Nickel cobalt sulfide treatment method
By using oxidants and catalysts for selective oxidation leaching and preliminary impurity removal in nickel cobalt sulfide treatment, combined with deep extraction and impurity removal, the problems of cumbersome process flow and low impurity removal efficiency in the traditional process are solved, and efficient nickel and cobalt sulfide treatment is achieved. The separation of manganese and cobalt impurities and the purification of nickel sulfate solution simplify the process and significantly reduce the impurity content.
Patent Information
- Application Number
- CN202211606872.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-13
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2042-12-13
AI Technical Summary
The traditional nickel-cobalt sulfide treatment process requires a huge flow extraction and separation system. The process is cumbersome and the impurity removal efficiency is low. It is difficult to quickly and efficiently convert the nickel-cobalt sulfide intermediate products produced by laterite nickel ore hydrometallurgy into ternary power. Nickel sulfate solution for batteries.
By adding oxidants and catalysts to the lateritic nickel ore hydrometallurgical intermediate product for selective oxidation leaching, combined with a neutralizing agent for preliminary impurity removal, controlling the temperature and pH value, filtering and extracting impurities, and using evaporation and crystallization to obtain pure sulfuric acid The nickel solution is loaded with organic reverse extraction and returned to the selective oxidation step to simplify the process and reduce the system volume.
It achieves efficient separation of impurities such as nickel and manganese and cobalt, shortens the process flow, significantly reduces the flow rate and number of stages of the extraction system, increases the nickel leaching rate and impurity precipitation rate, and reduces the impurity content in the nickel sulfate solution to ppm after deep extraction. level, the cobalt content is reduced hundreds of times.
Smart Images

Figure CN116043032B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metallurgy, and in particular to a method for treating nickel-cobalt sulfide. Background Art
[0002] The hydrometallurgical production of laterite nickel ore produces a large amount of nickel-cobalt intermediate products, among which nickel cobalt sulfide (MSP) has the advantages of high nickel-cobalt content and low impurity content. However, the traditional nickel-cobalt sulfide treatment process, in order to remove manganese and cobalt impurities in the final product nickel sulfate solution, uses an extraction and impurity removal and nickel-cobalt separation system with a huge flow rate and a cumbersome process flow.
[0003] Therefore, how to quickly and efficiently convert the nickel-cobalt sulfide intermediate product produced by laterite nickel ore hydrometallurgy into nickel sulfate solution to meet the application requirements in ternary power batteries is currently a major focus in laterite nickel ore hydrometallurgy. Summary of the invention
[0004] The purpose of the present invention is to provide a method for treating nickel cobalt sulfide to solve the problems that the prior art requires a huge flow rate extraction and separation system to remove impurities, the process is cumbersome, and the impurity removal efficiency is low. The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0005] According to one aspect of the present invention, the present invention provides a method for treating nickel-cobalt sulfide, comprising:
[0006] Using nickel cobalt sulfide, an intermediate product of laterite nickel ore hydrometallurgy, as raw material, adding an oxidant and a catalyst for selective oxidation leaching, controlling the temperature to 100°C to 200°C, the pH to 2.5 to 5.5, adding a neutralizing agent for preliminary impurity removal and controlling the end point pH to 4.5 to 5.5, filtering to obtain a nickel-containing solution and an impurity-containing filter residue; wherein the catalyst is selected from one or more sulfur-containing compounds;
[0007] The nickel-containing solution is extracted and impurities are removed to obtain a nickel sulfate solution, and nickel sulfate is obtained by evaporation and crystallization;
[0008] The loaded organic phase is reversely extracted, the organic phase is returned to the extraction and impurity removal step, and the impurity sulfate solution is returned to the selective oxidation leaching step.
[0009] Optionally, the selective oxidation leaching has an oxidation time of 1 hour to 24 hours, and a liquid-solid ratio of (2 to 8): 1. The selective oxidation leaching is pressurized oxidation leaching at a temperature of 100-200 degrees.
[0010] Optionally, the oxidant is one of oxygen, compressed air and enriched oxygen, wherein the oxygen partial pressure is controlled at 3 bar to 5 bar.
