A method for recovering platinum group metals from automobile waste catalysts using nickel-iron tailings as flux
By using nickel-iron tailings as a flux, combined with roasting and medium-frequency induction furnace smelting and capture technology, the problem of long and high-cost recycling process of platinum group metals in automobile waste catalysts in the existing technology has been solved, and an efficient and low-cost recycling process has been achieved. Platinum group metal recycling reduces environmental pollution and health risks.
Patent Information
- Application Number
- CN202211702956.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2042-12-29
AI Technical Summary
When recycling platinum group metals from spent automobile catalysts, the existing technology has long process flow, high cost, high environmental pollution and health risks, and lacks efficient and low-cost solutions.
Using nickel-iron tailings as a flux, through roasting and medium-frequency induction furnace smelting and capture processes, using carbon reducing agent and calcium oxide for roasting and smelting, glass slag and iron alloys containing platinum group metals are separated, simplifying the process and reducing resource investment .
It has achieved simplification of the process flow and efficient recovery of platinum group metals, reduced costs and environmental impact, and improved secondary resource utilization and economic benefits. The recovery rate of platinum group metals has reached more than 98%.
Smart Images

Figure CN116043028B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of resource recovery, and in particular to a method for recovering platinum group metals in automobile waste catalysts by using nickel-iron tailings as flux. Background Art
[0002] Platinum group metals mainly include six metal elements: ruthenium (Ru), rhodium (Rh), palladium (Pd), osmium (Os), iridium (Ir), and platinum (Pt). Due to their excellent corrosion resistance, oxidation resistance, ductility, electrical and thermal conductivity, they are widely used in many fields such as petrochemicals, aerospace, environmental protection, industry and agriculture, military industry, and high-tech. In recent years, the scientific and technological level of various industries has developed rapidly, and the demand for platinum group metals has increased. There are a large number of platinum group metals such as platinum, rhodium, and palladium in secondary resources such as waste automobile catalysts, so it is particularly important to strengthen the comprehensive utilization of secondary resources and extract and recover platinum group metals from secondary resources.
[0003] At present, automobile exhaust catalyst is the largest application field of platinum group metals in China. Platinum, rhodium and palladium used in automobile exhaust catalyst account for more than 60% of the total demand in China, of which rhodium accounts for 80%-90% of the total demand. While the usage is huge, the output of waste automobile catalyst is also increasing year by year. As hazardous solid waste, it is urgent to treat and recycle it to achieve environmental protection and secondary utilization of platinum group metals.
[0004] At present, there are two main methods for recycling platinum group metals from waste automobile catalysts: hydrometallurgy and pyrometallurgy. Among them, pyrometallurgy uses base metals such as copper, lead, iron, and nickel that have strong affinity with platinum group metals as collectors, and compared with the hydrometallurgical process, it has the characteristics of less wastewater and waste gas, high recovery rate of platinum group metals, and large processing capacity, and is widely used in the field of platinum group metal recycling.
[0005] Patent CN111575489 A discloses a method for treating waste automobile exhaust catalyst by pyrometallurgy, the steps of which are: (1) coarsely grinding and ultrafine grinding the waste automobile exhaust catalyst, and then mixing and granulating with copper-containing hazardous waste; (2) adding the waste automobile exhaust catalyst to an oxygen-enriched side-blown furnace for smelting, and using the copper in the copper-containing hazardous waste as a collector to capture rare and precious metals; (3) blowing and refining the matte and crude copper obtained in step (2) to obtain a copper anode plate and electrolyzing it to obtain copper anode mud; (4) subjecting the anode mud obtained in step (3) to a wet extraction process to extract rare and precious metals such as platinum, rhodium and palladium; (5) comprehensive utilization of slag; and (6) comprehensive utilization of furnace flue gas. This method uses Cu as a collector, can effectively recover rare and precious metals such as platinum group metals in automobile exhaust catalyst, and simultaneously treats automobile exhaust catalyst and copper-containing hazardous waste. However, obtaining platinum group metals from anode copper by electrolysis increases the extraction cost and prolongs the entire recovery cycle, and there are also problems such as difficulty in treating wastewater.
