Polyethylene composition and preparation method thereof

Through the combination of high-density polyethylene resin with antioxidants, acid absorbers and synergists, combined with pretreatment and twin-screw extrusion processing, the problem of poor sensory properties and physical properties of polyethylene bottle cap materials has been solved, and the polyethylene bottle cap material has been realized. The excellent performance and stability of the ethylene composition are suitable for bottled water and non-carbonated beverage bottle caps.

CN116041816BActive Publication Date: 2024-10-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111265766.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-28
Publication Date
2024-10-01
Estimated Expiration
2041-10-28

AI Technical Summary

Technical Problem

Existing polyethylene bottle cap materials have problems with poor sensory properties, unstable performance and unqualified performance indicators of domestic raw materials. As a result, domestic polyethylene bottle caps occupy a smaller share in the market, and the preparation process is complex, which affects product quality.

Method used

Using a combination of high-density polyethylene resin and antioxidants, acid absorbers and synergists, through pre-treatment and mixing of specific additives and twin-screw extrusion processing, a polyethylene combination with excellent sensory properties and physical properties is prepared things.

Benefits of technology

The polyethylene composition has good appearance color, no odor and no abnormal taste, and improved physical properties and processing properties. It is suitable for bottle caps of bottled drinking water and non-carbonated beverages to meet market demand.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003326929280000021
    Figure BDA0003326929280000021
  • Figure BDA0003326929280000111
    Figure BDA0003326929280000111
  • Figure BDA0003326929280000121
    Figure BDA0003326929280000121
Patent Text Reader

Abstract

The polyethylene composition prepared by adding 0.01-0.3 parts of antioxidant (based on 100 parts of high-density polyethylene by mass, the same below), 0.03-0.2 parts of acid absorber and 0.02-0.2 parts of synergist to high-density polyethylene, the proportion of low molecular weight components with molecular weight below 2000 of the high-density polyethylene raw material is less than 2%, the proportion of low molecular weight components with molecular weight below 1700 is less than 1.8%, and the proportion of low molecular weight components with molecular weight below 1000 is less than 0.7%. The composition has low volatile matter content, no odor and abnormal taste, good sensory performance and appearance color, excellent physical properties and processing properties, and can be applied to drinking water bottle caps, non-carbonated beverage bottle caps and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of plastic packaging materials, and more particularly to a polyethylene composition for plastic bottle caps and a preparation method thereof. Background Art

[0002] As the main raw material for plastic bottle caps, polyethylene has been widely used in various types of bottled water, herbal tea, juice and some carbonated beverages. As part of food contact materials, the sensory and hygienic properties of polyethylene bottle cap materials meet national standards, requiring no odor, and the sensory properties meet the requirements of downstream manufacturers. At the same time, the mechanical and physical properties must meet the requirements of the bottle cap's sealing, drop, impact resistance and other indicators. At present, the domestic market demand for high-density polyethylene (HDPE) bottle cap materials is about 500,000 tons per year. Downstream large and well-known manufacturers of bottled water, functional beverages and carbonated beverages still mainly use imported materials, and there is a large market gap. At present, imported polyethylene materials still occupy a large share of the domestic bottle cap market, and domestic raw materials still have problems such as unstable performance indicators and unqualified sensory performance.

[0003] In the prior art, in addition to the sensory problems caused by the base resin in the raw materials due to the influence of the catalyst and the polymerization process, the large number of components in the auxiliary agent system and the complicated and unreasonable preparation process are also important reasons for the poor sensory performance. When the low molecular content of the base resin is high, it is easy to produce odor, and it is easy to be oxidized or further thermally degraded during the high-temperature melting process, resulting in the production of substances that are not conducive to sensory performance. At the same time, the type and amount of additives are not appropriate, which can easily cause sensory problems such as taste and odor. In the prior art, for example, CN201210302019, CN201010500727, CN201210454986.0, CN2015101007695, and CN201710557738, etc., all have problems such as complex components and poor product performance.

