An organic compound and its application
By using organic compounds with a spirofluorene structure and triazine substituents in organic electroluminescent devices, the problems of low efficiency and short life of electron transport materials are solved, and organic electroluminescent devices with high efficiency and long life are realized.
Patent Information
- Application Number
- CN202310102999.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-10
AI Technical Summary
The electron transport materials in existing organic electroluminescent devices have low efficiency and short lifespan, making it difficult to meet the market's demand for high efficiency and long lifespan.
Organic compounds with a spirofluorene structure and triazine substituents are used as electron transport materials to increase the distance between molecules through the spiro ring steric hindrance effect, forming an amorphous disordered film, optimizing the HOMO/LUMO energy level of the molecule, and improving the electron mobility , improve the electron-hole imbalance problem.
The luminous efficiency of the organic electroluminescent device is improved, the driving voltage is reduced, and the service life of the device is extended.
Smart Images

Figure CN116041268B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of organic photoelectric materials and relates to an organic compound and application thereof. Background Art
[0002] Organic electroluminescence (EL) refers to a phenomenon in which organic materials directly convert electrical energy into light energy under the action of an electric field. It has the characteristics of self-luminescence, bright colors, thin thickness, light weight, fast response speed, wide viewing angle, low driving voltage, tolerance to harsh natural conditions, and can be made into flexible panels. It has gradually developed into the most advantageous technology in the field of new generation flat panel displays.
[0003] Research on organic electroluminescent devices (OEL), namely organic light-emitting diodes (OLED), began in the 1950s. A general organic electroluminescent device is composed of a cathode, an anode and an organic layer between the two. Generally, the anode is transparent ITO, and the cathode is composed of LiAl and the like. The organic layer includes a hole injection layer (HIL), a hole transport layer (HTL), an electron blocking layer (EBL), a light-emitting layer (EL), a hole blocking layer (HBL), an electron transport layer (ETL), and an electron injection layer (EIL). A voltage is formed between the two electrodes, electrons are injected from the cathode on one side, and holes are injected from the anode on the other side. The injected electrons and holes are recombined in the light-emitting layer, and the electronic state changes from the ground state to the excited state. Because the excited state is extremely unstable, the excited state returns to the stable ground state. At this time, energy is released in the form of light.
[0004] As the market demand for organic EL devices continues to increase, devices with high efficiency and long life have become a development trend. However, it is very difficult to find suitable materials. Tris(8-hydroxyquinoline)aluminum (Alq3) has been used as an electron transport material for nearly 30 years since its invention, and there is a lot of data proving that it is superior to conventional materials. However, as an electron transport material, its application is restricted by factors such as migration to other layers.
[0005] Therefore, developing a new type of electron transport material that meets the requirements of practicality has become a technical problem that people in this field urgently need to solve. Summary of the invention
[0006] In view of the shortcomings of the prior art, the object of the present invention is to provide an organic compound and its application. The organic compound of the present invention can make the organic electroluminescent device have excellent luminous efficiency, low driving voltage and long service life.
[0007] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0008] In one aspect, the present invention provides an organic compound having a structure as shown in the following formula I:
[0009]
[0010] Wherein, m and n are 0 or 1, and m and n are not 0 at the same time;
[0011] L1 and L2 are the same or different and each independently represents a single bond, a substituted or unsubstituted C6-C 30 Arylene, substituted or unsubstituted 3-20-membered heteroarylene, wherein the heteroatom is selected from oxygen, nitrogen or sulfur;
[0012] Ar1, Ar2, Ar3 and Ar4 are the same as or different from each other and each independently represents a substituted or unsubstituted C3-C 30 Cycloalkyl, substituted or unsubstituted 3-20-membered heterocycloalkyl, whose heteroatom is selected from oxygen, nitrogen or sulfur; substituted or unsubstituted C6-C 30 aryl or substituted or unsubstituted 3-30-membered heteroaryl, whose heteroatom is selected from oxygen, nitrogen or sulfur; substituted or unsubstituted 3-15-membered heteroarylamine, whose heteroatom is selected from oxygen, nitrogen or sulfur; substituted or unsubstituted C6-C 60 Arylamine, substituted or unsubstituted C6-C 60 Aryloxy, substituted or unsubstituted C 10 ~C 30 Condensed ring group, substituted or unsubstituted C5-C 30 One or a combination of at least two of the spirocyclic groups.
