded by the metal layer. After the subsequent removal of the organic polymer template and high-temperature reduction sintering process, the metal layer on the cross section of this part of the skeleton has a gap, so that the space left after the organic polymer porous material is removed can be directly connected to the external environment.

[0028] Furthermore, the method for removing the template in step (2) is one or more of incineration, thermal decomposition and dissolution.

[0029] Furthermore, the incineration method refers to heating the organic polymer material with a metal layer on the surface at a temperature of 200-700° C. to decompose or burn the organic polymer material.

[0030] Furthermore, the method of directional deposition or directional coating of the conductive layer is to deposit or coat the conductive layer only on one side of the template, leaving the other side non-conductive.

[0031] Furthermore, the directional deposition refers to vacuum plating, chemical plating, recrystallization, chemical deposition or electroplating.

[0032] Furthermore, the directional coating refers to spraying, scraping, dipping, rolling or brushing.

[0033] Furthermore, the reducing atmosphere refers to a hydrogen atmosphere, a mixed atmosphere of hydrogen and nitrogen, or a mixed atmosphere of hydrogen and argon.

[0034] Furthermore, the protective atmosphere refers to a nitrogen atmosphere, an argon atmosphere, or a mixed atmosphere of nitrogen and argon.

[0035] In some specific embodiments, the surface of the semi-finished product obtained in step (2) is re-treated once or multiple times before step (3) is performed.

[0036] In some specific embodiments, the surface of the porous metal product obtained in step (3) is re-treated once or multiple times.

[0037] In some specific embodiments, the surface of the porous metal product obtained in step (3) is re-treated once or multiple times, and then subjected to high-temperature reduction sintering treatment in step (3), and the re-treatment and high-temperature reduction sintering treatment are cycled multiple times.

[0038] Furthermore, the reprocessing refers to conductive deposition, coating or spraying processing.

[0039] In some specific embodiments, the organic polymer porous material is selected from one or more of polyurethane sponge, polymer non-woven fabric, polymer woven fabric, polymer felt, porous polyester PET, porous polyethylene PE, porous polypropylene PP, porous polyphenylene sulfide PPS, porous polycarbonate and porous polyimide.

[0040] In some specific embodiments, the directional coating of the conductive layer refers to coating with carbon-based coatings, conductive metal-based coatings or a mixture thereof.

[0041] The porous metal with an open skeleton provided by the present invention can be further modified by secondary deposition, coating with a metal layer or metal particles, or spraying with a metal layer to obtain physical and chemical properties such as lower resistivity, higher heat exchange coefficient, higher specific surface area, and higher catalytic activity.

[0042] The porous metal with an open skeleton provided by the present invention has an open skeleton of more than 20%, and the unusable inner surface of the original inner cavity has become an effective outer surface, which greatly increases the surface area of ​​the porous metal. When it is used as a battery current collector, this part of the space can be used to fill more electrolyte or electrode active substances, thereby increasing the battery capacity; at the same time, the electrolyte or electrode active substances can have a larger contact area with the current collector, and the battery internal resistance is smaller, so that the battery has better comprehensive performance such as charge and discharge characteristics. When the porous metal of the present invention is used as a catalyst carrier, the synthesized catalyst will have a larger catalytic area and catalytic sites, and its catalytic activity becomes higher. When the porous metal of the present invention is used as a heat conductor and heat dissipator, its effective thermal conductivity is close to that of a porous metal whose ribs are solid ribs. At the same time, due to its higher porosity and larger specific surface area, its comprehensive heat exchange capacity will exceed that of a similar porous metal whose ribs are solid ribs. Based on the porous metal with an open skeleton provided by the present invention, the performance of various products obtained can be improved.

[0043] The present invention has the following beneficial technical effects:

[0044] (1) The porous metal with an open skeleton provided by the present invention is a porous metal manufactured by a template method and the closed space in the metal skeleton is opened. Compared with the porous metal manufactured by the ordinary template method, the product of the present invention has a higher effective porosity and a higher specific surface area, and also has a lower bulk density.

