Catalyst component and preparation method thereof, catalyst system and application thereof
By adding halogen-containing inert reagents and controlling magnesium phase dispersion during the preparation of catalyst components, the problems of uneven catalyst particle size and adhesion were solved, achieving high efficiency, stability and excellent performance of the catalyst, which is suitable for the field of olefin polymerization.
Patent Information
- Application Number
- CN202111264987.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-10-28
AI Technical Summary
Existing technologies make it difficult to prepare supported Ziegler-Natta catalysts with uniform particle size distribution that do not contain rod-shaped, bulk, or agglomerated materials, and these catalysts are prone to causing unstable operation of the equipment during polymerization.
By adding a halogen-containing inert reagent to a magnesium-containing solution and avoiding mixing with an inert dispersion medium before mixing with titanium compounds, the dispersion and crystallization process of the magnesium phase is controlled. A precipitant and a surfactant are used for heating treatment to form a spherical catalyst component.
This achieves uniform particle size distribution and morphological stability of the catalyst components, avoids adhesion, improves catalyst activity and stereotactic orientation, and ensures the stability of the polymerization process.
Smart Images

Figure CN116041578B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of catalysts, and specifically relates to catalyst components and preparation methods thereof, catalyst systems and applications thereof. Background Art
[0002] Supported Ziegler-Natta catalysts are widely developed because their morphology can be regulated by the carrier morphology, especially olefin polymerization catalysts supported by magnesium chloride carriers. The preparation of catalysts with good particle morphology is beneficial to the operation of industrial devices and has always been one of the keys to catalyst development. Currently, there are many technologies that can prepare olefin polymerization catalyst components with good morphology.
[0003] One of them is to first prepare a magnesium compound or a complex solid, then contact it with a titanium-containing compound to generate a titanium- and magnesium-containing catalyst solid, and load an internal electron donor compound to form a catalyst component. The morphology and particle size distribution of the catalyst in this type of technology are determined by the pre-prepared magnesium compound or complex solid. For example, well-known high-speed stirring technology, high-pressure extrusion technology, spray technology, supergravity technology, etc. are all used to prepare such solids, which can usually be spherical. However, these technologies usually have high energy consumption and complex processes, and cannot produce catalyst components in a continuous manner.
[0004] Another type of preparation technology is to first obtain a magnesium compound or a magnesium-containing solution of a complex, then contact it with a titanium-containing compound, crystallize and precipitate a catalyst solid containing titanium and magnesium, and load an internal electron donor compound to form a catalyst component. The morphology and particle size distribution of this type of catalyst are controlled by the crystallization precipitation process of the solution. For example, the early disclosed patents such as CN85100997A and CN1097597C precipitate a granular catalyst with a wide particle size distribution and poor particle shape. In recent years, disclosed patents such as CN103619475B and CN107207657A control the crystallization process through emulsion technology, and precipitate a spherical solid, and the morphology has been greatly improved, but the catalyst still has some shortcomings. Specifically, CN103619475B and CN107207657A complete phase separation through solvent selection means, that is, by significantly reducing toluene and adding non-aromatic hydrocarbons such as hexane to promote the non-polar solvent phase and polar magnesium phase separation into two phases. Therefore, the magnesium phase is extracted from the solvent phase, and the viscosity is very high. Even if an emulsifier is used to stabilize the magnesium phase, it will cause stickiness and adhesion during the precipitation process, and it is easy to form rod-shaped materials, large blocks and adhesion materials. Especially in the scale-up preparation, the problem will be more prominent. In addition, this phenomenon of the catalyst is easy to produce coarse powder during polymerization, and the coarse powder is easy to break into fine powder, which is very unfavorable for the stable operation of the polymerization device. Summary of the invention
[0005] The object of the present invention is to provide an olefin polymerization catalyst component, the particle size distribution of the catalyst component is uniform, does not contain rod-shaped materials, large blocks and sticking materials, and the catalyst performance is excellent, with high activity and stereospecific ability. Another object of the present invention is to provide a method for preparing the catalyst component of the present invention. The method of the present invention can more stably control the magnesium phase, avoid the stickiness and adhesion of particles during the precipitation process, and eliminate the rod-shaped materials, large blocks and sticking materials of the catalyst. The present invention also aims to provide the application of the catalyst system of the present invention.
[0006] The above-mentioned object of the present invention is achieved through the following technical solutions.
[0007] In a first aspect, the present invention provides a method for preparing a catalyst component, comprising the following steps:
[0008] (1) mixing a magnesium halide compound, an organic epoxy compound, an organic phosphorus compound and optionally a hydroxyl-containing compound with a halogen-containing inert reagent and an organic solvent to form a magnesium-containing solution;
[0009] (2) mixing an inert dispersion medium with a titanium-containing compound to form a titanium-containing solution;
[0010] (3) mixing the magnesium-containing solution with the titanium-containing solution to form a mixture;
[0011] (4) in the presence of a precipitation aid and a surfactant, heating the mixture to precipitate a spherical solid;
[0012] (5) Mixing the spherical solid object with an internal electron donor compound to obtain the catalyst component.
[0013] The inventors unexpectedly found that the method of the present invention can more stably control the magnesium phase, avoid particle sticking and adhesion during precipitation, and eliminate rods, lumps and adhesions of the catalyst. Without wishing to be bound by theory, this may be attributed to the method of the present invention (i) adding a halogen-containing inert agent to the magnesium-containing solution; and (ii) the present invention uses the magnesium-containing solution without mixing it with an inert dispersion medium before mixing it with the titanium compound.
[0014] Specifically, the inventors have found that the dispersed phase containing the magnesium phase in the two-phase system is dispersed in the solvent continuous phase, and the magnesium phase has high viscosity and high concentration, is not easy to disperse and is very easy to recombine and adhere, which is the main reason for the catalyst group to analyze rod-shaped materials, bulk materials and adhesion materials. The inventors unexpectedly found that: on the one hand, the halogen-containing inert reagent is more easily soluble in the magnesium phase than the halogen-free inert reagent. When the halogen-containing inert reagent is added to the two-phase system, the halogen-containing inert reagent in the dispersed phase is not easily extracted and enters the continuous phase, so that the viscosity and concentration of the dispersed phase can be adjusted by the halogen-containing inert reagent. Therefore, adding a halogen-containing inert reagent in the preparation of the catalyst component can better control the emulsion droplets, so that the crystallization process of the particles will be more stable, and the precipitated particles are also more uniform, reducing the sticking phenomenon. On the other hand, after the magnesium-containing solution is mixed with the inert dispersion medium, the magnesium phase is gradually or quickly separated from the dispersion medium, and in the subsequent mixing process with the titanium compound, the adhesion problem of the magnesium phase will be faced. Therefore, the present invention adopts a method in which the magnesium-containing solution is not mixed with an inert dispersion medium before being mixed with the titanium compound to avoid magnesium phase separation, which can further reduce the stickiness phenomenon.