[0013] In the present invention, the organic compound parent core is a spirofluorene structure, as an electron transmission organic electroluminescent compound material, through the steric effect of the spiro ring, the intermolecular distance is increased, so that the molecules are not easy to crystallize and not easy to aggregate, which is conducive to forming an amorphous disordered film. At the same time, compared to the prior art, the spiro ring structure adopts a fluorene spiro ring, because the presence of C hybridized with SP3 on the spiro ring effectively shortens the conjugated interval of the overall molecule while ensuring the increase in molecular weight, and it is easier to adjust the HOMO / LUMO energy level of the molecule, and other layer materials (such as main materials, injection layer materials) can be effectively matched. And the side chain is a triazine structure is a functional group with strong electron-withdrawing ability, and the functional group with strong electron-withdrawing ability adopted can effectively improve the electron mobility of the electron transmission material. Improve the problem of electron-hole imbalance inside the organic electroluminescent device, improve luminous efficiency, reduce driving voltage, and extend device life.
[0014] Preferably, L1 and L2 represent a single bond or a substituted or unsubstituted phenyl, naphthyl, tolyl, phenanthryl, anthracenyl, biphenyl, triphenylene, pyrenyl, spirobifluorenyl, peryl, indenyl, azulenyl, triphenylene, pyrrolyl, furanyl, oxazolyl, isoxazolyl, thienyl, thiazolyl, isothiazolyl, thiadiazolyl, oxadiazolyl, imidazolyl, pyrazolyl, triazole, pyridazinyl, pyrazinyl, pyridinyl, pyrimidinyl, triazinyl, indolyl, quinolyl, isoquinolyl, acridinyl, purinyl, pteridinyl, benzofuranyl, benzothiophenyl, benzimidazolyl, benzothiazolyl, benzotriazolyl, benzoxadiazolyl, benzoxazolyl, cinnoline, quinoxalinyl, dibenzofuranyl, dibenzothiophenyl, carbazolyl, phenanthrolinyl, indolizinyl, naphthyridinyl or phthalazinyl.
[0015] More preferably, L1 and L2 represent a single bond, phenyl, naphthyl, biphenyl, terphenyl, phenylnaphthyl or tolyl.
[0016] Preferably, the Ar1-Ar4 are the same as or different from each other, and are each independently represented by the following groups:
[0017]
[0018]
[0019] Wherein, R4 represents a substituted or unsubstituted C6-C 20 Aryl, substituted or unsubstituted 3- to 10-membered heteroaryl, wherein the heteroatom is selected from oxygen, nitrogen or sulfur; * represents the attachment site of the group.
[0020] In the present invention, the term "substituted" refers to substitution by one or at least two substituents selected from the following: deuterium, cyano, halogen, nitro, hydroxyl, phosphate, borane, silicon, C1-C8 alkyl, C2-C 15 Alkenyl, C2-C 10 Alkynyl, C6-C 20 Aryl, C3-C 10 Heteroaryl, C1-C 10 Alkoxy, C6-C 20 Arylamino.
[0021] In the present invention, the range of the number of carbon atoms in the defined group represents any integer within the defined range, for example, C6-C30 means that the number of carbon atoms can be 6, 8, 10, 13, 16, 19, 20, 23, 25, 28 or 30, etc., C3-C30 means that the number of carbon atoms can be 3, 5, 6, 8, 10, 12, 14, 16, 18, 20, 22, 24, 25, 28 or 30, etc., and so on.
[0022] Preferably, the organic compound is any one of the following compounds 1-282:
[0023]
[0024]
[0025]
[0026]
[0027]
[0028]
[0029]
[0030]
[0031]
[0032]
[0033]
[0034]
[0035]
[0036]
[0037]
[0038]
[0039]
[0040]
[0041]
[0042] For the specific implementation of the present invention, a preparation method known to a person skilled in the art is now provided. It is worth noting that the preparation method does not limit the preparation method of the electron transport type organic electroluminescent compound disclosed in the present invention, and all preparation methods obtained by synthetic methods known to a person skilled in the art and without creative labor belong to the prior art in the field of the preparation method of the present invention.