[0011] Optionally, the catalyst is one or more of sulfur dioxide or flue gas containing sulfur dioxide, sodium sulfite, sodium pyrosulfite, ferrous sulfate, ferrous sulfide, sodium bisulfite, ammonium sulfite, ammonium bisulfite, sodium thiosulfate, calcium sulfite, and sulfur.
[0012] Optionally, the catalyst is added in an amount of 1% to 25% of the dry weight of the raw material.
[0013] Optionally, the neutralizing agent is alkaline and is selected from one or more of sodium carbonate, sodium hydroxide, calcium hydroxide, ammonia water, calcium oxide, potassium hydroxide, magnesium oxide, magnesium carbonate, magnesium hydroxide, calcium carbonate, nickel hydroxide, nickel oxide, cobalt oxide, cobalt hydroxide, nickel cobalt hydroxide, manganese hydroxide, nickel carbonate, cobalt carbonate, and manganese carbonate.
[0014] Optionally, during the extraction and impurity removal process, the extracted organic phase is p204 and the O / A ratio is 1:1.
[0015] Optionally, after the preliminary impurity removal, the nickel leaching rate is not less than 99.9%, the cobalt precipitation rate is not less than 99.9%, and the manganese precipitation rate is not less than 99.9%.
[0016] Optionally, in the nickel sulfate solution obtained after the extraction and impurity removal, the cobalt content is <5ppm, the manganese content is <10ppm, and the total content of other impurities is <10ppm.
[0017] Beneficial effects: The nickel-cobalt sulfide treatment method of the present invention uses MSP as a raw material, and selectively oxidizes and leaches and performs preliminary impurity removal by adding an oxidant, a catalyst and a neutralizer and controlling the reaction conditions, thereby separating nickel from impurities such as cobalt, manganese, iron, aluminum and scandium (i.e., the Ni element is dissolved in the liquid phase, and other metal impurities form a precipitate), and the almost pure nickel-containing solution obtained by the preliminary impurity removal is subjected to deep extraction and impurity removal to obtain a pure nickel sulfate solution, which is then evaporated and crystallized to obtain nickel sulfate crystals. The entire process of the present invention is very short, the system volume is much reduced, and the number of extraction stages is greatly reduced compared to the traditional extraction and impurity removal system; wherein, in the nickel-containing leaching solution obtained by the preliminary impurity removal, impurities such as manganese are reduced to the ppm level, and cobalt is enriched in the manganese precipitate residue, which can be extracted separately; after deep extraction and impurity removal, the cobalt in the nickel sulfate solution is also reduced to the ppm level, and the concentration is several hundred times smaller than that in the original process. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 It is a schematic flow chart of a method for treating nickel-cobalt sulfide in one embodiment of the present invention. DETAILED DESCRIPTION
[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] Figure 1 The process of the nickel-cobalt sulfide treatment method in one embodiment is schematically shown. Figure 1 As shown, a method for treating nickel cobalt sulfide provided in this embodiment comprises: taking nickel cobalt sulfide, an intermediate product of laterite nickel ore hydrometallurgy, as a raw material, adding an oxidant and a catalyst for selective oxidation leaching, adding a neutralizing agent for preliminary impurity removal, filtering to obtain a liquid nickel-containing solution and a solid impurity-containing filter residue; adding an extraction organic phase to the nickel-containing solution for extraction and impurity removal to obtain a nickel sulfate solution, and evaporating and crystallizing to obtain nickel sulfate; after extraction, the organic phase is loaded for stripping, and the organic phase is returned to the extraction and impurity removal step, and the impurity sulfate solution is returned to the selective oxidation leaching step.