[0015] Preferably, in the method for preparing the catalyst component of the present invention, the general formula of the magnesium halide compound is MgX 2 , wherein X is bromine, chlorine or iodine. The magnesium halide compound may be at least one of magnesium dichloride, magnesium dibromide and magnesium diiodide, preferably magnesium dichloride.
[0016] Preferably, in the method for preparing the catalyst component of the present invention, the organic epoxy compound is selected from one or more of the oxidation products of C2-C8 aliphatic olefins or C2-C8 halogenated aliphatic olefins.
[0017] Preferably, in the method for preparing the catalyst component described in the present invention, the organic epoxy compound is selected from one or more of ethylene oxide, propylene oxide, ethylene oxide, epichlorohydrin, butylene oxide, butadiene oxide, butadiene dioxide, methyl glycidyl ether and diglycidyl ether, more preferably epichlorohydrin.
[0018] Preferably, in the method for preparing the catalyst component of the present invention, the organophosphorus compound is selected from one or more of the compounds represented by formula (I) and formula (II):
[0019]
[0020] Among them, R 1 , R 2 , R 3 , R 4 , R 5 and R 6Each is independently selected from a straight-chain alkyl group having 1 to 20 carbon atoms, a branched-chain alkyl group having 3 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, a halogenated hydrocarbon group having 1 to 20 carbon atoms, an aromatic hydrocarbon group having 6 to 20 carbon atoms, and an aromatic hydrocarbon group having a substituent.
[0021] Preferably, in the method for preparing the catalyst component of the present invention, the organophosphorus compound is selected from one or more of trimethyl phosphate, triethyl phosphate, tributyl phosphate, tripentyl phosphate, triphenyl phosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite and benzyl phosphite.
[0022] Preferably, in the method for preparing the catalyst component of the present invention, the general formula of the hydroxyl-containing compound is as shown in formula (III):
[0023] HOR a Formula (III)
[0024] Where R a It is a hydrocarbon group of 2 to 20 carbon atoms.
[0025] Preferably, in the method for preparing the catalyst component of the present invention, the hydrocarbon group is a saturated or unsaturated straight-chain or branched alkane group, cycloalkane group or aromatic hydrocarbon group.
[0026] Preferably, in the method for preparing the catalyst component of the present invention, the hydroxyl-containing compound is an alcohol compound.
[0027] Preferably, in the method for preparing the catalyst component of the present invention, the alcohol compound is selected from one or more of ethanol, propanol, butanol, 2-ethylhexanol, benzyl alcohol and phenylethyl alcohol.
[0028] Preferably, in the method for preparing the catalyst component of the present invention, the halogen-containing inert reagent is a halogenated hydrocarbon.
[0029] Preferably, in the method for preparing the catalyst component of the present invention, the halogen-containing inert reagent is selected from methyl bromide, dibromomethane, chloroform, ethyl bromide, dichloromethane, 1-chloroethane, 1,2-dichloroethane, 1,1-dichloroethane, 1,1,2-trichloroethane, 1,1,1-trichloroethane, 1,1-difluoro-1,2-dibromoethane, 1,1,2,2-tetrachloroethane, 1-chloropropane, bromopropane , 1,3-dibromopropane, 1,3-dichloropropane, 1,2,3-trichloropropane, 1-chlorobutane, 1-bromobutane, isobutyl bromide, 1-bromo-2-methylpropane, 1-bromo-4-chlorobutane, 2-chlorobutane, 1-chloro-3-methylbutane, 2-chloro-2-methylbutane, 1,3-dichlorobutane, 2,2-dichlorobutane, 2,3-dichlorobutane, 1,4-dichlorobutane, 1,1-dichlorobutane, 1, 2-Dichlorobutane, 1-bromopentane, 1-chloropentane, 1,5-dichloropentane, bromohexane, 1-chlorohexane, 1,6-dibromohexane, 1,6-dichlorohexane, 1-chloroheptane, 1,7-dichloroheptane, 1-bromoheptane, 1-chlorooctane, 1-bromooctane, 1,8-dichlorooctane, bromononane, 1-chlorononane, 1,9-dichlorononane, 1-chlorodecane, 1,10-dichlorodecane, bromodecane, 1-bromonoundecane , 1-chloroundecane, 1,11-dichloroundecane, 1-bromododecane, 1-chlorododecane, 1,12-dichlorododecane, 1-bromododecane, 1-chlorotridecane, chlorocyclopentane, chlorocyclohexane, 1-chloro-4-isopropylcyclohexane, 1,1-dichloroethylene, cis-1,2-dichloroethylene, trans-1,2-dichloroethylene, 1,1,2-trichloroethylene, monochlorobenzene, dichlorobenzene and bromobenzene.
[0030] Preferably, in the method for preparing the catalyst component of the present invention, the organic solvent is an aromatic hydrocarbon compound.
[0031] Preferably, in the method for preparing the catalyst component of the present invention, the organic solvent is selected from one or more of toluene, ethylbenzene, benzene and xylene.
[0032] Preferably, in the method for preparing the catalyst component of the present invention, the inert dispersion medium is selected from one or more of silicone oil, kerosene, paraffin oil, white oil, vaseline oil, methyl silicone oil, aliphatic and cycloaliphatic hydrocarbons.
[0033] Preferably, in the method for preparing the catalyst component of the present invention, the inert dispersion medium is selected from one or more of white oil, hexane, heptane, octane, nonane, decane, dodecane and cyclohexane.
[0034] Preferably, in the method for preparing the catalyst component of the present invention, the general formula of the titanium-containing compound is as shown in formula (IV):
[0035] TiXm (OR b ) 4-m Formula (IV)
[0036] Where X is a halogen, R b It is a hydrocarbon group of 1 to 20 carbon atoms, and m is an integer of 1 to 4.
[0037] Preferably, in the method for preparing the catalyst component of the present invention, the titanium-containing compound is selected from one or more of titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, tetrabutoxytitanium, tetraethoxytitanium, triethoxytitanium monochloride, diethoxytitanium dichloride and monoethoxytitanium trichloride.