[0043] The synthetic route of the organic compound of the present invention as described above is as follows:
[0044]
[0045]
[0046] Wherein Hal1, Hal2, and Hal3 represent halogen, such as chlorine or bromine. Specific implementation steps:
[0047] Step 1: Dissolve the raw material 1 in dichloromethane, add pyridine, protect with nitrogen, and stir at -20°C for 10 minutes. Add trifluoromethanesulfonic anhydride dropwise, react at low temperature for 1 hour, gradually raise the room temperature to react overnight. Post-treatment process: Add about 200mL of deionized water to wash twice, then wash once with sodium bicarbonate aqueous solution, and finally wash once with water, dry with anhydrous magnesium sulfate for 10-20 minutes, filter, and spin dry to obtain a yellow oil. Pass through the column, first use dichloromethane: petroleum ether = 1:4 to flush out impurities, then use dichloromethane: petroleum ether = 1:1 to flush out the product point, collect, and spin dry to obtain the compound shown in intermediate 1.
[0048] Step 2: Add intermediate 1 and raw material 2 to the reaction bottle, then add catalyst tetratriphenylphosphine palladium and potassium carbonate, and finally add to a mixed solvent of toluene, ethanol, and deionized water, protect with nitrogen, and react at 90-100°C for 18-24 hours. Post-treatment process: cool down, separate liquid at rest, wash the organic layer with water once, spin dry the organic solution to obtain a dark oil. The product is purified by column, rinsed with pure petroleum ether, the product spot is collected, and spin dried to obtain the compound shown in intermediate 2.
[0049] Step 3: Dissolve intermediate 2 in anhydrous tetrahydrofuran and stir for 30-40 minutes under nitrogen protection at -78°C. Inject n-butyl lithium (2.5 mol / L) to react for 2-4 hours, then slowly add raw material 3 to react at low temperature for 1-2 hours, and place the reaction bottle at room temperature to react overnight. Post-treatment process: Add deionized water and stir, separate the liquids, extract the water layer with ethyl acetate once, combine the organic layers, and dry over anhydrous magnesium sulfate. Spin dry to obtain a yellow oil, purify it through a column, rinse out the target product, and spin dry to obtain the compound shown in intermediate 3.
[0050] Step 4: Dissolve intermediate 3 in dichloromethane and stir at 0°C for 10-20 minutes. At the same time, weigh polyphosphoric acid and add it to anhydrous ethanol, stir evenly to prepare a mixed solution for use. Add methanesulfonic acid (MSA) to the reaction solution and react for 30-40 minutes, then add a mixture of polyphosphoric acid and ethanol and react for 10-20 minutes. Then heat the reaction to 60°C and reflux for 1 hour, stop heating and react overnight. Post-treatment process: Solid precipitates, filter to obtain a white solid, wash with petroleum ether, and dry to obtain intermediate 4.
[0051] Step 5: Under nitrogen protection, the intermediate 4 and the raw material 4 are dissolved in a mixed solution of toluene, ethanol and water, cesium carbonate, palladium catalyst, phosphine ligand are added, stirred evenly, heated and refluxed to react, and the intermediate 5 is prepared;
[0052] Step 6: Under nitrogen protection, the intermediate 5 and the raw material 5 are dissolved in a mixed solvent of toluene, ethanol and water, cesium carbonate, palladium catalyst, phosphine ligand are added, stirred evenly, heated and refluxed to react, and chemical formula 1 is prepared;
[0053] Note: When m=0, n=1 and m=1, n=0, the compound shown in Chemical Formula 1 can be obtained in the fifth step.
[0054] In another aspect, the present invention provides an electron transport material, wherein the electron transport material comprises any one or a combination of at least two of the organic compounds described above.
[0055] In another aspect, the present invention provides an organic electroluminescent device, comprising a first electrode, a second electrode, and an organic thin film layer disposed between the first electrode and the second electrode, wherein the organic thin film layer comprises the organic compound having the chemical formula I as described above.
[0056] Preferably, the organic thin film layer comprises an electron transport layer, and the electron transport layer comprises the organic compound as described above.