[0004] In order to solve the above problems, the purpose of the present invention is to provide a polyethylene composition with excellent sensory properties and good physical properties, and also provide a method for preparing the composition. The composition has excellent physical properties, good sensory properties and appearance color, no odor and abnormal taste, and can be applied to drinking water bottle caps, non-carbonated beverage bottle caps and other fields. Summary of the invention

[0005] The polyethylene composition of the present invention is composed of polyethylene resin, antioxidant, acid absorber and synergist, etc. The polyethylene resin is first pretreated, and then the components are weighed according to a certain mass ratio and mixed evenly according to the order of adding different additives, and then melt-extruded and granulated by a twin-screw extruder to prepare the polyethylene composition.

[0006] The composition of the present invention is composed of the following raw materials in parts by weight:

[0007]

[0008] The polyethylene is a high-density polyethylene, which is a copolymer of ethylene and α-olefin, wherein the α-olefin comonomer is 1-butene or 1-hexene, and the molar percentage of the comonomer is 0.1-0.5%. The density is 0.948-0.956 g / cm 3 The melt mass flow rate (MFR) (test temperature 190°C, load 2.16kg) is 3.0-8.0g / 10min, and the melting point measured by differential scanning calorimeter (DSC) is 128-131°C.

[0009] The high-density polyethylene in the present invention is produced by using a metallocene catalyst, and its number average molecular weight measured by the GPC method is 1.3×10 4 ~1.8×10 4 , the weight average molecular weight is 5×10 4 ~10×10 4 , the Z average molecular weight is 15×10 4 ~30×10 4 , wherein the proportion of low molecular weight components with a molecular weight below 2000 of the high-density polyethylene is less than 2%, the proportion of low molecular weight components with a molecular weight below 1700 is less than 1.8%, and the proportion of low molecular weight components with a molecular weight below 1000 is less than 0.7%; preferably, the proportion of low molecular weight components with a molecular weight below 2000 of the high-density polyethylene is less than 1.8%, the proportion of low molecular weight components with a molecular weight below 1700 is less than 1.4%, and the proportion of low molecular weight components with a molecular weight below 1000 is less than 0.5%. In the present invention, the high-density polyethylene is produced using a high-activity metallocene catalyst, and the obtained polyethylene has high stereoregularity, moderate molecular weight distribution, and low content of low molecular weight components, which can effectively reduce thermal degradation in the subsequent extrusion process and avoid the generation of odor. The high-density polyethylene resin is preferably the high-density polyethylene resin Q504 produced by Sinopec Qilu Branch.

[0010] Antioxidants, acid absorbers and synergists are added to the polyethylene composition obtained by the present invention to ensure the thermal oxygen stability, good appearance color and necessary durability of the polyethylene composition. The selected additives should not bring adverse sensory properties to the polyethylene composition.

[0011] Based on 100 parts by mass of polyethylene, the added amount of antioxidant is 0.01 to 0.3 parts, and the antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate (1010), 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (1330), 1,3,5-tris[[4-(1,1-dimethylethyl)-3-hydroxy-2,6-dimethylphenyl]methyl]-1,3,5 -triazine-2,4,6-trione (1790), N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine (1098), tris(2,4-di-tert-butylphenyl) phosphite (168), bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite (626) or at least one of 3,9-dioctadecyloxy-2,4,8,10-tetraoxy-3,9-diphosphaspiro[5.5]undecane (618).

[0012] Based on 100 parts by mass of polyethylene, the amount of the added acid absorber is 0.03 to 0.2 parts, and the acid absorber is one or more of magnesium stearate, calcium stearate, zinc stearate, and zinc oxide.

[0013] The amount of the synergist added is 0.02 to 0.2 parts per 100 parts of polyethylene, and the synergist is one or more of fumed nano-silicon dioxide, hydrated aluminate magnesium carbonate, and hydrated magnesium silicate. The nano-silicon dioxide is a commercially available product with an active surface treatment, wherein the particle size of the active nano-silicon dioxide is 10 to 30 nm. The particle sizes of the hydrated aluminate magnesium carbonate and hydrated magnesium silicate are D50≤150 nm. The synergist can help disperse the acid absorber and avoid the loss of the acid absorber and antioxidant in the subsequent processing.