[0021] The present invention can obtain a pure nickel sulfate solution through two main processes of selective oxidation leaching and preliminary impurity removal and deep extraction and impurity removal. The whole treatment process is very short, and the nickel-containing solution obtained after oxidation leaching and preliminary impurity removal is almost pure, the nickel leaching rate is not less than 99.9%, the cobalt precipitation rate is not less than 99.9%, and the manganese precipitation rate is not less than 99.9%, which effectively realizes the separation of nickel and impurities such as manganese and cobalt, and then facilitates the subsequent deep extraction and impurity removal, so that the subsequent deep extraction and impurity removal system is greatly reduced, and the extraction stage is greatly reduced, thereby solving the problem of the traditional process of extracting and removing impurities from the nickel-cobalt solution and the huge flow rate of the nickel-cobalt separation system; and the impurity content in the nickel sulfate solution obtained after the deep extraction and impurity removal of the present invention is very low, especially the cobalt content is reduced to ppm level, which is hundreds of times lower than the traditional process.
[0022] In addition, in the selective oxidation leaching and preliminary impurity removal step, the following reagents are selected.
[0023] The catalyst is selected from one or more sulfur-containing compounds; further, selected from one or more compounds containing SO2 groups; further, it can be one or more of sulfur dioxide or flue gas containing sulfur dioxide, sodium sulfite, sodium pyrosulfite, ferrous sulfate, ferrous sulfide, sodium bisulfite, ammonium sulfite, ammonium bisulfite, sodium thiosulfate, calcium sulfite, and sulfur. In order to improve the selective oxidation leaching effect, sodium pyrosulfite, sulfur dioxide, or flue gas containing sulfur dioxide is preferred.
[0024] The oxidant is an oxygen-containing gas, and further can be one of oxygen, compressed air, and oxygen-enriched air.
[0025] The neutralizing agent is an alkaline aqueous solution, and is a compound that can provide hydroxide ions or carbonate ions to precipitate metal impurities other than nickel and separate impurities from nickel; for example, it can be selected from one or more of sodium carbonate, sodium hydroxide, calcium hydroxide, ammonia water, calcium oxide, potassium hydroxide, magnesium oxide, magnesium carbonate, magnesium hydroxide, calcium carbonate, nickel hydroxide, nickel oxide, cobalt oxide, cobalt hydroxide, nickel cobalt hydroxide, manganese hydroxide, nickel carbonate, cobalt carbonate, and manganese carbonate. Selecting the above neutralizing agent can reduce the introduction of other impurities. Preferably, the neutralizing agent is selected from nickel carbonate or nickel hydroxide. Further preferably, using nickel hydroxide as a neutralizing agent can avoid the introduction of other impurities, and also reduce the subsequent deep extraction and impurity removal process steps, reduce the flow rate of the extraction and impurity removal system, and be safer.
[0026] The neutralization and preliminary impurity removal and the selective oxidation leaching are carried out simultaneously in the present invention; the oxidation precipitation is mainly the oxidation of variable valence metals, such as manganese and cobalt, which are catalytically oxidized and precipitated in the kettle. During the oxidation process of manganese and cobalt, hydrolysis and acid release are carried out, and these acids are neutralized by adding an alkaline neutralizer. Taking cobalt as an example, the following describes some of the chemical reactions involved in the process:
[0027] CoS+O2=CoSO4(leaching);
[0028] Co 2+ +O2=Co 3+ (catalytic oxidation);
[0029] Co 3+ +H2O=Co(OH)3+H + ;
[0030] The oxidized precipitate is filtered and retained in the filter cake, which can be treated separately after washing to recover the various metals therein.
[0031] In an optional embodiment, the selective oxidation leaching adopts pressurized leaching, and the leaching temperature is controlled at 100°C to 200°C, for example, it can be 120°C, 140°C, 160°C, 180°C, etc. The total pressure of the kettle can be the saturated vapor pressure of water at this temperature. On the basis of this pressure, oxygen is introduced to increase 3 to 5 bar. Specifically, pure oxygen can be introduced as an oxidant to control the oxygen partial pressure at 3 bar to 5 bar. Selective oxidation leaching based on the above conditions can accelerate the catalytic oxidation process, accelerate the leaching speed, and improve the leaching efficiency.