[0038] Preferably, in the method for preparing the catalyst component of the present invention, the mixing in step (1) is carried out under the following conditions: the mixing temperature is 10°C-150°C, preferably 30°C-130°C; the mixing time is 0.05-10 hours, preferably 0.1-6 hours.
[0039] Preferably, in the method for preparing the catalyst component of the present invention, the mixing in step (3) is carried out under the following conditions: the mixing temperature is -30°C to 60°C, preferably -10°C to 40°C; the mixing time is 1 minute to 10 hours, preferably 3 minutes to 7 hours.
[0040] Preferably, in the method for preparing the catalyst component of the present invention, the heating in step (4) is carried out under the following conditions: the mixture is heated to 20°C-110°C, and the heating rate is 0.01°C / min to 4°C / min, preferably 0.05°C / min to 1°C / min.
[0041] Preferably, in the method for preparing the catalyst component of the present invention, the precipitation aid is selected from one or more of organic acids, organic acid anhydrides and organic ketones.
[0042] Preferably, in the method for preparing the catalyst component of the present invention, the precipitation aid is selected from one or more of acetic anhydride, phthalic anhydride, succinic anhydride, maleic anhydride, pyromellitic anhydride, acetic acid, propionic acid, butyric acid, acrylic acid, methacrylic acid, acetone, methyl ethyl ketone, benzophenone, methyl ether, ethyl ether, propyl ether, butyl ether and pentyl ether.
[0043] Preferably, in the method for preparing the catalyst component of the present invention, the surfactant is selected from one or more of alcoholysis products of maleic anhydride polymers, alcoholysis products of maleic anhydride copolymers, (meth)acrylic acid alkyl ester polymers and (meth)acrylic acid alkyl ester copolymers.
[0044] Preferably, in the preparation method of the catalyst component described in the present invention, the surfactant is selected from one or more of the group consisting of polymaleic anhydride alcoholysis products, maleic anhydride-styrene copolymer alcoholysis products, maleic anhydride-styrene-(meth)acrylate terpolymer alcoholysis products, maleic anhydride-(meth)acrylate alkyl ester alcoholysis products, poly(meth)acrylate alkyl esters, (meth)acrylate alkyl ester-maleic anhydride copolymers, and (meth)acrylate alkyl ester-maleic anhydride-styrene copolymers.
[0045] Preferably, in the method for preparing the catalyst component of the present invention, the internal electron donor compound is selected from one or more of esters, ethers, ketones, amines and silanes.
[0046] Preferably, in the method for preparing the catalyst component of the present invention, the internal electron donor compound is selected from one or more of monovalent or polyvalent aliphatic carboxylic acid esters, aromatic carboxylic acid esters, diol ester compounds and diether compounds.
[0047] Preferably, in the method for preparing the catalyst component of the present invention, the internal electron donor compound is selected from one or more of phthalates, malonates, succinates, glutarates, glycol esters, 1,3-diethers, pivalates and carbonates.
[0048] Preferably, in the preparation method of the catalyst component described in the present invention, the internal electron donor compound is selected from one or more of di-n-butyl phthalate, diisobutyl phthalate, 2,4-pentanediol dibenzoate, 3,5-heptanediol dibenzoate, diethyl 2,3-diisopropylsuccinate, diisobutyl 2,3-diisopropylsuccinate, di-n-butyl 2,3-diisopropylsuccinate, dimethyl 2,3-diisopropylsuccinate, diisobutyl 2,2-dimethylsuccinate, diisobutyl 2-ethyl-2-methylsuccinate, diethyl 2-ethyl-2-methylsuccinate, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and 9,9-dimethoxymethylfluorene.
[0049] Preferably, in the method for preparing the catalyst component of the present invention, the mixing in step (5) is carried out under the following conditions: the mixing temperature is 10°C-150°C, preferably 10°C-100°C; the mixing time is 0.05-8 hours, preferably 1-6 hours.
[0050] Preferably, in the preparation method of the catalyst component of the present invention, per mole of magnesium halide compound, the organic epoxy compound is 0.1-10 moles, preferably 0.4-4 moles; and / or the hydroxyl-containing compound is 0-10 moles, preferably 0-5 moles; and / or the organic phosphorus compound is 0.1-10 moles, preferably 0.8-4 moles; and / or the halogen-containing inert reagent is 0.01-40 moles, preferably 0.01-30 moles; and / or the organic solvent is 0-40 moles, preferably 0-30 moles; and / or the titanium-containing compound is 0.5-25 moles, preferably 1-20 moles; and / or the precipitation aid is 0.01-1 mole, preferably 0.04-0.4 moles; and / or the internal electron donor is 0.01-1 mole.
[0051] Preferably, the amount of the inert dispersion medium added is 0.1 g to 300 g, preferably 1 g to 150 g, per gram of the magnesium halide compound.
[0052] In a second aspect, the present invention provides a catalyst component, which is prepared by the method for preparing the catalyst component of the present invention.
[0053] In a third aspect, the present invention provides a catalyst system comprising the catalyst component of the present invention, an alkyl aluminum compound and optionally an external electron donor compound.
[0054] Preferably, in the catalyst system of the present invention, the general formula of the alkyl aluminum compound is AlR n X 3-n , wherein R is hydrogen, a hydrocarbon group having 1 to 20 carbon atoms, preferably an alkyl group, an aralkyl group, or an aryl group; X is a halogen, and n is an integer of 1 to 3.
[0055] Preferably, in the catalyst system described in the present invention, the alkyl aluminum compound is selected from one or more of trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, trioctylaluminum, diethyl aluminum monohydrogenate, diisobutyl aluminum monohydrogenate, diethyl aluminum monochloride, diisobutyl aluminum monochloride, sesquiethyl aluminum chloride and ethyl aluminum dichloride.
[0056] Preferably, in the catalyst system of the present invention, the molar ratio of the aluminum in the alkyl aluminum compound to the titanium in the catalyst component is 5-5000:1, preferably 20-800:1.
[0057] Preferably, in the catalyst system of the present invention, the general formula of the external electron donor compound is R' n Si(OR y ) 4-n , wherein n is an integer of 0-3, and R' is selected from one or more of an alkyl group, a cycloalkyl group, an aryl group, a halogenated alkyl group, a halogen group and a hydrogen atom; R yOne or more selected from alkyl, cycloalkyl, aryl and halogenated alkyl.
[0058] More preferably, the external electron donor compound is selected from one or more of trimethylmethoxysilane, trimethylethoxysilane, trimethylphenoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methyltert-butyldimethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, dicyclohexyldimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, methylcyclohexyldimethoxysilane, dicyclopentyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane.