[0057] Preferably, the organic thin film layer further comprises any one layer or a combination of at least two layers of a hole injection layer, a hole transport layer, an electron blocking layer, a light emitting layer, a hole blocking layer or an electron injection layer.
[0058] In another aspect, the present invention provides a display panel, comprising the organic electroluminescent device as described above.
[0059] In another aspect, the present invention provides an electronic device, comprising the display panel as described above.
[0060] Compared with the prior art, the present invention has the following beneficial effects:
[0061] The organic compound of the present invention has a spirofluorene structure and has a triazine substituent at a specific position. The steric effect of the spiro ring increases the distance between molecules, making it difficult for the molecules to crystallize and aggregate, thereby being conducive to forming an amorphous disordered film. The spiro ring structure adopts a fluorene spiro ring. Because of the presence of SP3 hybridized C on the spiro ring, while ensuring the increase of the molecular weight, the conjugation interval of the overall molecule is effectively shortened, and the HOMO / LUMO energy level of the molecule is more easily adjusted. When used as an electron transport material, it can effectively match other layer materials (such as a main material and an injection layer material), and the side chain triazine substituent is a functional group with strong electron-withdrawing ability. The adopted functional group with strong electron-withdrawing ability can effectively improve the electron mobility of the electron transport material. The problem of electron-hole imbalance inside the organic electroluminescent device is improved, the luminous efficiency is improved, the driving voltage is reduced, and the device life is extended. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 This is the H NMR spectrum of compound 3 prepared in Example 1. DETAILED DESCRIPTION
[0063] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0064] Example 1
[0065]
[0066] Step 1: Dissolve the raw material 1 (1.0 eq) in 500 mL of dichloromethane, add pyridine (3.0 eq), protect with nitrogen, and stir at -20 ° C for 10 minutes. Add trifluoromethanesulfonic anhydride (1.5 eq) dropwise, react at low temperature for 1 hour, gradually raise the room temperature to react overnight. Post-treatment process: Add about 200 mL of deionized water to wash twice, then wash once with sodium bicarbonate aqueous solution, and finally wash once with water, dry with anhydrous magnesium sulfate for 10 minutes, filter, and spin dry to obtain a yellow oil. Pass through the column, first use dichloromethane: petroleum ether = 1:4 to flush out impurities, then use dichloromethane: petroleum ether = 1:1 (volume ratio) to flush out the product point, collect, and spin dry to obtain a light yellow-green oil, which is the compound shown in intermediate 1 (yield 50.4%).
[0067] Step 2: Add intermediate 1 (1.0 eq) and raw material 2 (1.2 eq) to a reaction bottle, then add catalyst tetrakis triphenylphosphine palladium (0.01 eq) and potassium carbonate (2.0 eq), and finally add 300 mL of toluene, 100 mL of ethanol, and 200 mL of deionized water, under nitrogen protection, react at 90 ° C for 24 hours. Post-processing process: cool down, separate liquid at rest, wash the organic layer with water once, spin dry the organic solution to obtain a dark oil. The product is purified by column, rinsed with pure petroleum ether, the product spot is collected, and spin dried to obtain a colorless oil, which is the compound shown in intermediate 2 (yield 67.2%).
[0068] Step 3: Dissolve intermediate 2 (1.0 eq) in 300 mL of anhydrous tetrahydrofuran and stir for 30 minutes at -78 °C under nitrogen protection. Inject n-butyl lithium (2.5 mol / L) (1.1 eq) and react for 2 hours, then slowly add raw material 3 (1.2 eq) and react at low temperature for 1 hour, and place the reaction bottle at room temperature to react overnight. Post-treatment process: Add 70 mL of deionized water and stir for 10 minutes, separate the liquids, extract the water layer with ethyl acetate once, combine the organic layers, and dry over anhydrous magnesium sulfate. Spin dry to obtain a yellow oil, purify it through a column, rinse out the target product with dichloromethane: petroleum ether = 1:4, and spin dry to obtain a colorless oil, which is the compound shown in intermediate 3 (yield 57.9%).