[0006] Patent CN 102134647 A discloses a method for extracting platinum group metals from waste automobile three-way catalysts. This method mainly utilizes the lead metal smelting and capturing method. This method uses the existing technology to smelt and capture the waste automobile three-way catalyst with lead metal to obtain a lead alloy, and then vacuum distills the lead and platinum group metals. This method is simple in process and low in cost, but because lead is volatile and toxic, it is easy to pollute the environment during the recovery process and endanger the health of workers. In addition, this method also has the disadvantages of poor raw material adaptability, long process flow, and low metal leaching rate.
[0007] Patent CN109338107 A discloses a method for comprehensive environmentally friendly recycling of waste three-way catalysts. The method mainly uses iron-based metals as a collector to recover platinum group metals. The steps are as follows: (1) crushing and separating the waste automobile exhaust pipe of the waste three-way catalyst to obtain the waste three-way catalyst; (2) incinerating the waste three-way catalyst obtained by step (1) and preparing it into powder; (3) using an electric arc furnace to dry extract and smelt the waste three-way catalyst powder obtained by step (2) to obtain an iron block enriched with platinum group metals and a harmless waste three-way catalyst carrier; (4) using a process of graded extraction and resin adsorption to separate the iron block and the platinum group metals, and then further purifying the platinum group metals to obtain platinum group metals with a purity of more than 99.9%. This method combining pyrometallurgy and hydrometallurgy has a high recovery rate, and the purity of the obtained platinum group metals has also reached the level of industrial application. However, this method has disadvantages such as complicated process, high energy consumption, single type of waste treatment, many types and quantities of auxiliary materials added, and high cost of subsequent tailings treatment. Therefore, the overall recycling cost is high and the economic benefits are low.
[0008] Therefore, there is an urgent need for a method for recovering platinum group metals from automobile waste catalysts with a short process flow, high efficiency and low cost. Summary of the invention
[0009] The technical problem to be solved by the present invention is to provide a method for recovering platinum group metals in automobile waste catalysts by using nickel-iron tailings as flux, which has a short process flow, high efficiency and low cost.
[0010] In order to solve the above technical problems, the present invention provides a method for recovering platinum group metals from automobile waste catalysts using nickel-iron tailings as flux, comprising the following steps:
[0011] The nickel-iron tailings, automobile waste catalyst, carbon reducing agent, calcium oxide flux and iron collector are uniformly mixed to obtain a mixture;
[0012] roasting the mixture to obtain a roasted product;
[0013] The roasted product is smelted and captured to obtain glass slag and ferroalloy containing platinum group metals.
[0014] Furthermore, the mass ratio of the automobile waste catalyst and the nickel-iron tailings is controlled to be (30-10): (70-90), the mass of the carbon reducing agent is 5.9wt%-23wt% of the mass of the automobile waste catalyst, and the mass of the carbon reducing agent is 1.4-1.6 times the theoretical amount for fully reducing the iron oxides in the nickel-iron tailings, the mass of the iron collector is 2.0wt%-59wt% of the mass of the automobile waste catalyst, and the mass of the iron collector is to ensure that the content of platinum group metals in the ferroalloy is above 0.2%.
[0015] Furthermore, the ternary basicity of the mixture is controlled at 0.6 to 0.8.
[0016] Furthermore, the nickel-iron tailings, automobile waste catalyst, carbon reducing agent, calcium oxide and iron collector are all crushed into powders of 150-250 mesh.
[0017] Furthermore, the carbon reducing agent is metallurgical coke or coal powder, and the iron collector is iron powder.
[0018] Furthermore, the mixture is calcined in a muffle furnace at a temperature of 800-1000° C. for a time of 1-2 hours.