[0014] The method for preparing the polyethylene composition comprises the following steps:

[0015] (1) Resin pretreatment: Place the polyethylene resin on a multi-layer distribution plate or mesh, and place it in a vacuum drying oven for vacuum drying; the preferred vacuum drying conditions are: the mesh aperture is between 80 and 120 mesh, the vacuum drying oven temperature is set between 75 and 95°C, the treatment time is 2 to 4 hours, and the vacuum degree is 0.01 to 0.03 bar. After pretreatment, the volatile matter can be further reduced, which helps to improve and enhance the sensory properties of the composition product.

[0016] (2) Mixing according to certain steps: first, add the weighed antioxidant to the pretreated polyethylene resin, place it in a high-speed stirrer and mix it evenly (preferably the speed is 1000-1500r / min, and the stirring time is 1-3min); secondly, mix the acid absorber and the synergist and add them to the polyethylene resin powder, and mix them evenly (preferably stir at a speed of 1000-1500r / min for 2-3min); this can ensure that the acid absorber and the synergist are fully dispersed, and at the same time avoid the accumulation of the acid absorber due to the influence of mechanical heat to a certain extent.

[0017] (3) Extrusion granulation: The uniformly mixed materials are added to a co-rotating twin-screw extruder for melt mixing, and the polyethylene composition is obtained by extrusion granulation. Preferably, the twin-screw extruder has a diameter of 25 mm and an aspect ratio of 40:1, the seventh section of the extruder barrel is equipped with a vacuum pump for degassing, the vacuum degree is 0.03-0.05 bar, the highest section temperature of the extruder is 160-200° C., the main engine speed of the extruder is 150-350 r / min, and the feed speed is 20-40 r / min.

[0018] The present invention also relates to the use of the polyethylene composition as described above or the polyethylene composition obtained by the method in the field of packaging materials, especially plastic bottle caps.

[0019] The present invention has the following beneficial technical effects:

[0020] 1) In the present invention, by specifically selecting and limiting the polyethylene component in the polyethylene composition, the final product has good appearance and color, good sensory properties, no odor, no abnormal taste, excellent physical properties and processing properties, can meet the requirements of compression molding or injection molding process, and is applied to bottled drinking water bottle caps, non-carbonated beverage bottle caps and other fields.

[0021] 2) The high-density polyethylene of the present invention is produced by using a high-activity metallocene catalyst, and the obtained polyethylene has high stereoregularity, moderate molecular weight distribution, and low content of low molecular weight components, which can effectively reduce thermal degradation in the subsequent extrusion process and avoid the generation of odor.

[0022] 3) The present invention improves and enhances the physical properties and sensory properties of the composition product through specific resin pretreatment and mixing steps in the preparation method. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0024] The present invention is further described below in conjunction with embodiments, and the specific embodiments and testing methods are as follows:

[0025] Example 1

[0026] High-density polyethylene (MFR is 3.5g / 10min, density is 0.9512g / cm 3 ), 100 parts of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol ester, 0.10 parts of tris(2,4-di-tert-butylphenyl) phosphite, 0.05 parts of magnesium stearate, and 0.05 parts of hydrated magnesium silicate.

[0027] Preparation method and steps of Example 1

[0028] a. Resin pretreatment: Place high-density polyethylene powder on a multi-layer distribution plate or mesh screen with a mesh aperture of 80 to 120 mesh, place in a vacuum drying oven, set the temperature to 80°C, the treatment time to 2 hours, and the vacuum degree to 0.01 to 0.02 bar.

[0029] b. Mixing according to certain steps: first, add the weighed antioxidant to the pretreated polyethylene resin, place it in a high-speed mixer and mix it evenly, the speed is 1500r / min, and the stirring time is 3min; secondly, mix the acid absorber and the synergist and add them to the polyethylene resin powder, stir at a speed of 1500r / min for 2min, and mix them evenly;

[0030] c. Extrusion granulation: The uniformly mixed materials are added to a co-rotating twin-screw extruder with a diameter of 25 mm and an aspect ratio of 40:1 for melting and kneading. The seventh section of the extruder barrel is equipped with a vacuum pump for degassing, the vacuum degree is 0.03 bar, the highest section temperature of the extruder is 180°C, the main extruder speed is 300 r / min, and the feed speed is 35 r / min. The polyethylene composition is obtained by extrusion granulation.