[0045] (2) The porous metal with an open skeleton provided by the present invention will be compressed to a thickness of less than 1 mm when used to manufacture an ultra-thin absorbent core of a heat spreader or a heat spreader plate. Due to the high compression rate, the internal pores of the porous metal are reduced and the distance between the skeletons is reduced. At this time, the porous metal with an open skeleton can still provide more capillary channels and internal space for absorbing liquid, and can provide better capillary absorption performance. However, after being compressed, the tiny hollow cavity inside the traditional porous metal composed of a hollow rib structure still occupies a large amount of space, and the hollow cavity cannot be used as a capillary channel for absorbing liquid. Therefore, its capillary performance as an ultra-thin absorbent core is poor. Compared with the traditional porous metal composed of a hollow rib structure, the porous metal provided by the present invention can provide higher capillary suction and permeability at the same thickness.

[0046] (3) The porous metal with an open skeleton provided by the present invention is used to manufacture an electrolytic hydrogen production electrode or a battery electrode. Its higher specific surface area can provide a wider interfacial electrochemical charge transfer space, and its higher effective porosity can provide more space for storing electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 It is a schematic diagram of the hollow skeleton structure when the organic polymer template is not removed, wherein 111, 121 and 131 are organic polymer templates, and 112, 122 and 132 are metal layers.

[0048] Figure 2 It is a schematic diagram of an open skeleton structure when the organic polymer template is not removed, wherein 211, 221 and 231 are organic polymer templates, and 212, 222 and 232 are metal layers.

[0049] Figure 3 It is a schematic diagram of the hollow skeleton structure after the organic polymer template has been removed, wherein 311, 321 and 331 are spaces left after the organic polymer template has been removed, and 312, 322 and 332 are metal layers.

[0050] Figure 4 It is a schematic diagram of an open skeleton structure after the organic polymer template has been removed, wherein 411, 421 and 431 are spaces left after the organic polymer template has been removed, and 412, 422 and 432 are metal layers.

[0051] Figure 5 This is a front SEM image of a hollow skeleton in a porous metal with an open skeleton provided by the present invention.

[0052] Figure 6 This is a front SEM image of an open skeleton in a porous metal with an open skeleton provided by the present invention.

[0053] Figure 7 and Figure 8 This is a SEM image of a hollow skeleton cross section in a porous metal with an open skeleton provided by the present invention.

[0054] Fig. 9 and Fig.10 This is a SEM image of a cross section of an open skeleton in a porous metal with an open skeleton provided by the present invention.

[0055] Fig.11 It is a schematic diagram of a porous metal with an open skeleton provided by the present invention, in which part of the structure is a two-dimensional structure. DETAILED DESCRIPTION

[0056] The technical solution of the present invention is described clearly and completely below in conjunction with the accompanying drawings of the specification. Obviously, the described implementation is only a part of the implementation of the present invention, not all of the implementations. Based on the implementation of the present invention, all other implementations obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0057] Example 1

[0058] A three-dimensional porous metal with an open skeleton is composed of an open skeleton and a hollow skeleton. The open skeleton accounts for 60% of the total metal skeleton. The overall thickness of the three-dimensional porous metal is 65 mm, the average pore size is 5 mm, the metal layer thickness of the metal skeleton is 1000 μm, and the metal type is pure nickel.

[0059] The manufacturing method of the porous metal is as follows:

[0060] (1) Directional conductive treatment: With polyurethane sponge material as the template, vacuum plating is used on only one side of the polyurethane sponge material to deposit metal nickel on one side of the pores inside the template, and then electroplating is used to make the metal layer thickness reach 1000μm, and the outer surface of the template is not completely surrounded by the conductive layer, so as to obtain an open skeleton without removing the polyurethane sponge material (such as Figure 1 ) and hollow skeletons (such as Figure 2 );

[0061] (2) The template is removed by heating and burning at a temperature of 600-700°C to obtain a semi-finished product without organic polymer porous materials, thereby obtaining an open skeleton (such as Figure 3 ) and hollow skeletons (such as Figure 4 );

[0062] (3) High-temperature reduction sintering: The semi-finished product obtained in step (2) is treated under hydrogen and nitrogen at a temperature of 1400-1500°C for 50-60 minutes to obtain a porous metal product.

[0063] Figure 5 This is a front SEM image of a hollow skeleton of a porous metal with an open skeleton in this embodiment. Figure 7 and Figure 8 This is a SEM image of a hollow skeleton cross section of a porous metal with an open skeleton provided by the present invention. Figure 6 , Fig. 9 and Fig.10 It can be seen that the space left after the polyurethane sponge template is removed is surrounded by the metal layer, and the space inside them and the area on the inner wall of the hollow cavity cannot be effectively utilized.