[0019] Furthermore, the calcined product is smelted in a medium frequency induction furnace at a smelting temperature of 1550-1600° C. for a smelting time of 1-2 hours.
[0020] Furthermore, the slag system in the roasting product is a SiO2-CaO-Al2O3-MgO-FeO five-element slag system, and the mass proportions of SiO2, CaO, Al2O3, MgO and FeO in the slag system are: SiO2:CaO:Al2O3:MgO:FeO=(39.3~51.9):(3.8~5.1):(38.1~18.4):(18.2~24.0):(0~2).
[0021] Furthermore, the roasted product is naturally stratified during the smelting and capturing process, with the upper layer being the glassy slag and the lower layer being the ferroalloy containing platinum group metals.
[0022] Furthermore, after the calcined product is smelted and captured, the glass slag on the upper layer is poured away, and the ferroalloy containing platinum group metals on the lower layer is cooled and separated to obtain the ferroalloy containing platinum group metals.
[0023] The present invention provides a method for recovering platinum group metals in automobile waste catalysts by using nickel-iron tailings as flux. The nickel-iron tailings are used as flux to recover platinum group metals in automobile waste catalysts. While treating waste automobile catalysts to recover platinum group metals, the nickel-iron tailings, a solid waste, are also treated. Furthermore, the amount of iron collector and slag-making material added is greatly reduced, thereby improving the utilization rate of secondary resources, saving resources, reducing costs, and improving economic benefits.
[0024] In addition, the method provided by the present invention uses nickel-iron tailings as flux to recover platinum group metals in automobile waste catalysts, which mainly involves two processes: roasting and smelting and capturing. The entire process flow is relatively short, and not only can it process a variety of solid wastes at the same time, but also requires less resource input, is environmentally friendly, has low production costs, and has high economic benefits.
[0025] At the same time, the present invention provides a method for recovering platinum group metals from automobile waste catalysts using nickel-iron tailings as flux. Since the upper layer after smelting and capturing is glass slag, and the lower layer is produced as ferroalloy containing platinum group metals, the glass slag can well fix the ferroalloy containing platinum group metals, and after cooling, the ferroalloy containing platinum group metals can be easily separated from the glass slag. At the same time, the recovery efficiency of platinum group metals in automobile waste catalysts is also very high. After the recovery is completed, the content of platinum group metals in the glass slag is less than 10g / t, and the recovery rate is as high as more than 98%. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A flow chart of a method for recovering platinum group metals from automobile waste catalysts using nickel-iron tailings as flux is provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0027] See also Figure 1 The present invention provides a method for recovering platinum group metals from automobile waste catalysts using nickel-iron tailings as flux, comprising the following steps:
[0028] Firstly, nickel-iron tailings, automobile waste catalyst, carbon reducing agent, calcium oxide flux and iron collector are uniformly mixed to obtain a mixture.
[0029] Among them, nickel-iron tailings, automobile waste catalysts, carbon reducing agents, calcium oxide and iron collectors are all crushed into powders of 150-250 meshes by a crusher before mixing.
[0030] The mass ratio of automobile waste catalyst to nickel-iron tailings is controlled to be (30-10): (70-90), the mass of the carbon reducing agent is controlled to be 5.9wt%-23wt% of the mass of the automobile waste catalyst, and the mass of the carbon reducing agent is 1.4-1.6 times the theoretical amount for fully reducing the iron oxides in the nickel-iron tailings. The mass of the iron collector is controlled to be 2.0wt%-59wt% of the mass of the automobile waste catalyst, and the mass of the iron collector is required to ensure that the content of the platinum group metal in the ferroalloy is above 0.2%.
[0031] Wherein, the carbon reducing agent is metallurgical coke or coal powder, and the iron collector is iron powder.