[0069] Step 4: Dissolve intermediate 3 (1.0 eq) in 300 mL of dichloromethane and stir at 0°C for 10 minutes. At the same time, weigh 0.15 mol of polyphosphoric acid and add it to 180 mL of anhydrous ethanol, stir evenly to prepare a mixed solution for use. Add methanesulfonic acid (10.0 eq) to the reaction solution and react for 30 minutes, then add a mixture of polyphosphoric acid and ethanol and react for 10 minutes. Then heat the reaction to 60°C and reflux for 1 hour, stop heating and react overnight. Post-treatment process: Solid precipitates, filter to obtain a white solid, wash with petroleum ether, and dry to obtain the product, which is the compound shown in intermediate 4 (yield 39.7%).
[0070] Step 5: Under nitrogen protection, the intermediate 4 (1.0 eq) and the raw material 4 (1.0 eq) were dissolved in a mixed solution of toluene, ethanol and water, cesium carbonate (2.0 eq), palladium catalyst (0.01 eq), phosphine ligand 7 (0.05 eq) were added, stirred evenly, heated and refluxed to prepare compound 3 (yield 51.6%, Mw: 765.96);
[0071] The obtained compound-3 was tested and analyzed, and the results were as follows:
[0072] Its H NMR spectrum is Figure 1 shown.
[0073] HPLC purity: >99%.
[0074] MS (ESI, m / z): [M+H] + :766.98;
[0075] Elemental Analysis:
[0076] Calculated values: C, 89.38; H, 5.13; N, 5.49.
[0077] The test values are: C, 88.59; H, 5.36; N, 5.68.
[0078] Example 2
[0079]
[0080] Step 1: Dissolve the raw material 1 (1.0 eq) in 500 mL of dichloromethane, add pyridine (3.0 eq), protect with nitrogen, and stir at -20°C for 10 minutes. Add trifluoromethanesulfonic anhydride (1.5 eq) dropwise, react at low temperature for 1 hour, gradually raise the room temperature to react overnight. Post-treatment process: Add about 200 mL of deionized water to wash twice, then wash once with sodium bicarbonate aqueous solution, and finally wash once with water, dry with anhydrous magnesium sulfate for 10 minutes, filter, and spin dry to obtain a yellow oil. Pass through the column, first use dichloromethane: petroleum ether = 1:4 to flush out impurities, then use dichloromethane: petroleum ether = 1:1 to flush out the product point, collect, and spin dry to obtain a light yellow-green oil, which is the compound shown in intermediate 1 (yield 50.6%).
[0081] Step 2: Add intermediate 1 (1.0 eq) and raw material 2 (1.2 eq) to a reaction bottle, then add catalyst tetrakis triphenylphosphine palladium (0.01 eq) and potassium carbonate (2.0 eq), and finally add 300 mL of toluene, 100 mL of ethanol, and 200 mL of deionized water, under nitrogen protection, react at 90 ° C for 24 hours. Post-processing process: cool down, separate liquid at rest, wash the organic layer with water once, spin dry the organic solution to obtain a dark oil. The product is purified by column, rinsed with pure petroleum ether, the product spot is collected, and spin dried to obtain a colorless oil, which is the compound shown in intermediate 2 (yield 67.8%).
[0082] Step 3: Dissolve intermediate 2 (1.0 eq) in 300 mL of anhydrous tetrahydrofuran and stir for 30 minutes at -78 ° C under nitrogen protection. Inject n-butyl lithium (2.5 mol / L) (1.1 eq) and react for 2 hours, then slowly add raw material 3 (1.2 eq) and react at low temperature for 1 hour, and place the reaction bottle at room temperature to react overnight. Post-treatment process: Add 70 mL of deionized water and stir for 10 minutes, separate the liquids, extract the water layer with ethyl acetate once, combine the organic layers, and dry over anhydrous magnesium sulfate. Spin dry to obtain a yellow oil, purify it through a column, rinse out the target product with dichloromethane: petroleum ether = 1:4, and spin dry to obtain a colorless oil, which is the compound shown in intermediate 3 (yield 59.3%).
[0083] Step 4: Dissolve intermediate 3 (1.0 eq) in 300 mL of dichloromethane and stir at 0°C for 10 minutes. At the same time, weigh 0.15 mol of polyphosphoric acid and add it to 180 mL of anhydrous ethanol, stir evenly to prepare a mixed solution for use. Add methanesulfonic acid (10.0 eq) to the reaction solution and react for 30 minutes, then add a mixture of polyphosphoric acid and ethanol and react for 10 minutes. Then heat the reaction to 60°C and reflux for 1 hour, stop heating and react overnight. Post-treatment process: Solid precipitates, filter to obtain a white solid, wash with petroleum ether, and dry to obtain the product, which is the compound shown in intermediate 4 (yield 41.7%).