[0064] Figure 6This is a front SEM image of a part of the open skeleton of a three-dimensional porous metal with an open skeleton in this embodiment. Fig. 9 and Fig.10 FIG. 1 is a cross-sectional SEM image of a part of the open skeleton of a porous metal having an open skeleton in this embodiment. Figure 6 , Fig. 9 and Fig.10 It can be seen that the space left after the polyurethane sponge template is removed is connected to the external environment. This part of the space can be used to fill active substances, etc. Their effective porosity and surface area are larger than those of the hollow skeleton.

[0065] Comparative Example 1

[0066] The high-porosity foamed silver material is prepared according to the method described in the Chinese invention application with publication number CN112853409A and titled "A method for preparing a silver-containing plating solution and a foamed metal material".

[0067] First, 0.1 to 5.0 g of potassium permanganate and 1 to 10 mL of concentrated sulfuric acid were dissolved in 200 mL of deionized water to obtain a template surface roughening solution. The polyurethane foam was squeezed and soaked in it for 5 minutes to increase the porosity and roughness of the material.

[0068] Dissolve 0.1-2g of dopamine hydrochloride in 200mL of deionized water to obtain a functional group modification solution, and soak the roughened foam in the functional group modification solution for 18 hours to complete the surface functional group modification process of the foam. This step can enhance the attraction between the foam surface and anions, thereby initiating the smooth progress of chemical silver plating.

[0069] Dissolve an appropriate amount of ammonia water in 50 mL of deionized water to prepare ammonia solution A. Dissolve silver salt in 30 mL of deionized water to obtain silver source solution B; then mix solutions A and B, and add sodium hydroxide solution to adjust the pH value to obtain a silver-ammine complex solution. Dissolve 8 to 10 g of glucose, 0.6 to 1.0 g of tartaric acid and 2 mL of ethanol in 200 mL of deionized water to obtain a reducing agent C. Soak the foam after surface modification in the previous step in the silver-ammine complex solution and fully contact it with the solution, then pour the reducing solution C and continue stirring to fully reduce the silver ions. When the solution becomes clear, indicating that the reduction process has ended, rinse the foam and dry it.

[0070] After the foam is modified with functional groups, a large number of PDA groups are present on the foam surface, and the PDA groups provide attachment sites for silver ions in the subsequent chemical silver plating process.

[0071] After chemical silver plating, the foam surface turns slightly yellow, and a relatively thin silver layer appears on the surface of the foam fiber.

[0072] Preparation of plating solution D:

[0073] S1. First prepare 200mL of 200 g / L sodium thiosulfate solution;

[0074] S2. Next, 250 mL of 40 g / L silver nitrate solution was prepared;

[0075] S3. Prepare 250mL of 40 g / L potassium pyrosulfite solution;

[0076] S4. The solutions prepared in S2 and S3 are mixed under constant stirring, and a white precipitate is generated;

[0077] S5. Immediately add the sodium thiosulfate solution prepared in S1 and continue stirring to completely dissolve the white precipitate, and then add water to the required amount;

[0078] S6. Expose the prepared plating solution under sunlight for 2-3 hours, filter it with filter paper to obtain a clear plating solution.

[0079] During the electroplating process, the anode clamp holds the silver sheet, and the cathode clamp holds the chemically silver-plated foam. During electroplating, the cathode current density should be set to 20 mA cm-2, and the time can be adjusted according to the area and thickness of the foam. After electroplating, the foam surface changes to white-gray due to the attachment of a large number of silver particles.

[0080] The electroplated foam was placed in a muffle furnace and calcined at 600° C. for 30 minutes to remove the polymer foam and obtain porous silver foam.

[0081] As shown in the attached drawing of the patent application specification Figure 6 and Figure 7 As shown, the foam metal skeletons prepared by the preparation method are all hollow skeletons, and their structures are consistent with those described in the monograph "Introduction to Porous Materials" cited in the background technology section. The existing technologies all seek to make the metal completely wrap the template, so that after removing the template, only the hollow skeleton can be left. The proportion of the internal void space of the hollow skeleton to the entire void increases with the increase of the skeleton density, and the proportion can even reach 40%, which has a serious impact on the performance of the foam metal.

[0082] Example 2

[0083] A two-dimensional porous metal with an open skeleton is composed of an open skeleton, the open skeleton accounts for 100% of the entire metal skeleton, the overall thickness of the two-dimensional porous metal is 0.005 mm, the average pore size is 0.05 mm, the metal layer thickness of the metal skeleton is 1-2 μm, and the metal types are copper and palladium.