[0032] Furthermore, in order to control the viscosity and other properties of the glass slag obtained by smelting and capturing at high temperatures during the subsequent smelting process of the raw materials, so that the properties of the glass slag meet the smelting requirements and facilitate the separation of the glass slag obtained by smelting and capturing and the ferroalloy containing platinum group metals, the ternary basicity of the mixture obtained after mixing the raw materials is controlled within the range of 0.6 to 0.8 by controlling the amount of calcium oxide added.
[0033] Then, in order to speed up the smelting and capturing progress in the next step, the above mixture is pre-reduced to a certain extent. The mixture is placed in a muffle furnace for roasting to obtain a roasted product. The roasting temperature is controlled at 800-1000°C and the roasting time is controlled at 1-2h.
[0034] By controlling the composition of the raw materials and the mass ratio of each component, the slag system in the calcined product obtained after the mixture is calcined is a five-element slag system of SiO2-CaO-Al2O3-MgO-FeO, wherein the mass proportions of SiO2, CaO, Al2O3, MgO and FeO in the slag system are: SiO2:CaO:Al2O3:MgO:FeO=(39.3~51.9):(3.8~5.1):(38.1~18.4):(18.2~24.0):(0~2).
[0035] Finally, the roasted product is melted and captured in a graphite crucible of a medium frequency induction furnace to obtain glass slag and an iron alloy containing platinum group metals. The melting temperature is controlled at 1550-1600°C and the melting time is controlled at 1-2 hours.
[0036] During the smelting and capturing process of the roasted product, due to the different specific gravities of the ferroalloy containing platinum group metals and the glass slag obtained by smelting, the two substances will settle in the graphite crucible and naturally stratify, wherein the glass slag with lower density is in the upper layer, and the ferroalloy containing platinum group metals with higher density is in the lower layer. After the smelting and capturing of the roasted product is completed, the glass slag in the upper layer of the graphite crucible is poured into another graphite crucible, and the glass slag is obtained after cooling. The remaining ferroalloy containing platinum group metals in the graphite crucible is naturally cooled in the graphite crucible to obtain the solidified ferroalloy containing platinum group metals. The ferroalloy containing platinum group metals can be subsequently separated to obtain the platinum group metals.
[0037] The following is a specific description of a method for recovering platinum group metals from automobile waste catalysts using nickel-iron tailings as flux provided by the present invention. The composition of the nickel-iron tailings used in the following embodiments is shown in Table 1.
[0038] Example 1
[0039] 1. Take the above 0.7 kg of nickel iron tailings and crush them in a sample making machine to 120-200 mesh.
[0040] 2. Evenly mix the crushed nickel-iron tailings, 0.3kg of discarded automobile catalyst, 0.017kg of carbon reducing agent, 0.035kg of calcium oxide flux and 0.17kg of iron collector. The discarded automobile catalyst contains 99.22% Al2O3 and 1594.9g / t Pd, the main component of the carbon reducing agent is metallurgical coke (fixed carbon content is 69.7%, ash content is 7.65%, and volatile matter is 16.13%), and high-purity iron powder is used as the Pd collector.
[0041] 3. Place the mixed materials in a muffle furnace for full roasting at a temperature of 800-1000°C for 1 hour. After roasting, place them in a medium frequency induction furnace for smelting and capture at a temperature of 1550-1600°C for 2 hours. During the smelting process, they are naturally stratified, with the upper layer being a glass slag layer and the lower layer being an iron alloy layer containing platinum group metals.
[0042] 4. After the smelting is completed, the upper slag liquid of the graphite crucible is poured into another graphite crucible, and the remaining part is taken out from the graphite crucible and separated after it is naturally cooled in the air, and finally glass slag and iron alloy containing platinum group metals are obtained.
[0043] 5. Finally, the composition of the glass slag and the alloy was determined. The content of platinum group metals in the slag was 8.3 g / t, and the recovery rate of platinum group metals was 98.35%.
[0044] Example 2
[0045] 1. Take the above 0.8 kg of nickel-iron tailings and crush them in a sample making machine to 120-200 mesh.