[0032] In order to improve the oxidation leaching effect, during the oxidation process, the pH is controlled at 2.5-5.5, the liquid-solid ratio is controlled at (2-8):1, and the oxidation time is 1h-24h. Furthermore, the neutralizer is pumped into the autoclave in the form of slurry, and the pH end point of the above process is controlled to be 4.5-5.5. Based on the oxidation leaching under the above conditions, the oxidation rate of manganese and cobalt can be increased, so that most of the cobalt is oxidized and precipitated.
[0033] In order to ensure the degree of nickel leaching and the degree of precipitation of impurities such as manganese and cobalt, the added amount of the catalyst is preferably 1% to 25% of the dry weight of the raw material, for example, 5%, 10%, 15%, 20%, etc.
[0034] In the selective oxidation leaching and preliminary impurity removal step, by selecting a catalyst and a neutralizing agent and controlling the reaction conditions, the obtained nickel-containing solution is almost pure and the separation of nickel from impurities such as manganese and cobalt is achieved, providing convenient conditions for subsequent deep extraction and impurity removal. Specifically, after the leaching and impurity removal treatment in this step, the nickel leaching rate is not less than 99.9%, the cobalt precipitation rate is not less than 99.9%, and the manganese precipitation rate is not less than 99.9%. Other impurities remain in the slag. In the leachate, impurities such as manganese are reduced to the ppm level, most of the cobalt is enriched in the manganese slag and can be extracted separately, and the liquid phase cobalt is also reduced to the ppm level, which is several hundred times smaller than that in the original process.
[0035] In the deep extraction and impurity removal step: P204 or the like can be used to extract and remove impurities from the filtered liquid phase, and the O / A ratio is preferably 1:1. After extraction, a pure nickel sulfate solution is obtained, and the nickel sulfate solution is subjected to an evaporation crystallization process to produce nickel sulfate crystals, thereby achieving deep extraction and purification of nickel sulfate, and the extraction process is simple.
[0036] In addition, P507 can also be used to extract cobalt, but the cobalt extraction level of P507 is also far lower than the existing process; moreover, if all the cobalt is precipitated, the step of extracting cobalt with P507 can be omitted, thereby simplifying the extraction process to the greatest extent.
[0037] The technical solution of the present invention is further described below in conjunction with specific embodiments:
[0038] Example 1
[0039] MSP nickel cobalt sulfide is used as raw material, with a moisture content of 40%, a nickel content of 50%, a cobalt content of 5%, and a manganese content of 10% on a dry basis.
[0040] The process adopts pressure leaching, the temperature is 150℃, the leaching time is 4h, the pH is controlled at 3.5, the liquid-solid ratio is 8:1, pure oxygen is introduced as an oxidant, the oxygen partial pressure is controlled at 4bar, a saturated solution of sodium metabisulfite is added as a catalyst, the catalyst accounts for 5% of the dry weight of the raw material, nickel hydroxide is used as a neutralizer, and the end point pH is controlled at 4.8; after the reaction is completed, the slurry is filtered, and the filter cake is washed and treated separately as iron-cobalt-manganese-scandium-aluminum slag. According to the test, the nickel leaching rate is 99.9%, the cobalt precipitation rate is 99.9%, the manganese precipitation rate is 99.9%, and other impurities remain in the slag. The nickel sulfate solution contains cobalt <5ppm, manganese <10ppm, and the sum of other impurities is <10ppm, realizing the chemical precipitation separation of nickel and manganese and cobalt.
[0041] The filtered liquid phase is extracted and impurities are removed using p204 with an O / A ratio of 1:1. After extraction, a pure nickel sulfate solution is obtained. The nickel sulfate is also evaporated and crystallized to obtain nickel sulfate crystals. The loaded organic phase is reversely extracted to obtain an impurity sulfate solution, which is returned to the above-mentioned autoclave for precipitation treatment, and the organic phase is returned to the extraction and impurity removal step for reuse.
[0042] In Example 1 of the present invention, impurities such as manganese in the leachate are reduced to the ppm level, cobalt is enriched in manganese slag and extracted separately, and liquid phase cobalt is also reduced to the ppm level, which is several hundred times lower than that in the original process. The extraction level of the nickel sulfate solution p204 extraction and impurity removal process and the p507 cobalt extraction level are greatly reduced compared with the original process.