[0031] Example 2

[0032] High-density polyethylene (MFR is 8.0g / 10min, density is 0.9501g / cm 3 ) 100 parts, antioxidant N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine (1098) 0.15 parts, calcium stearate 0.05 parts, hydrated magnesium aluminate carbonate 0.05 parts.

[0033] Example 3

[0034] High-density polyethylene (MFR is 4.5g / 10min, density is 0.9509g / cm 3) 100 parts, antioxidant 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (1330) 0.08 parts, 3,9-dioctadecyloxy-2,4,8,10-tetraoxy-3,9-diphosphaspiro[5.5]undecane 0.08 parts, zinc oxide 0.08 parts, nano silicon dioxide 0.15 parts.

[0035] Example 4

[0036] High-density polyethylene (MFR 4.0g / 10min, density 0.9513g / cm 3 ) 100 parts, antioxidant 1,3,5-tris[[4-(1,1-dimethylethyl)-3-hydroxy-2,6-dimethylphenyl]methyl]-1,3,5-triazine-2,4,6-trione 0.05 parts, bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite 0.10 parts, zinc stearate 0.08 parts, hydrated magnesium silicate 0.08 parts.

[0037] The preparation methods and steps of Examples 2 to 4 are the same as those of Example 1.

[0038] In Examples 1 to 4, the high-density polyethylene used is produced by Sinopec Qilu Branch using metallocene catalysts, and its specifications are in compliance with the requirements in the specification; antioxidants, acid absorbers and synergists are all commercially available products; as for the synergist, the nano-silica is a commercially available product with an active surface treatment, wherein the particle size of the active nano-silica is 10 to 30 nm; the particle size of the hydrated magnesium aluminate carbonate and hydrated magnesium silicate is D50≤150 nm.

[0039] Comparative Example 1

[0040] High-density polyethylene (MFR is 4.5g / 10min, density is 0.9509g / cm 3 ), 100 parts of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol antioxidant, 0.05 parts of tris(2,4-di-tert-butylphenyl) phosphite, 0.10 parts of magnesium stearate, and 0.05 parts of hydrated magnesium silicate.

[0041] Preparation steps of Comparative Example 1

[0042] Material mixing: weigh all components according to the proportion and mix them evenly in a high-speed mixer at a speed of 1500r / min and a stirring time of 5min;

[0043] Extrusion granulation: The uniformly mixed materials are added to a co-rotating twin-screw extruder with a diameter of 25 mm and an aspect ratio of 40:1 for melting and kneading. The seventh section of the extruder barrel is equipped with a vacuum pump for degassing, the vacuum degree is 0.03 bar, the highest section temperature of the extruder is 180°C, the main engine speed of the extruder is 300 r / min, and the feed speed is 35 r / min. The polyethylene composition is obtained by extrusion granulation.

[0044] Comparative Example 2

[0045] High-density polyethylene (MFR is 2.3g / 10min, density is 0.9560g / cm 3 ), 100 parts of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] pentaerythritol antioxidant, 0.05 parts of tris(2,4-di-tert-butylphenyl) phosphite, 0.10 parts of magnesium stearate, and 0.05 parts of hydrated magnesium silicate.

[0046] Among them, high-density polyethylene (MFR is 2.3g / 10min, density is 0.9560g / cm 3 ) is a product produced by a non-metallocene catalyst. The comonomer of the product is 1-butene. The weight average molecular weight measured by GPC method is 10.8×10 4 , number average molecular weight 1.5×10 4 Among them, the proportion of low molecular weight components with a molecular weight of less than 2000 in the high-density polyethylene is 2.2%, the proportion of low molecular weight components with a molecular weight of less than 1700 is 1.7%, and the proportion of low molecular weight components with a molecular weight of less than 1000 is 0.7%.

[0047] Preparation method and steps of comparative example 2

[0048] a. Resin pretreatment: Place high-density polyethylene on a multi-layer distribution plate or mesh screen with a mesh aperture of 80 to 120 mesh, place in a vacuum drying oven, set the temperature to 80°C, the treatment time to 2 hours, and the vacuum degree to 0.01 to 0.02 bar.