[0046] 2. Evenly mix the crushed nickel-iron tailings, 0.2kg of discarded automobile catalyst, 0.020kg of carbon reducing agent, 0.040kg of calcium oxide flux and 0.090kg of iron collector. The discarded automobile catalyst contains 99.22% Al2O3 and 1594.9g / t Pd, the carbon reducing agent mainly contains metallurgical coke (fixed carbon content is 69.7%, ash content is 7.65%, and volatile matter content is 16.13%), and the iron collector mainly contains high-purity iron powder.
[0047] 3. Place the mixed materials in a muffle furnace for full roasting at a temperature of 800-1000°C for 1 hour. After roasting, place them in a medium frequency induction furnace for smelting and capture at a temperature of 1550-1600°C for 2 hours. During the smelting process, they are naturally stratified, with the upper layer being a glass slag layer and the lower layer being an iron alloy layer containing platinum group metals.
[0048] 4. After the smelting is completed, the upper slag liquid of the graphite crucible is poured into another graphite crucible, and the remaining part is taken out from the graphite crucible and separated after it is naturally cooled in the air, and finally glass slag and ferroalloy containing platinum group metals are obtained.
[0049] 5. Finally, the composition of the glass slag and the alloy was determined. The content of platinum group metals in the slag was 5.2 g / t, and the recovery rate of platinum group metals was greater than 98.51%.
[0050] Example 3
[0051] 1. Take the above 0.9 kg of nickel iron tailings and crush them in a sample making machine to 120-200 mesh.
[0052] 2. Evenly mix the crushed nickel-iron tailings, 0.1kg of discarded automobile catalyst, 0.023kg of carbon reducing agent, 0.045kg of calcium oxide flux and 0.0020kg of iron collector. The discarded automobile catalyst contains 99.22% Al2O3 and 1594.9g / t Pd, the carbon reducing agent mainly contains metallurgical coke (fixed carbon content is 69.7%, ash content is 7.65%, and volatile matter content is 16.13%), and the iron collector mainly contains high-purity iron powder.
[0053] 3. Place the mixed materials in a muffle furnace for full roasting at a temperature of 800-1000°C for 1 hour. After roasting, place them in a medium frequency induction furnace for smelting and capture at a temperature of 1550-1600°C for 2 hours. During the smelting process, they are naturally stratified, with the upper layer being a glass slag layer and the lower layer being an iron alloy layer containing platinum group metals.
[0054] 4. After the smelting is completed, the upper slag liquid of the graphite crucible is poured into another graphite crucible, and the remaining part is taken out from the graphite crucible and separated after it is naturally cooled in the air, and finally glass slag and ferroalloy containing platinum group metals are obtained.
[0055] 5. Finally, the composition of the glass slag and the alloy was determined. The Pd content in the slag was 4.8 g / t, and the recovery rate of platinum group metals was 99.83%.
[0056] Comparative Example 1
[0057] 1. Take analytically pure samples of 0.36 kg SiO2, 0.014 kg CaO, 0.05 kg Al2O3, 0.17 kg MgO and 0.034 kg FeO and mix the samples evenly.
[0058] 2. The mixed sample was mixed evenly with 0.3 kg of discarded automobile catalyst, 0.017 kg of carbon reducing agent, 0.035 kg of calcium oxide flux and 0.17 kg of iron collector. The discarded automobile catalyst contained 99.22% Al2O3 and 1594.9 g / t Pd, the main component of the carbon reducing agent was metallurgical coke (fixed carbon content was 69.7%, ash content was 7.65%, and volatile matter content was 16.13%), and high-purity iron powder was used as the Pd collector.
[0059] 3. Place the mixed materials into a muffle furnace for full roasting.
[0060] 800~1000℃, roasting for 1h. After roasting, it is placed in a medium frequency induction furnace for smelting and capture, the smelting temperature is 1550~1600℃, smelting for 2h, and natural stratification occurs during the smelting process, with the upper layer being the glass slag layer.