[0084] The manufacturing method of the porous metal is as follows:

[0085] (1) Directed conductive treatment: Using a woven or non-woven fabric with polymer material as a template, vacuum copper plating is used on one side of the polymer material to deposit metal copper on one side of the pores inside the template so that the thickness of the copper metal layer reaches 1~2μm, and the outer surface of the template is not completely surrounded by the conductive layer, thereby obtaining an open skeleton without removing the polymer material;

[0086] (2) heating and decomposing the polymer material at a temperature of 200° C. to obtain a semi-finished product that does not contain an organic polymer porous material;

[0087] (3) coating the palladium metal on the copper metal surface by spraying;

[0088] (4) High-temperature reduction sintering: The semi-finished product obtained in step (3) is treated under hydrogen at a temperature of 400°C for 200 minutes to obtain a porous metal product (such as Fig.11 as shown).

[0089] Example 3

[0090] A three-dimensional porous metal with an open skeleton is composed of an open skeleton, the open skeleton accounts for 100% of the entire metal skeleton, the overall thickness of the three-dimensional porous metal is 0.6 mm, the average pore size is 0.2 mm, the metal layer thickness of the metal skeleton is 500 μm, and the metal types are nickel, molybdenum and iron.

[0091] The manufacturing method of the porous metal is as follows:

[0092] (1) Directional conductive treatment: With polyurethane sponge material as the template, vacuum nickel plating is performed on only one side of the polyurethane sponge material to deposit metal nickel on one side of the pores inside the template, and then electroplating is performed to make the nickel metal layer thickness reach 500 μm, and the outer surface of the template is not completely surrounded by the conductive layer, thereby obtaining an open skeleton without removing the polyurethane sponge material (such as Figure 1 );

[0093] (2) The template is removed by heating and burning at a temperature of 600-700°C to obtain a semi-finished product 1 that does not contain organic polymer porous materials, thereby obtaining an open skeleton (such as Figure 3 );

[0094] (3) High-temperature reduction sintering: the semi-finished product 1 obtained in step (2) is treated under hydrogen and nitrogen at a temperature of 1500° C. for 20 minutes to obtain a semi-finished product 2;

[0095] (4) electroplating the semi-finished product 2 obtained in step (3) to deposit molybdenum metal on its surface, and performing step (3) again to obtain the target semi-finished product 3;

[0096] (5) The semi-finished product 3 obtained in step (4) is electroplated again to deposit iron metal on its surface, and step (3) is performed again to obtain a porous metal product.

[0097] Example 4

[0098] A three-dimensional porous metal with an open skeleton is composed of an open skeleton, the open skeleton accounts for 20% of the total metal skeleton, the overall thickness of the three-dimensional porous metal is 2 mm, the average pore size is 0.6 mm, the metal layer thickness of the metal skeleton is 300 μm, and the metal types are nickel, aluminum and tin.

[0099] The manufacturing method of the porous metal is as follows:

[0100] (1) Directional conductive treatment: Using porous polypropylene (PP) material as a template, vacuum nickel plating is performed on only one side of the porous polypropylene (PP) material to deposit metal nickel on the pore side of the template material. Then, electroplating is performed to make the nickel metal layer thickness reach 300 μm, and the outer surface of the template is not completely surrounded by the conductive layer, thereby obtaining an open skeleton without removing the polyurethane sponge material (such as Figure 1 ) and hollow skeletons (such as Figure 2 );

[0101] (2) The template is removed by heating and burning at a temperature of 600-700°C to obtain a semi-finished product 1 that does not contain organic polymer porous materials, thereby obtaining an open skeleton (such as Figure 3 ) and hollow skeletons (such as Figure 4 );

[0102] (3) High-temperature reduction sintering: the semi-finished product 1 obtained in step (2) is treated under hydrogen and nitrogen at a temperature of 700-900° C. for 100 minutes to obtain a semi-finished product 2;

[0103] (4) The semi-finished product 2 obtained in step (3) is subjected to vacuum plating to deposit aluminum metal on its surface to obtain the target semi-finished product 3.

[0104] (5) The semi-finished product 3 obtained in step (4) is subjected to vacuum plating to deposit tin metal on its surface to obtain a porous metal product.