[0043] The description of the present invention is given for the purpose of illustration and description, and is not intended to be exhaustive or to limit the invention to the disclosed form. Many modifications and variations will be apparent to those of ordinary skill in the art. The embodiments are selected and described in order to better illustrate the principles and practical applications of the present invention and to enable those of ordinary skill in the art to understand the present invention and thereby design various embodiments with various modifications suitable for particular uses.
Claims
1. A method for treating nickel-cobalt sulfide, characterized in that: include: The method uses nickel cobalt sulfide, an intermediate product of laterite nickel ore hydrometallurgy, as a raw material, adds an oxidant and a catalyst for selective oxidation leaching, wherein the selective oxidation leaching is pressurized oxidation leaching, the temperature is controlled to be 100° C. to 200° C., the pH is 2.5 to 5.5, the oxidation leaching time is 1 hour to 24 hours, the liquid-solid ratio is (2 to 8): 1, the oxygen partial pressure is 3 bar to 5 bar, and a neutralizer is added for preliminary impurity removal, and the endpoint pH is controlled to be 4.5 to 5.5, and a nickel-containing solution and an impurity-containing filter residue are obtained by filtration; wherein the oxidant is one of oxygen, compressed air, and oxygen-enriched air; the catalyst is selected from one or more sulfur-containing compounds; and the neutralizer is alkaline; The nickel-containing solution is extracted and impurities are removed to obtain a nickel sulfate solution, which is then evaporated and crystallized to obtain nickel sulfate; the loaded organic phase is reversely extracted, the organic phase is returned to the extraction and impurity removal step, and the impurity sulfate solution is returned to the selective oxidation leaching step.
2. The method for treating nickel-cobalt sulfide according to claim 1, characterized in that: The catalyst is one or more of sulfur dioxide or flue gas containing sulfur dioxide, sodium sulfite, sodium pyrosulfite, ferrous sulfate, ferrous sulfide, sodium bisulfite, ammonium sulfite, ammonium bisulfite, sodium thiosulfate, calcium sulfite, and sulfur.
3. The method for treating nickel-cobalt sulfide according to claim 1, characterized in that: The added amount of the catalyst is 1% to 25% of the dry weight of the raw material.
4. The method for treating nickel-cobalt sulfide according to claim 1, characterized in that: The neutralizing agent is one or more selected from sodium carbonate, sodium hydroxide, calcium hydroxide, ammonia water, calcium oxide, potassium hydroxide, magnesium oxide, magnesium carbonate, magnesium hydroxide, calcium carbonate, nickel hydroxide, nickel oxide, cobalt oxide, cobalt hydroxide, nickel cobalt hydroxide, manganese hydroxide, nickel carbonate, cobalt carbonate, and manganese carbonate.
5. The method for treating nickel-cobalt sulfide according to claim 1, characterized in that: In the extraction and impurity removal process, the extraction organic phase is p204, and the O / A ratio is 1:
1.
6. The method for treating nickel-cobalt sulfide according to claim 1, characterized in that: After the preliminary impurity removal, the nickel leaching rate is not less than 99.9%, the cobalt precipitation rate is not less than 99.9%, and the manganese precipitation rate is not less than 99.9%.
7. The method for treating nickel-cobalt sulfide according to claim 1, characterized in that: In the nickel sulfate solution obtained after the extraction and impurity removal, the cobalt content is less than 5ppm, the manganese content is less than 10ppm, and the total content of other impurities is less than 10ppm.
Citation Information
Patent Citations
Production method of battery grade nickel sulfate
CN109110826A
Laterite nickel ore treatment method
CN109234526A
Method for producing nickel sulfate with high-iron low-nickel sulfonium as raw material
CN109824096A
Method for selectively extracting cobalt and nickel from nickel sulfide concentrate
CN113388743A
Method for preparing nickel sulfate from nickel sulfide concentrate lixivium
CN113416855A