[0059] Preferably, in the catalyst system of the present invention, the molar ratio of the aluminum in the alkyl aluminum compound to the external electron donor compound is 0.1-500:1, preferably 1-300:1, more preferably 3-100:1.
[0060] In a fourth aspect, the present invention further provides use of the catalyst component or catalyst system of the present invention in the field of olefin polymerization.
[0061] Specific embodiments of the present invention are further described below.
[0062] In a specific embodiment of the present invention, the magnesium halide compound may be at least one of magnesium dichloride, magnesium dibromide and magnesium diiodide, preferably magnesium dichloride.
[0063] In a specific embodiment of the present invention, the organic epoxy compound is selected from one or more of the oxidation products of C2-C8 aliphatic olefins and C2-C8 halogenated aliphatic olefins, preferably one or more of ethylene oxide, propylene oxide, ethylene oxide, epichlorohydrin, butylene oxide, butadiene oxide, butadiene dioxide, methyl glycidyl ether and diglycidyl ether, more preferably epichlorohydrin.
[0064] In a specific embodiment of the present invention, the organic solvent may be an aromatic hydrocarbon compound, specifically one or more of toluene, ethylbenzene, benzene, and xylene, among which toluene is preferred.
[0065] In a specific embodiment of the present invention, the inert dispersion medium is one or more of silicone oil, kerosene, paraffin oil, white oil, vaseline oil, methyl silicone oil, aliphatic and cycloaliphatic hydrocarbons, preferably one or more of white oil, hexane, heptane, octane, nonane, decane, dodecane and cyclohexane, preferably one or more of white oil, hexane and decane.
[0066] In a specific embodiment of the present invention, the mixing method for forming the magnesium-containing solution is not particularly limited, and the purpose of mixing is to form a uniform solution containing magnesium.
[0067] In a specific embodiment of the present invention, the titanium-containing compound is titanium tetrachloride.
[0068] In a specific embodiment of the present invention, the mixing method for forming the titanium-containing solution is not particularly limited, and the purpose of mixing is to form a uniform titanium-containing solution.
[0069] In a specific embodiment of the present invention, the magnesium-containing solution and the titanium-containing solution are mixed to form a mixture, preferably by dropping the titanium-containing solution into the magnesium-containing solution to form a mixture.
[0070] In specific embodiments of the present invention, the mixture comprises a colloid, a two-phase solution, an emulsion and other forms.
[0071] In a specific embodiment of the present invention, the preparation method of the present invention further comprises: using one or more methods such as vibration, stirring, atomization, shearing, etc. to promote uniform dispersion of the mixture, further heating the mixture to 20°C-110°C, solidifying and precipitating solid matter, and then stirring the suspension at this temperature or at a higher temperature for 10 minutes to 24 hours.
[0072] In a specific embodiment of the present invention, the mixture heating process is not specifically limited, and any known method can be used to heat up, such as slowly, step by step, quickly or program heating. The specific heating method should be adjusted according to the specific formula, mixing temperature, etc. In addition, the inventors have found that in the preparation method of the present invention, when other conditions are the same, different heating processes will affect the particle morphology and particle size distribution of the final catalyst. Specifically, a slower heating process can be used to obtain a better particle morphology, otherwise, the heating rate is too fast, which will cause the particle shape to deteriorate. Therefore, the mixture heating process can be 1 minute to 36 hours, preferably 3 minutes to 24 hours.
[0073] In a specific embodiment of the present invention, after the solid matter is precipitated from the mixture, the suspension is stirred at a certain temperature for 10 minutes to 24 hours in order to make the crystal form more stable and improve the particle strength.
[0074] In a specific embodiment of the present invention, the precipitation aid of the present invention is phthalic anhydride.
[0075] In a specific embodiment of the present invention, the surfactant is selected from one or more of the alcoholysis products of maleic anhydride polymers and alcoholysis products of maleic anhydride copolymers, preferably one or more of the alcoholysis products of polymaleic anhydride, alcoholysis products of maleic anhydride-styrene copolymers, alcoholysis products of maleic anhydride-styrene-(meth)acrylic acid alkyl ester terpolymers, and alcoholysis products of maleic anhydride-(meth)acrylic acid alkyl ester copolymers, wherein the alkyl ester side chain is a straight-chain alkane of 1 to 30 carbon atoms. The alcoholysis product refers to a polymer product obtained by reacting the alcoholysis product with an organic alcohol compound, wherein the organic alcohol compound has a structure of ROH, wherein R is a straight-chain alkane group of 2 to 20 carbon atoms, a branched-chain alkane group of 3 to 20 carbon atoms, a cycloalkane group of 3 to 20 carbon atoms, or an aromatic hydrocarbon group of 6 to 30 carbon atoms, preferably those with 1 to 20 carbon atoms; the alcoholysis product refers to a polymer product obtained by reacting the alcoholysis product with an organic alcohol compound, wherein the organic alcohol compound has a structure of ROH, wherein R is a straight-chain alkane group of 2 to 20 carbon atoms, a branched-chain alkane group of 3 to 20 carbon atoms, a cycloalkane group of 3 to 20 carbon atoms, or an aromatic hydrocarbon group of 6 to 20 carbon atoms.
[0076] In a specific embodiment of the present invention, the surfactant described in the present invention also comprises at least one of a (meth)acrylic acid alkyl ester polymer and a (meth)acrylic acid alkyl ester copolymer, for example, it may be at least one of a poly (meth)acrylic acid alkyl ester, a (meth)acrylic acid alkyl ester-maleic anhydride copolymer, and a (meth)acrylic acid alkyl ester-maleic anhydride-styrene copolymer; wherein the ester side chain is a straight-chain alkane group of 1 to 30 carbon atoms, a branched-chain alkane group of 3 to 30 carbon atoms, a cycloalkane group of 3 to 30 carbon atoms, or an aromatic hydrocarbon group of 6 to 30 carbon atoms, preferably those of 1 to 20 carbon atoms.
[0077] In a specific embodiment of the present invention, the surfactant of the present invention may be 0.05 g to 1 g per gram of the magnesium halide compound.
[0078] In a specific embodiment of the present invention, the poly (meth) acrylate polymer surfactant of the present invention can be a surfactant product purchased from an additive company with the trade name T602.
[0079] In a specific embodiment of the present invention, the surfactant can be added at any position in the preparation method, and can be added as a whole or in a dispersed manner. According to the present invention, the surfactant can be added as a whole or in part during or after the formation of a uniform solution containing magnesium.