[0049] b. Mixing according to certain steps: first, add the weighed antioxidant to the pretreated polyethylene resin, place it in a high-speed mixer and mix it evenly, the speed is 1500r / min, and the stirring time is 3min; secondly, mix the acid absorber and the synergist and add them to the polyethylene resin powder, stir at a speed of 1500r / min for 2min, and mix them evenly;

[0050] c. Extrusion granulation: The uniformly mixed materials are added to a co-rotating twin-screw extruder with a diameter of 25 mm and an aspect ratio of 40:1 for melting and kneading. The seventh section of the extruder barrel is equipped with a vacuum pump for degassing, the vacuum degree is 0.03 bar, the highest section temperature of the extruder is 200°C, the main speed of the extruder is 200 r / min, and the feed speed is 25 r / min. The polyethylene composition is obtained by extrusion granulation.

[0051] Comparative Example 3

[0052] High-density polyethylene (MFR is 2.3g / 10min, density is 0.9560g / cm 3 ) 100 parts, antioxidant 1,3,5-trimethyl-2,4,6-tri(3,5-di-tert-butyl-4-hydroxybenzyl)benzene (1330) 0.10 parts, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite (626) 0.20 parts, zinc stearate 0.10 parts, hydrated magnesium silicate 0.10 parts.

[0053] Preparation steps of comparative example 3

[0054] Material mixing: weigh all components according to the proportion and mix them evenly in a high-speed mixer at a speed of 1500r / min and a stirring time of 5min;

[0055] Extrusion granulation: The uniformly mixed materials are added to a co-rotating twin-screw extruder with a diameter of 25 mm and an aspect ratio of 40:1 for melt mixing. The seventh section of the extruder barrel is equipped with a vacuum pump for degassing, the vacuum degree is 0.03 bar, the highest section temperature of the extruder is 200°C, the main speed of the extruder is 200r / min, and the feed speed is 25r / min. The polyethylene composition is obtained by extrusion granulation.

[0056] The high-density polyethylene of Comparative Example 3 is the same as that of Comparative Example 2.

[0057] Among them, the antioxidants, acid absorbers and synergists in Comparative Examples 1 to 3 are all commercially available products.

[0058] Comparative Example 4

[0059] Commercially available high-density polyethylene A.

[0060] The weight average molecular weight measured by GPC method is 12.1×10 4 , number average molecular weight 0.82×10 4 The proportion of low molecular weight components with a molecular weight below 2000 is 5.3%, the proportion of low molecular weight components with a molecular weight below 1700 is 4.5%, and the proportion of low molecular weight components with a molecular weight below 1000 is 2.2%.

[0061] Comparative Example 5

[0062] Commercially available high-density polyethylene B.

[0063] The weight average molecular weight measured by GPC method is 9.4×10 4 , number average molecular weight 1.4×10 4 The proportion of low molecular weight components with a molecular weight below 2000 is 2.2%, the proportion of low molecular weight components with a molecular weight below 1700 is 1.8%, and the proportion of low molecular weight components with a molecular weight below 1000 is 0.8%.

[0064] Comparative Example 6

[0065] Commercially available high-density polyethylene C.

[0066] The weight average molecular weight measured by GPC method is 7.1×10 4 , number average molecular weight 1.4×10 4 The proportion of low molecular weight components with a molecular weight below 2000 is 2.1%, the proportion of low molecular weight components with a molecular weight below 1700 is 1.7%, and the proportion of low molecular weight components with a molecular weight below 1000 is 0.7%.

[0067] Note: The resins in Comparative Examples 4-6 are all commercially available high-density polyethylene.

[0068] The physical properties, sensory properties and gas chromatography-mass spectrometry analysis results of the polyethylene compositions prepared in various examples and comparative examples are shown in Tables 1 and 2 below.