[0105] Example 5

[0106] A three-dimensional porous bimodal metal with an open skeleton is composed of an open skeleton and a hollow skeleton. The open skeleton accounts for 80% of the total metal skeleton. The overall thickness of the three-dimensional porous metal is 1.2 mm, the average pore size is 2 mm, the metal layer thickness of the metal skeleton is 700 μm, and the metal type is pure copper.

[0107] The manufacturing method of the porous metal is as follows:

[0108] (1) Directional conductive treatment: With polyurethane sponge material as the template, vacuum plating is used on only one side of the polyurethane sponge material to deposit metal copper on one side of the pores inside the template, and then electroplating is used to make the metal layer thickness reach 500μm, and the outer surface of the template is not completely surrounded by the conductive layer, so as to obtain an open skeleton without removing the polyurethane sponge material (such as Figure 1 ) and hollow skeletons (such as Figure 2 );

[0109] (2) High-temperature reduction sintering: the material after directional conductive treatment is placed in hydrogen and nitrogen for treatment at a temperature of 600-700°C for 150 minutes to obtain a semi-finished product 1;

[0110] (3) Ultrafine-grained copper is sprayed onto the surface of the semi-finished product 1 by spraying, and step (2) is performed again to obtain a three-dimensional porous metal with a bimodal crystal distribution.

[0111] Example 6

[0112] A three-dimensional porous metal with an open skeleton is composed of an open skeleton, the open skeleton accounts for 90% of the total metal skeleton, the overall thickness of the three-dimensional porous metal is 1.8 mm, the average pore size is 0.3 mm, the metal layer thickness of the metal skeleton is 100 μm, and the metal types are nickel, palladium, titanium, zinc and iron.

[0113] The manufacturing method of the porous metal is as follows:

[0114] (1) Directed conductive treatment: With a porous polyethylene PE material as a template, only one side of the porous polyethylene PE material is coated with a sensitizing solution containing tin ions on one side of the pores inside the template material by spraying, and then an activation solution containing palladium ions is dipped to reduce the palladium. The organic polymer porous material after sensitization and activation treatment is placed in a chemical plating solution, and nickel metal is deposited on its surface under the catalytic action of palladium through controlled reduction to obtain a metal deposition layer, and the outer surface of the template is not completely surrounded by the conductive layer, thereby obtaining an open skeleton without removing the polyurethane sponge material (such as Figure 1 ) and hollow skeletons (such as Figure 2 );

[0115] (2) The template is removed by heating and burning at a temperature of 600-700°C to obtain a semi-finished product 1 that does not contain organic polymer porous materials, thereby obtaining an open skeleton (such as Figure 3 ) and hollow skeletons (such as Figure 4 );

[0116] (3) High-temperature reduction sintering: the semi-finished product 1 obtained in step (2) is treated under hydrogen and nitrogen at a temperature of 800-900° C. for 40 minutes to obtain a semi-finished product 2;

[0117] (4) vacuum plating the semi-finished product 2 obtained in step (3) to deposit titanium metal on its surface, thereby obtaining a semi-finished product 3;

[0118] (5) vacuum plating the semi-finished product 3 obtained in step (4) to deposit zinc metal on its surface, thereby obtaining a semi-finished product 4;

[0119] (6) The semi-finished product 4 obtained in step (5) is electroplated again to deposit iron metal on its surface to obtain the target porous metal.

[0120] Although the embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and cannot be understood as limiting the present invention. A person skilled in the art may change, modify, replace and modify the above embodiments within the scope of the present invention without departing from the principles and purpose of the present invention. The protection scope of the present invention is defined by the claims and their equivalent technical solutions.

Claims

1. A porous metal with an open skeleton, wherein the porous metal is composed of a metal skeleton and pores, wherein the metal skeleton is obtained by depositing metal on the surface of an organic polymer porous material and then removing the organic polymer porous material; characterized in that: The metal skeleton is a mixture of an open skeleton and a hollow skeleton; The open frame includes a space left after the metal deposition layer and the organic polymer porous material are removed, and the space left is not completely surrounded by the metal deposition layer and can be directly connected to the external space; The hollow skeleton includes a space left after the metal deposition layer and the organic polymer porous material are removed, and the remaining space is completely surrounded by the metal deposition layer and cannot be directly connected with the external space.

2. The porous metal according to claim 1, characterized in that The open frame accounts for 20% to 80% of the total metal frame.