[0080] In a specific embodiment of the present invention, after the surfactant is added, the temperature of the system can be controlled to be 10°C-100°C, preferably 10°C-80°C, and more preferably 10°C-60°C.
[0081] In a specific embodiment of the present invention, the internal electron donor compound can be selected from one or more of esters, ethers, ketones, amines, and silanes; preferably one or more of monovalent or polyvalent aliphatic carboxylic acid esters, aromatic carboxylic acid esters, glycol ester compounds, and diether compounds; more preferably one or more of divalent aliphatic carboxylic acid esters, aromatic carboxylic acid esters, glycol esters, and diether compounds; further preferably one or more of phthalates, malonic acid esters, succinates, glutarates, glycol esters, 1,3-diethers, pivalates, or carbonates.
[0082] In a particular embodiment of the present invention, the catalyst component has a spherical or spheroidal structure.
[0083] In a specific embodiment of the present invention, the catalyst component has a 2 / g specific surface area.
[0084] In a specific embodiment of the present invention, the alkylaluminum compound is triethylaluminum and / or triisobutylaluminum.
[0085] In a specific embodiment of the present invention, the external electron donor compound is cyclohexylmethyldimethoxysilane.
[0086] In a particular embodiment of the invention, the olefin comprises propylene.
[0087] In a specific embodiment of the present invention, the olefin polymerization catalyst system of the present invention can be used for homopolymerization of olefins, and can also be used for copolymerization of multiple olefins. At least one of the olefins is a olefin having the formula CH 2 =CHR represented by olefins, wherein R is hydrogen or C 1 -C 6 A straight chain or branched alkyl group of the formula CH 2 Specific examples of the olefin represented by =CHR may include: ethylene, propylene, 1-n-butene, 1-n-pentene, 1-n-hexene, 1-n-octene and 4-methyl-1-pentene. 2 =CHR represents one or more of ethylene, propylene, 1-n-butene, 1-n-hexene and 4-methyl-1-pentene. More preferably, the olefin represented by the formula CH 2 The olefin represented by =CHR is propylene, or a copolymer of propylene and other olefins.
[0088] In a specific embodiment of the present invention, the polymerization of olefins is carried out according to known methods, in the liquid phase of a liquid monomer or a solution of a monomer in an inert solvent, or in the gas phase, or by a combined polymerization process in the gas and liquid phase. The polymerization temperature is generally 0° C. to 150° C., preferably 60° C. to 100° C. The polymerization pressure is normal pressure or higher.
[0089] The present invention has the following beneficial effects:
[0090] Compared with the prior art, the method of the present invention can precipitate catalyst spherical solids with intact particle shape, uniform particle size distribution, no rod-shaped materials, large blocks and sticky materials, and the catalyst has excellent performance, high activity and stereo-orientation ability, and the polymer has no blocky materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0091] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention, but do not constitute a limitation of the present invention. In the accompanying drawings:
[0092] Figure 1 This is a microscope image of the solid object prepared in Example 1.
[0093] Figure 2 This is a microscope image of the solid object prepared in Comparative Example 1.
[0094] Figure 3 This is a microscope image of the solid object prepared in Comparative Example 2.
[0095] Figure 4 This is a microscope image of the solid object prepared in Comparative Example 3. DETAILED DESCRIPTION
[0096] The present invention will be further described below in conjunction with specific embodiments, but they do not constitute any limitation to the present invention.
[0097] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or the conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be obtained through commercial channels.
[0098] 1. Determination of titanium content in catalyst: Use UV-Vis spectrophotometer 722 for colorimetric determination.
[0099] 2. Magnesium content is measured by magnesium ion and EDTA complexometric titration.
[0100] 3. Catalyst particle size distribution: measured by Malvern 2000 n-hexane dispersant laser diffraction method.
[0101] 4. Determination of the content of internal electron donor compounds in the catalyst: The chromatographic method is used. The catalyst dry powder is decomposed with dilute acid, and the internal electron donor compounds are extracted with an extractant. The internal electron donor compounds are determined using an Agilent 6890N gas chromatograph.
[0102] 5. The bulk density (BD) of polymers is determined according to ASTM D1895-96.
[0103] 6. The isotacticity index (II) of propylene polymer is determined by the heptane extraction method: 2 g of dried polymer sample is placed in an extractor and extracted with boiling heptane for 6 hours. The residue is dried to constant weight. The ratio of the obtained polymer weight (g) to 2 (g) is the isotacticity.
[0104] 7. The melt flow index (MI) of the polymer is measured using the MI-4 melt flow index tester from GOTTFERT, Germany, in accordance with GB / T 3682.1-2018 standard.
[0105] 8. The specific surface area of the magnesium-containing carrier or catalyst is determined by nitrogen adsorption method using ASAP2460 specific surface area and porosity analyzer produced by Micromeritics, USA.
[0106] Example 1
[0107] In a reactor that has been repeatedly replaced with high-purity nitrogen, 10.86g of anhydrous magnesium chloride, 65g of toluene, 10.8g of epichlorohydrin, and 40.2g of tributyl phosphate are added in sequence, and maintained at a stirring rate of 300RMP for 2 hours at a temperature of 60°C. Then 3.3g of phthalic anhydride, 5.7g of T602 and 6.3mL of 1-bromooctane are added, and maintained at 60°C for another hour. Then the temperature is lowered to 0°C to form a magnesium-containing solution. 155.4g of titanium tetrachloride and 180.2g of hexane are mixed evenly to form a titanium-containing solution. Increase the stirring rate to 400RMP, drip the titanium-containing solution into the magnesium-containing solution, and continue to maintain it for 1 hour after the addition is completed. Gradually heat up to 80°C within 4 hours and maintain it for 1 hour. Filter the mother liquor, wash the solid with hot toluene twice, then wash it with hexane twice, and dry it to obtain a solid. The average particle size D50 of the solid material is 67.7 μm, and the SPAN value is 0.73. Figure 1 As shown, the solids are spherical and evenly distributed.