[0069] Table 1 Performance test results of the embodiment

[0070]

[0071]

[0072] Table 2 Performance test results of comparative examples

[0073]

[0074] *Note 1: The volatile matter content is expressed as the peak area of ​​the response of C6-C18 alkane compounds;

[0075] The test method is tested in accordance with the relevant national standards and industry standards:

[0076] Melt flow rate (MFR) is carried out according to GB / T 3682.1-2018;

[0077] The simply supported beam notched impact strength is tested according to GB / T 1043-2008;

[0078] Tensile properties are tested according to GB / T1040.2-2006;

[0079] Bending properties are tested according to GB / T 9341-2008;

[0080] The yellowness index is tested in accordance with HG / T 3862-2006 using sample particles.

[0081] The volatile substances were analyzed by headspace-gas chromatography, headspace conditions: 130℃, 1h; gas chromatography conditions: injection port temperature 250℃, column initial temperature 40℃, temperature program at a heating rate of 8℃ / min, from 50℃ to 250℃, maintained for 10min, carrier gas flow rate 0.8ml / min, injection volume 1ml; mass spectrometry conditions: ion source EI, ion strength 70eV, ion source temperature 150℃, scanning range 25-450.

[0082] The odor test is to place 50g of the sample in a 1000ml wide-mouth bottle with a stopper, place it in an oven at 80℃ for 2h, cool it for 0.5h, select six people with experience in odor evaluation to smell it, and make a grade evaluation according to the evaluation criteria in Table 2.

[0083] The taste test is to prepare the sample and pure water in a mass ratio of 4:100, put it in a 500ml stoppered glass bottle, put it in a 90℃ water bath for 2 hours, and after cooling, six people drink the water soaked with the sample, and then compare it with the blank sample (pure water). The grade is judged according to the evaluation criteria in Table 3.

[0084] Table 2 Evaluation criteria

[0085] grade Judging Criteria 1 Hard to feel, no obvious difference compared with the blank sample 2 Can be felt, but not pungent 3 Can clearly feel the unpleasant smell 4 Pungent 5 Very pungent 6 Unbearable

[0086] Table 3 Evaluation criteria

[0087] grade Judging Criteria 1 No odor, no significant difference compared to blank sample 2 Can feel the taste 3 Can obviously feel the unusual taste 4 Unbearable taste

[0088] It can be seen that the polyethylene composition obtained by using the technical solution of the present invention has good appearance and color, good sensory properties, no odor, no abnormal taste, a melt mass flow rate of 3.4-8.0 g / 10 min, and a density of 0.9500-0.9513 g / cm 3 , tensile strength is 25.6~26.0Mpa, and the room temperature simply supported beam notch impact strength is 4.7~5.8kJ / m 2 The flexural elastic modulus is 1148-1180 MPa, and it has excellent physical and processing properties. It can meet the requirements of compression molding or injection molding processes and is used in bottled drinking water caps, non-carbonated beverage caps and other fields.

[0089] It can be seen from the experimental data of the comparative examples that when the technical solution of the present invention is not used, its performance has various defects. For example, the method described in comparative example 1 does not perform resin pretreatment, and its volatile matter content is high, and the odor and taste test results are different from those of Examples 1-4; the MFR and low molecular weight component ratio of the high-density polyethylene used in comparative example 2 are different from those of the present invention, and the MFR of the high-density polyethylene used in comparative example 3 is different from that of the present invention, and no resin pretreatment is performed, and its volatile matter content, odor and taste test results and other test data are obviously inferior to those of the present application; comparative examples 4-6 are different from examples 1-4 in the low molecular weight component ratio, but it can be clearly seen from their performance that they are also inferior to the present application; especially comparative example 6 has only a slight difference in the low molecular weight component ratio with the corresponding range of the present application, but has significant differences in the test results of volatile matter content, odor and taste test results with the present application. It can be seen that when the proportion of low molecular weight components in high-density polyethylene falls within the range described in the present invention, the composition can have a low content of volatile substances, no odor and abnormal taste, good sensory properties and appearance color, etc., and excellent physical properties and processing properties, and can ultimately be applied to drinking water bottle caps, non-carbonated beverage bottle caps and other fields.