3. The porous metal according to claim 1, characterized in that: The average pore size of the pores is 0.05-5 mm.

4. The porous metal according to claim 1, characterized in that: The thickness of the metal layer of the metal skeleton is 1-1000 μm.

5. The porous metal according to claim 1, characterized in that: The thickness of the porous metal is 0.005-65 mm.

6. The porous metal according to claim 1, characterized in that: The metal deposition layer is a multi-modal metal deposition layer composed of grains of multiple different sizes.

7. The porous metal according to claim 1, characterized in that: The metal deposition layer is a single metal material formed by any one of iron, nickel, copper, iron, aluminum, chromium, cadmium, germanium, tin, lead, zinc, gold, silver, titanium, cobalt, vanadium, niobium, hafnium, tantalum, bismuth, molybdenum, tungsten, manganese, platinum, palladium, ruthenium, rhodium, iridium, and osmium, or a multilayer metal material or alloy material formed by two or more of the above metals.

8. The porous metal according to claim 1, characterized in that: The porous metal is a three-dimensional porous metal.

9. The porous metal according to claim 1, characterized in that: The porous metal is a two-dimensional porous metal.

10. The method for producing a porous metal according to any one of claims 1 to 9, characterized in that: The following steps are included: (1) Directed conductive treatment: Using organic polymer porous material as a template, the outer surface of the template is partially conductive by directional deposition or directional coating of a conductive layer, so that the outer surface of the template is not completely surrounded by the conductive layer; (2) removing the template to obtain a semi-finished product that does not contain organic polymer porous materials; (3) High-temperature reduction sintering: The semi-finished product obtained in step (2) is placed in a reducing or protective atmosphere for treatment at a temperature of 400-1500°C for a time of 20-200 minutes to obtain a porous metal product.

11. The manufacturing method according to claim 10, characterized in that: The method for removing the template in step (2) is one or more of incineration, thermal decomposition and dissolution.

12. The manufacturing method according to claim 11, characterized in that: The incineration method refers to heating the organic polymer material with the metal layer on the surface at a temperature of 300-700° C. to burn and remove the organic polymer material.

13. The manufacturing method according to claim 10, characterized in that: The method of directional deposition or directional coating of the conductive layer is to deposit or coat the conductive layer only on one side of the template, leaving the other side non-conductive.

14. The manufacturing method according to claim 10, characterized in that: The directional deposition refers to vacuum plating, chemical plating or electroplating.

15. The manufacturing method according to claim 10, characterized in that: The directional coating refers to spraying, scraping, dipping, rolling or brushing.

16. The manufacturing method according to claim 10, characterized in that: The reducing atmosphere refers to a hydrogen atmosphere, a mixed atmosphere of hydrogen and nitrogen, or a mixed atmosphere of hydrogen and argon.

17. The manufacturing method according to claim 10, characterized in that: The protective atmosphere refers to a nitrogen atmosphere, an argon atmosphere or a mixed atmosphere of nitrogen and argon.

18. The manufacturing method according to claim 10, characterized in that: After the surface of the semi-finished product obtained in step (2) is reprocessed once or multiple times, step (3) is then performed, wherein the reprocessing refers to conductive deposition, coating or spraying.

19. The manufacturing method according to claim 10, characterized in that: The surface of the porous metal product obtained in step (3) is reprocessed once or multiple times, wherein the reprocessing refers to conductive deposition, coating or spraying treatment.

20. The manufacturing method according to claim 10, characterized in that: After the surface of the porous metal product obtained in step (3) is reprocessed multiple times, the high-temperature reduction sintering treatment of step (3) is performed again, and the reprocessing and high-temperature reduction sintering treatment are cycled multiple times; the reprocessing refers to conductive deposition or coating or spraying treatment.

21. The manufacturing method according to claim 10, characterized in that: The organic polymer porous material is selected from one or more of polyurethane sponge, porous polyester PET, porous polyethylene PE, porous polypropylene PP, porous polyphenylene sulfide PPS, porous polycarbonate and porous polyimide.

22. The manufacturing method according to claim 10, characterized in that: The organic polymer porous material is selected from one or more of polymer non-woven fabrics, polymer woven fabrics, and polymer felt.

23. The manufacturing method according to claim 10, characterized in that: The directional coating of the conductive layer refers to coating of carbon-based paint, conductive metal-based paint or a mixture thereof.