[0061] The lower layer is an iron alloy layer containing platinum group metals.
[0062] 4. After the smelting is completed, the upper slag liquid of the graphite crucible is poured into another graphite crucible, and the remaining part is taken out from the graphite crucible and separated after it is naturally cooled in the air, and finally glass slag and ferroalloy containing platinum group metals are obtained.
[0063] 5. Finally, the composition of the glass slag and alloy was determined. The Pd content in the slag was 7.8g / t, and the platinum group
[0064] The recovery rate of metal was 98.45%.
[0065] By comparing Examples 1-3 provided by the present invention with Comparative Example 1, it can be seen that the three embodiments of the present invention add nickel-iron tailings to discarded automobile catalysts to recover platinum group metals, and the same smelting effect is achieved as that of recovering platinum group metals using pure substances.
[0066] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for recovering platinum group metals from automobile waste catalysts using nickel-iron tailings as flux, It is characterized in that The steps include: The nickel-iron tailings, automobile waste catalyst, carbon reducing agent, calcium oxide flux and iron collector are uniformly mixed to obtain a mixture with a ternary basicity of 0.6-0.8; The mixture is calcined at 800-1000°C for 1-2h to obtain a calcined product; The roasted product is smelted and captured to obtain glass slag and ferroalloy containing platinum group metals; The mass ratio of the automobile waste catalyst and the nickel-iron tailings is controlled to be (30-10): (70-90), the mass of the carbon reducing agent is 5.9wt%-23wt% of the mass of the automobile waste catalyst, and the mass of the carbon reducing agent is 1.4-1.6 times the theoretical amount for fully reducing the iron oxides in the nickel-iron tailings, the mass of the iron collector is 2.0wt%-59wt% of the mass of the automobile waste catalyst, and the mass of the iron collector is to ensure that the content of platinum group metals in the ferroalloy is above 0.2%.
2. The method for recovering platinum group metals from automobile waste catalysts using ferronickel tailings as flux according to claim 1, Features: The nickel-iron tailings, automobile waste catalyst, carbon reducing agent, calcium oxide and iron collector are all crushed into powders of 150-250 meshes.
3. The method for recovering platinum group metals from automobile waste catalysts using ferronickel tailings as flux according to claim 1, Features: The carbon reducing agent is metallurgical coke or coal powder, and the iron collecting agent is iron powder.
4. The method for recovering platinum group metals from automobile waste catalysts using ferronickel tailings as flux according to claim 1, Features: The mixture is calcined in a muffle furnace.
5. The method for recovering platinum group metals from automobile waste catalysts using ferronickel tailings as flux according to claim 1, Features: The calcined product is smelted in a medium frequency induction furnace at a smelting temperature of 1550-1600° C. for a smelting time of 1-2 hours.
6. The method for recovering platinum group metals from automobile waste catalysts using ferronickel tailings as flux according to claim 5, Features: The slag in the calcined product is SiO 2 -CaO-Al 2 O 3 -MgO-FeO five-element slag system, the SiO 2 、CaO、Al 2 O 3 The mass proportions of SiO, MgO and FeO in the slag system are: 2 :CaO:Al 2 O 3 : MgO: FeO= (39.3~51.9): (3.8~5.1): (38.1~18.4): (18.2~24.0): (0~2).
7. The method for recovering platinum group metals from automobile waste catalysts using ferronickel tailings as flux according to claim 5, Features: The roasted product is naturally stratified during the smelting and capturing process, wherein the upper layer is the glassy slag and the lower layer is the ferroalloy containing platinum group metals.
8. The method for recovering platinum group metals from automobile waste catalysts using ferronickel tailings as flux according to claim 7, Features: After the calcined product is smelted and captured, the glass slag on the upper layer is poured away, and the ferroalloy containing platinum group metals on the lower layer is cooled and separated to obtain the ferroalloy containing platinum group metals.