[0084] Step 5: Under nitrogen protection, intermediate 4 (1.0 eq) and raw material 4 (1.0 eq) were dissolved in a mixed solution of toluene, ethanol and water, cesium carbonate (2.0 eq), palladium catalyst (0.01 eq), phosphine ligand (0.05 eq) were added, stirred evenly, heated and refluxed to prepare compound 91 (yield 59.2%, Mw: 613.76);
[0085] The obtained compound-91 was tested and analyzed, and the results were as follows:
[0086] HPLC purity: >99%.
[0087] MS (ESI, m / z): [M+H] + :614.80
[0088] Elemental Analysis:
[0089] Calculated values: C, 88.06; H, 5.09; N, 6.85.
[0090] The test values are: C, 87.65; H, 5.34; N, 7.01.
[0091] Example 3
[0092]
[0093] Step 1: Dissolve the raw material 1 (1.0 eq) in 500 mL of dichloromethane, add pyridine (3.0 eq), protect with nitrogen, and stir at -20°C for 10 minutes. Add trifluoromethanesulfonic anhydride (1.5 eq) dropwise, react at low temperature for 1 hour, gradually raise the room temperature to react overnight. Post-treatment process: Add about 200 mL of deionized water to wash twice, then wash once with sodium bicarbonate aqueous solution, and finally wash once with water, dry with anhydrous magnesium sulfate for 10 minutes, filter, and spin dry to obtain a yellow oil. Pass through the column, first use dichloromethane: petroleum ether = 1:4 to flush out impurities, then use dichloromethane: petroleum ether = 1:1 to flush out the product point, collect, and spin dry to obtain a light yellow-green oil, which is the compound shown in intermediate 1 (yield 51.2%).
[0094] Step 2: Add intermediate 1 (1.0 eq) and raw material 2 (1.2 eq) to a reaction bottle, then add catalyst tetrakis triphenylphosphine palladium (0.01 eq) and potassium carbonate (2.0 eq), and finally add 300 mL of toluene, 100 mL of ethanol, and 200 mL of deionized water, under nitrogen protection, react at 90 ° C for 24 hours. Post-processing process: cool down, separate liquid at rest, wash the organic layer with water once, spin dry the organic solution to obtain a dark oil. The product is purified by column, rinsed with pure petroleum ether, the product spot is collected, and spin dried to obtain a colorless oil, which is the compound shown in intermediate 2 (yield 71.5%).
[0095] Step 3: Dissolve intermediate 2 (1.0 eq) in 300 mL of anhydrous tetrahydrofuran and stir for 30 minutes at -78 °C under nitrogen protection. Inject n-butyl lithium (2.5 mol / L) (1.1 eq) and react for 2 hours, then slowly add raw material 3 (1.2 eq) and react at low temperature for 1 hour, and place the reaction bottle at room temperature to react overnight. Post-treatment process: Add 70 mL of deionized water and stir for 10 minutes, separate the liquids, extract the water layer with ethyl acetate once, combine the organic layers, and dry over anhydrous magnesium sulfate. Spin dry to obtain a yellow oil, purify it through a column, rinse out the target product with dichloromethane: petroleum ether = 1:4, and spin dry to obtain a colorless oil, which is the compound shown in intermediate 3 (yield 57.4%).
[0096] Step 4: Dissolve intermediate 3 (1.0 eq) in 300 mL of dichloromethane and stir at 0°C for 10 minutes. At the same time, weigh 0.15 mol of polyphosphoric acid and add it to 180 mL of anhydrous ethanol, stir evenly to prepare a mixed solution for use. Add methanesulfonic acid (10.0 eq) to the reaction solution and react for 30 minutes, then add a mixture of polyphosphoric acid and ethanol and react for 10 minutes. Then heat the reaction to 60°C and reflux for 1 hour, stop heating and react overnight. Post-treatment process: Solid precipitates, filter to obtain a white solid, wash with petroleum ether, and dry to obtain the product, which is the compound shown in intermediate 4 (yield 41.5%).