[0108] Example 2
[0109] In a reactor that has been repeatedly replaced with high-purity nitrogen, 10.86g of anhydrous magnesium chloride, 42.8g of toluene, 9.2mL of 1-bromobutane, 10.8g of epichlorohydrin, and 40.2g of tributyl phosphate are added in sequence, and maintained at a stirring rate of 300RMP for 2 hours at a temperature of 60°C. Then 3.3g of phthalic anhydride is added and maintained at 60°C for another hour. Then the temperature is lowered to 10°C, 5.7g of T602 is added, and it is maintained for another hour to form a magnesium-containing solution. 155.4g of titanium tetrachloride and 131.1g of hexane are mixed evenly to form a titanium-containing solution. The stirring rate is increased to 400RMP, and the titanium-containing solution is dripped into the magnesium-containing solution. After the dripping is completed, it is maintained for another hour. The temperature is gradually raised to 80°C within 4 hours and maintained for 1 hour. The mother liquor is filtered, and the solid is washed twice with hot toluene, and then washed twice with hexane, and then dried to obtain a solid. The average particle size D50 of the solid obtained in this example is 26.4 μm, and the SPAN value is 0.85.
[0110] Example 3
[0111] In a reactor that has been repeatedly replaced with high-purity nitrogen, 10.86g of anhydrous magnesium chloride, 85.6g of toluene, 10.8g of epichlorohydrin, and 40.2g of tributyl phosphate are added in sequence, and maintained at a temperature of 60°C and a stirring rate of 300RMP for 2 hours. Then 2.5g of phthalic anhydride and 6ml of butyl ether are added, and maintained at 60°C for another hour. Then the temperature is lowered to 20°C, 11.2mL of 1,6-dibromohexane and 5.7g of T602 are added, and the temperature is maintained for another hour to form a magnesium-containing solution. 155.4g of titanium tetrachloride and 115.7g of hexane are mixed evenly to form a titanium-containing solution. Increase the stirring rate to 600RMP, drip the titanium-containing solution into the magnesium-containing solution, and continue to maintain it for 1 hour after the addition is completed. Gradually heat up to 80°C within 3 hours and maintain it for 1 hour. Filter the mother liquor, wash the solid with hot toluene twice, then wash it with hexane twice, and dry it to obtain a solid. The average particle size D50 of the solid obtained in this example is 15.7 μm, and the SPAN value is 0.91.
[0112] Example 4
[0113] The solid material was prepared by the same method as in Example 1, except that the amount of 1-bromooctane was changed to 4.5 mL of 1-chlorobutane. The average particle size D50 of the solid material prepared in this example was 56.5 μm.
[0114] Example 5
[0115] The solid material was prepared by the same method as in Example 1, except that the amount of 1-bromooctane was changed to 14.5 mL of 1,4-dichlorobutane. The average particle size D50 of the solid material prepared in this example was 45.2 μm.
[0116] Example 6
[0117] The solid was prepared by the same method as in Example 1, except that when preparing the magnesium-containing solution, the amount of epichlorohydrin was changed to 8.7 g, the amount of tributyl phosphate was changed to 43.2 g, and 3.2 g of ethanol was used. The average particle size D50 of the solid obtained in this example was 65.2 μm.
[0118] Comparative Example 1
[0119] The solid was prepared by the same method as in Example 1, except that 1-bromooctane was not used. An optical microscope photograph of the precipitated particles is shown in Figure 2 The solid obtained in this comparative example is spherical and contains agglomerates and sticky materials.
[0120] Comparative Example 2
[0121] The solid material was prepared by the same method as in Example 1, except that a preparation method similar to that of CN201280032149.7 and CN201580067255.2 was used, that is, instead of mixing titanium tetrachloride and hexane to form a titanium-containing solution, hexane was added to a magnesium-containing solution to form a new magnesium-containing solution. Titanium tetrachloride was then dripped into the new magnesium-containing solution. An optical microscope photograph of the precipitated particles was taken at Figure 3 The solid obtained in this comparative example is spherical and contains a certain amount of sticky material.
[0122] Comparative Example 3
[0123] The solid was prepared in the same manner as in Comparative Example 2, except that 1-bromooctane was not used. An optical microscope photograph of the precipitated particles is shown in Figure 4 The solid part is spherical and contains a lot of agglomerates and sticky materials.
[0124] Example 7
[0125] Preparation of catalyst components: Prepare solids using the method of Example 1, and continue to mix with an internal electron donor to prepare catalyst components. Add 160 ml of toluene, 40 ml of titanium tetrachloride, and 3 ml of 2-isopropyl-2-isopentyl-1,3-dimethoxypropane, heat to 80°C and maintain for 1 hour, filter the clear liquid, and remove the filtrate. Add 120 ml of toluene, 80 ml of titanium tetrachloride, treat at 110°C for 1 hour, and remove the filtrate. Repeat the treatment once. After washing with 200 ml of hexane for 5 times, a solid olefin polymerization catalyst component is obtained. Catalyst component data is shown in Table 1. The specific surface area tested by the BET method is 254.7 m 2 / g.
[0126] Propylene polymerization: In a 5-liter autoclave, after nitrogen is fully replaced, 5 ml of triethylaluminum hexane solution (the concentration of triethylaluminum is 0.5 mmol / ml), 1 ml of cyclohexylmethyldimethoxysilane (CHMMS) hexane solution (the concentration of CHMMS is 0.1 mmol / ml), 10 ml of anhydrous hexane and 10 mg of the catalyst component of Test Example 1 are added at room temperature. 1 liter of hydrogen under standard conditions and 1.15 kg of liquid propylene are introduced. The temperature is raised to 70°C, and the polymerization reaction is carried out at 70°C for 1 hour. After the reaction is completed, the reactor is cooled and stirring is stopped to discharge the reaction product to obtain an olefin polymer. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0127] Comparative Example 4
[0128] Preparation of catalyst components: The solid material was prepared by the method of Comparative Example 1, and the catalyst component was prepared by the method of Example 7.
[0129] The propylene polymerization method was the same as in Example 7. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0130] Comparative Example 5
[0131] Preparation of catalyst components: The solid material was prepared by the method of Comparative Example 2, and the catalyst component was prepared by the method of Example 7.
[0132] The propylene polymerization method was the same as in Example 7. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0133] Comparative Example 6
[0134] Preparation of catalyst components: The solid material was prepared by the method of Comparative Example 3, and the catalyst component was prepared by the method of Example 7.
[0135] The propylene polymerization method was the same as in Example 7. The polymerization results of the catalyst and the polymer data are shown in Table 1.
[0136] Table 1 Catalyst components and propylene polymerization performance
[0137]
[0138] In Table 1, BD represents polymer bulk density; II represents polymer isotacticity; MI represents polymer melt index; PP represents polypropylene; and Cat represents catalyst.
[0139] According to the above examples and comparative examples, in the preparation method of the present invention, a halogen-containing inert reagent is added, and the magnesium-containing solution is not mixed with an inert dispersion medium before mixing with the titanium compound, thereby reducing the phenomenon of solid catalyst agglomeration. The precipitated catalyst spherical solid particles are more uniform, do not contain rod-shaped materials, large blocks and adhesion materials, and the catalyst has excellent performance, high activity and stereo-orientation ability, and high polymer bulk density.