[0090] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A polyethylene composition, characterized in that It is composed of the following raw materials in parts by weight: Polyethylene 100 parts; Antioxidant 0.01~0.3 parts; Acid absorbent 0.03~0.2 parts; Synergist 0.02~0.2 parts; The density of polyethylene used is 0.948~0.956g / cm 3 , melt mass flow rate MFR is 3.0~8.0g / 10min, melting point is 128~131℃; The polyethylene is high-density polyethylene; the high-density polyethylene is produced using a metallocene catalyst and has a number average molecular weight of 1.3×10 4 ~1.8×10 4 , the weight average molecular weight is 5×10 4 ~10×10 4 , the Z average molecular weight is 15×10 4 ~30×10 4 ; Among them, the proportion of low molecular weight components with a molecular weight of less than 2000 in the high-density polyethylene is less than 2%, the proportion of low molecular weight components with a molecular weight of less than 1700 is less than 1.8%, and the proportion of low molecular weight components with a molecular weight of less than 1000 is less than 0.7%.

2. The polyethylene composition according to claim 1, characterized in that The polyethylene is a copolymer of ethylene and α-olefin, wherein the α-olefin comonomer is 1-butene or 1-hexene, and the molar percentage of the comonomer is 0.1-0.5%.

3. The polyethylene composition as claimed in claim 1, further, the proportion of low molecular weight components with a molecular weight of less than 2000 in the high density polyethylene is less than 1.8%, the proportion of low molecular weight components with a molecular weight of less than 1700 is less than 1.4%, and the proportion of low molecular weight components with a molecular weight of less than 1000 is less than 0.5%.

4. The polyethylene composition according to claim 1, characterized in that The antioxidant is pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, 1,3,5-tris[[4-(1,1-dimethylethyl)-3-hydroxy-2,6-dimethylphenyl]methyl]-1,3,5-triazine-2,4,6-trione, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionyl)hexanediamine, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl) At least one of pentaerythritol diphosphite or 3,9-dioctadecyloxy-2,4,8,10-tetraoxy-3,9-diphosphospiro[5.5]undecane; the acid absorber is one or more of magnesium stearate, calcium stearate, zinc stearate and zinc oxide.

5. The polyethylene composition according to claim 1, characterized in that: The synergist is one or more of fumed nano silicon dioxide, hydrated magnesium aluminate carbonate and hydrated magnesium silicate.

6. The polyethylene composition according to claim 5, characterized in that The surface of the nano silicon dioxide is treated with activation, and its particle size is 10-30 nm; the particle size of the hydrated magnesium aluminate carbonate and hydrated magnesium silicate is D50≤150nm.

7. The method for preparing the polyethylene composition according to any one of claims 1 to 6, characterized in that: The steps include: (1) Resin pretreatment: Place the polyethylene resin on a multi-layer distribution plate or mesh screen and place it in a vacuum drying oven for vacuum drying; (2) Mixing in certain steps: first, add the weighed antioxidant to the pretreated polyethylene resin and mix it evenly in a high-speed mixer; then, mix the acid absorber and the synergist and add them to the polyethylene resin powder and mix evenly; (3) Extrusion granulation: The uniformly mixed materials are added to a co-rotating twin-screw extruder for melt mixing, and the polyethylene composition is obtained by extrusion granulation.

8. The method for preparing a polyethylene composition according to claim 7, wherein the vacuum drying conditions in step (1) are as follows: the mesh size is between 80 mesh and 120 mesh, the temperature of the vacuum drying oven is set between 75 and 95°C, the treatment time is 2 to 4 hours, and the vacuum degree is 0.01 to 0.03 bar; the stirring parameters after adding the antioxidant in step (2) are as follows: the speed is 1000 to 1500 r / min and the stirring time is 1 to 3 min, and the stirring parameters after adding the acid absorber and the synergist are as follows: the speed is 1000 to 1500 r / min and the stirring time is 2 to 3 min; the diameter of the twin-screw extruder in step (3) is 25 mm and the aspect ratio is 40:1; the seventh section of the extruder barrel is equipped with a vacuum pump for degassing, the vacuum degree is 0.03 to 0.05 bar, the temperature of the highest section of the extruder is 160 to 200°C, the main engine speed of the extruder is 150 to 350 r / min, and the feeding speed is 20 to 40 r / min.

9. Use of the polyethylene composition according to any one of claims 1 to 6 or the polyethylene composition obtained by the method according to any one of claims 7 to 8 in packaging materials.