[0097] Step 5: Under nitrogen protection, intermediate 4 (1.0 eq) and raw material 4 (1.0 eq) were dissolved in a mixed solution of toluene, ethanol and water, cesium carbonate (2.0 eq), palladium catalyst (0.01 eq), phosphine ligand (0.05 eq) were added, stirred evenly, heated and refluxed to prepare compound 130 (yield 61.6%, Mw: 806.03);
[0098] The obtained compound-130 was tested and analyzed, and the results were as follows:
[0099] HPLC purity: >99%.
[0100] MS (ESI, m / z): [M+H] + :807.06
[0101] Elemental Analysis:
[0102] Calculated values: C, 89.41; H, 5.38; N, 5.21.
[0103] The test values are: C, 88.98; H, 5.51; N, 5.36.
[0104] The following compounds were synthesized by referring to the synthesis methods of Examples 1 to 3. Their molecular formulas and mass spectrometry characterization data are shown in Table 1 below:
[0105] Table 1
[0106]
[0107]
[0108] Device Example 1 Organic electroluminescent device
[0109] The structure of the OLED device is: ITO anode / HIL / HTL / EBL / EML / HBL / ETL / EIL / cathode / light extraction layer.
[0110] a. ITO anode: the coating thickness is The ITO (indium tin oxide)-Ag-ITO (indium tin oxide) glass substrate was cleaned twice in distilled water, ultrasonically cleaned for 30 minutes, and then repeatedly cleaned twice with distilled water, ultrasonically cleaned for 10 minutes. After washing, it was ultrasonically cleaned with methanol, acetone, and isopropanol in sequence (5 minutes each time), dried, and then transferred to a plasma cleaning machine for washing for 5 minutes. It was then sent to a vapor deposition machine, and the substrate was used as the anode, and other functional layers were deposited thereon in sequence.
[0111] b. HIL (hole injection layer): The evaporation rate of HT-1 and P-dopant was vacuum evaporated as hole injection layer materials, and the chemical formula thereof is shown below. The evaporation rate ratio of HT-1 and P-dopant was 97:3, and the thickness was 10 nm;
[0112] c. HTL (hole transport layer): At a deposition rate of 100%, 130 nm of HT-1 was vacuum-deposited on the hole injection layer as a hole transport layer.
[0113] d. EBL (electron blocking layer): At a deposition rate of 10 nm, EB-1 was vacuum-deposited on the hole transport layer as a light-emitting auxiliary layer.
[0114] e. EML (light-emitting layer): Then on the above-mentioned light-emitting auxiliary layer, The evaporation rate of Host-1 and Dopant-1 is 98:2. The host material (Host-1) and dopant material (Dopant-1) with a thickness of 20nm are vacuum evaporated as the light-emitting layer. The chemical formulas of Host-1 and Dopant-1 are as follows.
[0115] f. HBL (hole blocking layer): The hole blocking layer HB with a thickness of 5.0 nm was vacuum deposited at a deposition rate of .
[0116] g. ETL (Electron Transport Layer): The compound 3 provided in the above embodiment is vacuum evaporated to a thickness of 35 nm as an electron transport layer.
[0117] h. EIL (electron injection layer): At a evaporation rate of , a 1.0 nm Yb film layer was evaporated to form an electron injection layer.
[0118] i. Cathode: The evaporation rate ratio is 1:9, and magnesium and silver are evaporated at 18nm, and the evaporation rate ratio is 1:9 to obtain an OLED device.
[0119] j. Light extraction layer: At a deposition rate of , CPL with a thickness of 70 nm was vacuum-deposited on the cathode as a light extraction layer.
[0120] k. Then the vapor-deposited substrate is packaged. First, the cleaned cover is coated with UV glue using glue coating equipment, and then the coated cover is moved to the pressing section, the vapor-deposited substrate is placed on the upper end of the cover, and finally the substrate and cover are bonded by bonding equipment, and the UV glue is cured by light.