[0140] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
Claims
1. A method for preparing a catalyst component, comprising the following steps: (1) mixing a magnesium halide compound, an organic epoxy compound, an organic phosphorus compound and optionally a hydroxyl-containing compound with a halogen-containing inert reagent and an organic solvent to form a magnesium-containing solution; (2) mixing an inert dispersion medium with a titanium-containing compound to form a titanium-containing solution; (3) mixing the magnesium-containing solution with the titanium-containing solution to form a mixture; (4) in the presence of a precipitation aid and a surfactant, heating the mixture to precipitate a spherical solid; (5) mixing the spherical solid object with an internal electron donor compound to obtain the catalyst component; Wherein, the halogen-containing inert reagent is a halogenated hydrocarbon; and the organic solvent is an aromatic hydrocarbon compound.
2. The method for preparing the catalyst component according to claim 1, wherein: The general formula of the magnesium halide compound is MgX2, wherein X is bromine, chlorine or iodine; And / or, the organic epoxy compound is one or more selected from the oxidation products of C2-C8 aliphatic olefins or C2-C8 halogenated aliphatic olefins; And / or, the organophosphorus compound is selected from one or more of the compounds represented by formula (I) and formula (II): Wherein, R1, R2, R3, R4, R5 and R6 are each independently selected from a straight-chain alkyl group of 1 to 20 carbon atoms, a branched-chain alkyl group of 3 to 20 carbon atoms, a cycloalkyl group of 3 to 20 carbon atoms, a halogenated hydrocarbon group of 1 to 20 carbon atoms, or an aromatic hydrocarbon group of 6 to 20 carbon atoms and an aromatic hydrocarbon group with a substituent; And / or, the general formula of the hydroxyl-containing compound is as shown in formula (III): HORa formula (III) Wherein Ra is a hydrocarbon group of 2 to 20 carbon atoms, and the hydrocarbon group is a saturated or unsaturated straight chain or branched alkyl group, cycloalkyl group or aromatic hydrocarbon group; and / or, the halogen-containing inert reagent is selected from methyl bromide, dibromomethane, chloroform, ethyl bromide, dichloromethane, 1-chloroethane, 1,2-dichloroethane, 1,1-dichloroethane, 1,1,2-trichloroethane, 1,1,1-trichloroethane, 1,1-difluoro-1,2-dibromoethane, 1,1,2,2-tetrachloroethane, 1-chloropropane, bromopropane, 1,3-dibromopropane, 1,3- Dichloropropane, 1,2,3-trichloropropane, 1-chlorobutane, 1-bromobutane, isobutyl bromide, 1-bromo-2-methylpropane, 1-bromo-4-chlorobutane, 2-chlorobutane, 1-chloro-3-methylbutane, 2-chloro-2-methylbutane, 1,3-dichlorobutane, 2,2-dichlorobutane, 2,3-dichlorobutane, 1,4-dichlorobutane, 1,1-dichlorobutane, 1,2-dichlorobutane, 1- Bromopentane, 1-chloropentane, 1,5-dichloropentane, bromohexane, 1-chlorohexane, 1,6-dibromohexane, 1,6-dichlorohexane, 1-chloroheptane, 1,7-dichloroheptane, 1-bromoheptane, 1-chlorooctane, 1-bromooctane, 1,8-dichlorooctane, bromononane, 1-chlorononane, 1,9-dichlorononane, 1-chlorodecane, 1,10-dichlorodecane, bromodecane, 1-bromodencane, 1-bromonoundecane, 1-chlorodecane One or more of 1,1-dichloroundecane, 1-bromododecane, 1-chlorododecane, 1,12-dichlorododecane, 1-bromododecane, 1-chlorotridecane, chlorocyclopentane, chlorocyclohexane, 1-chloro-4-isopropylcyclohexane, 1,1-dichloroethylene, cis-1,2-dichloroethylene, trans-1,2-dichloroethylene, 1,1,2-trichloroethylene, monochlorobenzene, dichlorobenzene and bromobenzene; And / or, the organic solvent is selected from one or more of toluene, ethylbenzene, benzene and xylene; and / or, the inert dispersion medium is selected from one or more of silicone oil, kerosene, paraffin oil, white oil, vaseline oil, methyl silicone oil, aliphatic and cycloaliphatic hydrocarbons; And / or, the general formula of the titanium-containing compound is as shown in formula (IV): TiX m (OR b ) 4-m Formula (IV) Where X is a halogen, R b It is a hydrocarbon group of 1 to 20 carbon atoms, and m is an integer of 1 to 4.
3. The method for preparing the catalyst component according to claim 2, wherein: The organic epoxy compound is selected from one or more of ethylene oxide, propylene oxide, epichlorohydrin, epichlorohydrin, butylene oxide, butadiene oxide, butadiene dioxide, methyl glycidyl ether and diglycidyl ether; And / or, the organophosphorus compound is one or more selected from trimethyl phosphate, triethyl phosphate, tributyl phosphate, tripentyl phosphate, triphenyl phosphate, trimethyl phosphite, triethyl phosphite, tributyl phosphite and benzyl phosphite; And / or, the hydroxyl-containing compound is an alcohol compound, and the alcohol compound is selected from one or more of ethanol, propanol, butanol, 2-ethylhexanol, benzyl alcohol and phenylethyl alcohol; and / or, the inert dispersion medium is selected from one or more of white oil, hexane, heptane, octane, nonane, decane, dodecane and cyclohexane; And / or, the titanium-containing compound is one or more selected from titanium tetrachloride, titanium tetrabromide, titanium tetraiodide, titanium tetrabutoxide, titanium tetraethoxide, titanium triethoxide monochloride, titanium diethoxide dichloride and titanium triethoxide monochloride.
4. The method for preparing a catalyst component according to any one of claims 1 to 3, wherein: The mixing in step (1) is carried out under the following conditions: the mixing temperature is 10°C-150°C; the mixing time is 0.05-10 hours; And / or, the mixing in step (3) is carried out under the following conditions: the mixing temperature is -30°C to 60°C; the mixing time is 1 minute to 10 hours; And / or, the heating in step (4) is carried out under the following conditions: the mixture is heated to 20°C-110°C at a heating rate of 0.01°C / min to 4°C / min.
5. The method for preparing the catalyst component according to any one of claims 1 to 3, wherein: The precipitation aid is selected from one or more of organic acids, organic anhydrides and organic ketones; and / or The surfactant is selected from one or more of alcoholysis products of maleic anhydride polymers, alcoholysis products of maleic anhydride copolymers, (meth) alkyl acrylate polymers and (meth) alkyl acrylate copolymers; and / or, the internal electron donor compound is selected from one or more of esters, ethers, ketones, amines and silanes; And / or, the mixing in step (5) is carried out under the following conditions: the mixing temperature is 10° C.-150° C.; and the mixing time is 0.05-8 hours.
6. The method for preparing the catalyst component according to claim 5, wherein: The precipitation aid is selected from one or more of acetic anhydride, phthalic anhydride, succinic anhydride, maleic anhydride, pyromellitic anhydride, acetic acid, propionic acid, butyric acid, acrylic acid, methacrylic acid, acetone, methyl ethyl ketone, benzophenone, methyl ether, ethyl ether, propyl ether, butyl ether and pentyl ether; And / or, the surfactant is selected from one or more of alcoholysis products of polymaleic anhydride, alcoholysis products of maleic anhydride-styrene copolymer, alcoholysis products of maleic anhydride-styrene-(meth)acrylate terpolymer, alcoholysis products of maleic anhydride-(meth)acrylate alkyl ester copolymer, poly(meth)acrylate alkyl ester, (meth)acrylate alkyl ester-maleic anhydride copolymer, and (meth)acrylate alkyl ester-maleic anhydride-styrene copolymer; And / or, the internal electron donor compound is selected from one or more of monovalent or polyvalent aliphatic carboxylic acid esters, aromatic carboxylic acid esters, diol ester compounds and diether compounds.
7. The method for preparing the catalyst component according to claim 6, wherein: The internal electron donor compound is selected from one or more of phthalates, malonates, succinates, glutarates, glycol esters, 1,3-diethers, pivalates and carbonates.
8. The method for preparing the catalyst component according to claim 7, wherein: The internal electron donor compound is selected from one or more of di-n-butyl phthalate, diisobutyl phthalate, 2,4-pentanediol dibenzoate, 3,5-heptanediol dibenzoate, diethyl 2,3-diisopropylsuccinate, diisobutyl 2,3-diisopropylsuccinate, di-n-butyl 2,3-diisopropylsuccinate, dimethyl 2,3-diisopropylsuccinate, diisobutyl 2,2-dimethylsuccinate, diisobutyl 2-ethyl-2-methylsuccinate, diethyl 2-ethyl-2-methylsuccinate, 2-isopropyl-2-isopentyl-1,3-dimethoxypropane and 9,9-dimethoxymethylfluorene.
9. The method for preparing a catalyst component according to any one of claims 1 to 3, wherein: Based on each mole of magnesium halide compound, the organic epoxy compound is 0.1-10 moles; and / or the hydroxyl-containing compound is 0-10 moles; and / or the organic phosphorus compound is 0.1-10 moles; and / or the halogen-containing inert reagent is 0.01-40 moles; and / or the organic solvent is 0-40 moles; and / or the titanium-containing compound is 0.5-25 moles; and / or the precipitation aid is 0.01-1 mole; and / or the internal electron donor is 0.01-1 mole; and / or The added amount of the inert dispersion medium is 0.1 g-300 g per gram of the magnesium halide compound.
10. The method for preparing a catalyst component according to claim 9, wherein: Based on each mole of magnesium halide compound, the organic epoxy compound is 0.4-4 moles; and / or the hydroxyl-containing compound is 0-5 moles; and / or the organic phosphorus compound is 0.8-4 moles; and / or the halogen-containing inert reagent is 0.01-30 moles; and / or the organic solvent is 0-30 moles; and / or the titanium-containing compound is 1-20 moles; and / or the precipitation aid is 0.04-0.4 moles; and / or The amount of the inert dispersion medium added is 1 g to 150 g per gram of the magnesium halide compound.
11. A catalyst component obtained by the method for preparing a catalyst component according to any one of claims 1 to 10.
12. A catalyst system comprising the catalyst component according to claim 11, an alkyl aluminum compound and optionally an external electron donor compound.
13. The catalyst system according to claim 12, wherein The general formula of the alkyl aluminum compound is AlR n X 3-n , wherein R is hydrogen, a hydrocarbon group having 1 to 20 carbon atoms, wherein the hydrocarbon group is an alkyl group, an aralkyl group, or an aryl group; X is a halogen, and n is an integer of 1 to 3; And / or, the molar ratio of aluminum in the alkyl aluminum compound to titanium in the catalyst component is 5-5000:
1.
14. The catalyst system according to claim 13, wherein The alkyl aluminum compound is one or more selected from trimethyl aluminum, triethyl aluminum, triisobutyl aluminum, trioctylaluminum, diethyl aluminum monohydrogenate, diisobutyl aluminum monohydrogenate, diethyl aluminum monochloride, diisobutyl aluminum monochloride, sesquiethyl aluminum chloride and ethyl aluminum dichloride; And / or, the molar ratio of aluminum in the alkyl aluminum compound to titanium in the catalyst component is 20-800:
1.
15. The catalyst system according to any one of claims 12 to 14, wherein The general formula of the external electron donor compound is R' n Si(OR y ) 4-n , wherein n is an integer of 0-3, and R' is selected from one or more of an alkyl group, a cycloalkyl group, an aryl group, a halogenated alkyl group, a halogen group and a hydrogen atom; R y One or more selected from alkyl, cycloalkyl, aryl and halogenated alkyl; And / or, the molar ratio of aluminum in the alkyl aluminum compound to the external electron donor compound is 0.1-500:
1.
16. The catalyst system according to claim 15, wherein The external electron donor compound is selected from one or more of trimethylmethoxysilane, trimethylethoxysilane, trimethylphenoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, methyltert-butyldimethoxysilane, diphenyldimethoxysilane, diphenyldiethoxysilane, dicyclohexyldimethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, vinyltrimethoxysilane, methylcyclohexyldimethoxysilane, dicyclopentyldimethoxysilane, 2-ethylpiperidinyl-2-tert-butyldimethoxysilane, (1,1,1-trifluoro-2-propyl)-2-ethylpiperidinyldimethoxysilane and (1,1,1-trifluoro-2-propyl)-methyldimethoxysilane; And / or, the molar ratio of aluminum in the alkyl aluminum compound to the external electron donor compound is 3-100:
1.
17. Use of the catalyst component according to claim 11 or the catalyst system according to any one of claims 12 to 16 in the field of olefin polymerization.