[0121] The structure of the compound used in the preparation process of the organic electroluminescent device is shown below:
[0122]
[0123] Organic electroluminescent devices of device embodiments 2-29 were prepared according to the above-mentioned method for preparing an organic electroluminescent device, except that compound 3 in device embodiment 1 was replaced by compounds 91, 130, 1, 4, 7, 11, 15, 18, 20, 26, 32, 48, 56, 68, 77, 85, 92, 102, 137, 149, 167, 189, 203, 230, 239, 248, 268, and 281 as electron transport layers to prepare device embodiments 2 to 29.
[0124] In order to further demonstrate the beneficial effects of the present invention and to better understand the present invention, the properties and application performances of the electron transport organic electroluminescent compounds and devices containing the same described in the present invention are further illustrated by the following comparative examples, but they should not be construed as limitations on the present invention. The product properties obtained by other measurement experiments performed by technicians in this field based on the above invention content and the applications based on the above properties are also considered to fall within the protection scope of the present invention.
[0125] Comparative Examples 1 to 5
[0126] The organic electroluminescent device was prepared according to the above-mentioned method for preparing the organic electroluminescent device, except that the existing comparative compounds a, b, c, d, and e were used to replace the electron transport layer (compound 3) in the above-mentioned device embodiment 1 for evaporation, and the device comparative examples 1-5 were prepared. Among them, the chemical structural formulas of the comparative compounds a, b, c, d, and e are:
[0127]
[0128] The driving voltage and luminous efficiency of the organic electroluminescent devices prepared in device embodiments 1 to 29 and device comparison examples 1 to 5 were tested using IVL testing equipment at a brightness of 1000 (nits), and the life of the devices was tested using a life testing device (model: D3000-96). The test results are shown in Table 2 below.
[0129] Table 2 Test results of luminous properties of organic electroluminescent devices (brightness value is 1000 nits)
[0130]
[0131]
[0132]
[0133] Note: In blue top-emitting devices, the current efficiency is greatly affected by chromaticity. Therefore, the influence of chromaticity on efficiency is taken into account, and the ratio of current efficiency to CIEy is defined as BI value, that is, BI = (cd / A) / CIEy.
[0134] As can be seen from Table 2, the organic electroluminescent device prepared by using the organic electroluminescent compound provided by the present invention as the electron transport layer has a lower starting voltage (below 3.47V), and the luminous efficiency (above 8.02cd / A) and life (above 487h) are significantly improved compared with the organic electroluminescent device prepared by using compounds a, b, c, d, and e as the electron transport layer.
[0135] The applicant declares that the present invention illustrates the process method of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned process steps, that is, it does not mean that the present invention must rely on the above-mentioned process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. An organic compound, characterized in that The organic compound has a structure as shown in the following formula I: Wherein, m and n are 0 or 1, and m and n are not 0 at the same time; L1 and L2 are the same or different and are each independently a single bond, phenyl, naphthyl, biphenyl, terphenyl, phenylnaphthyl or tolyl; Ar1-Ar4 are the same as or different from each other, and are each independently represented by the following groups: * represents the attachment site of the group.
2. An organic compound, characterized in that The organic compound is any one of the following compounds:
3. An electron transport material, characterized in that The electron transport material comprises any one or a combination of at least two of the organic compounds as described in claim 1 or 2.
4. An organic electroluminescent device, characterized in that: The organic electroluminescent device comprises a first electrode, a second electrode and an organic thin film layer disposed between the first electrode and the second electrode, wherein the organic thin film layer comprises the organic compound as claimed in claim 1 or 2.
5. The organic electroluminescent device according to claim 4, characterized in that: The organic thin film layer comprises an electron transport layer, and the electron transport layer comprises the organic compound as claimed in claim 1 or 2.
6. The organic electroluminescent device according to claim 5, characterized in that: The organic thin film layer further comprises any one of a hole injection layer, a hole transport layer, an electron blocking layer, a light emitting layer, a hole blocking layer or an electron injection layer, or a combination of at least two layers.
7. A display panel, characterized in that: The display panel comprises the organic electroluminescent device according to any one of claims 4 to 6.
8. An electronic device, characterized in that: The electronic device comprises the display panel according to claim 7.
Citation Information
Patent Citations
Condensed-cyclic compound and organic light-emitting diode including the condensed-cyclic compound
CN103664749A