A processing method for high magnesium aluminum alloy plate for welding container

Through the integrated treatment of uniform heating and semi-continuous water-cooling casting method, combined with temperature-controlled rolling technology, the problem of long processing time of high magnesium aluminum alloy plates for welding vessels has been solved, rapid and uniform heating and rolling have been achieved, and the strength of the plates has been improved. Mechanical properties and flaw detection level reduce production costs.

CN116043076BActive Publication Date: 2024-10-25NORTHEAST LIGHT ALLOY CO LTD
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
CN202211689146.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-10-25
Estimated Expiration
2042-12-27
Patent Text Reader

Abstract

A processing method for a high-magnesium aluminum alloy plate for a welding container belongs to the technical field of metal materials. It solves the problem that the homogenization treatment and heating process of the existing high-magnesium alloy for welding containers are complicated and the processing time is long. Method: weigh the raw materials according to the mass percentage of the designed elements, and obtain the aluminum alloy solution after smelting; cast the aluminum alloy solution into an aluminum alloy ingot by a semi-continuous water-cooled casting method, perform a uniform heating integrated treatment after milling and sawing, and perform rolling, temperature-controlled rolling and precision sawing in sequence to obtain a high-magnesium aluminum alloy plate for welding containers. The process of the present invention is simple, the production cycle is short, the production capacity is saved, and the cost is reduced. The plate flaw detection result can be greatly improved, and it has a better safety level for welding containers, maritime and other fields. Taking GB / T 6519-2013 as the detection standard, the flaw detection results are all above grade A, and some can reach grade AA or AAA. The present invention is suitable for processing high-magnesium aluminum alloy plates for welding containers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal materials, and in particular relates to a processing method of a high-magnesium aluminum alloy plate for a welding container. Background Art

[0002] High magnesium aluminum alloy (Al-Mg alloy) for welding containers is a non-heat-treatable strengthening alloy. It is an aluminum alloy structural material with good comprehensive performance that is widely used in China. It is widely used in welding containers, maritime, automobile, subway and light rail manufacturing and other material fields because of its low density, high strength, excellent corrosion resistance, good weldability and excellent machinability. The main states of high magnesium aluminum alloy are O, F and H112 states, which are mainly used to manufacture welded structural parts, cold die forging parts, welded container stress parts, aircraft skin skeleton parts and other parts. High magnesium aluminum alloy sheet for welding containers needs to be homogenized annealed and ingot heated before rolling. The purpose of homogenization annealing is to make the unbalanced eutectic structure in the ingot uniformly distributed in the matrix, and the supersaturated solid solution elements are precipitated from the solid solution to achieve the purpose of eliminating casting stress, improving the plasticity of the ingot, reducing deformation resistance, and improving the structure and performance of the processed products; the purpose of ingot heating is to reduce the metal deformation resistance and improve the alloy plasticity for subsequent production and processing. Summary of the invention

[0003] The purpose of the present invention is to solve the problems of complicated homogenization and heating process and long processing time of high-magnesium alloy for welding containers, and to provide a processing method of high-magnesium aluminum alloy plate for welding containers.

[0004] A method for processing a high-magnesium aluminum alloy plate for a welded container, which is carried out according to the following steps:

[0005] 1. According to the mass percentage of elements, Si: 0% to 0.4%, Fe: 0% to 0.35%, Cu: 0% to 0.1%, Mn: 0.50% to 0.80%, Mg: 5.80% to 6.80%, Cr: 0.05% to 0.15%, Zn: 0% to 0.20%, Ti: 0.02% to 0.10%, Be: 0.0001% to 0.005% and the balance is Al; respectively weigh an aluminum-manganese master alloy, an aluminum-chromium master alloy, an aluminum-titanium master alloy, anode magnesium and an aluminum ingot as raw materials, place the weighed raw materials in a dry smelting furnace for smelting, and obtain an aluminum alloy solution;

[0006] 2. The aluminum alloy solution is cast into an aluminum alloy square ingot by a semi-continuous water-cooling casting method, and after milling and sawing, it is placed in a push-type ingot heating furnace for uniform heating and integrated treatment to obtain a uniform heating and integrated aluminum alloy ingot that can be directly rolled;

[0007] 3. The above-mentioned directly rollable uniformly heated integrated aluminum alloy ingot is rolled to obtain a hot-rolled long plate, which is then temperature-controlled rolled to obtain a prefabricated plate. After precision sawing, a high-magnesium aluminum alloy plate for a welding container is obtained, thereby completing the processing method.

[0008] Furthermore, the smelting in step 1 is: smelting at 700° C. to 750° C. for 5 h to 6 h.

[0009] Furthermore, the process of the semi-continuous water-cooled casting method described in step 2 is: using a 30PPi+50PPi two-stage filtration device and a bipolar degassing device, the casting temperature is 690°C~720°C, the casting speed is 50mm / min, the liquid level height is 90mm, and the water flow rate is 120T / h.

[0010] Furthermore, the aluminum alloy ingot in step 2 has a thickness of 420 mm and a width of 1780 mm.

[0011] Furthermore, the process of integrated equalizing heating treatment described in step 2 is as follows: four N-type or K-type galvanic couples are arranged in the push-type ingot heating furnace to measure the metal temperature, and the heating temperature is set to 560°C. When one of the four galvanic couples measures the maximum metal temperature of 470°C, the heating temperature is set to 475°C. When one of the four galvanic couples measures the minimum metal temperature of 470°C, the furnace is kept warm for 41 hours, and then the furnace is stopped for cooling. When the maximum metal temperature measured by one of the four galvanic couples drops to below 470°C, an aluminum alloy ingot with integrated equalizing heating that can be directly rolled is obtained.

[0012] Furthermore, in step three, the rolling temperature is 430° C. to 470° C., the maximum processing deformation is controlled to be 35% to 43%, the plate is rolled to 70% to 81% of the finished product thickness, and a thickness margin of 15% to 23% is retained.

[0013] Furthermore, the temperature-controlled rolling described in step three: use the hot rolling mill emulsion to spray cool the hot-rolled long plate, control the temperature of the hot-rolled long plate to 150°C ~ 210°C, continue rolling, complete the rolling of the retained thickness margin, and reserve a 100mm margin according to the finished product size length.

[0014] The processing method of the high-magnesium aluminum alloy plate for welding containers in the present invention has a simple process. During the ingot homogenization treatment and ingot heating, the two-step process is shortened to a one-step process by adopting an integrated method of equalizing heating. The production process takes about 58 hours, which saves 22 hours compared with the existing process, and obtains the same mechanical properties as normal equalizing and hot-rolled plates, greatly speeds up metal circulation, greatly shortens the production cycle, saves manufacturing capacity, and reduces production costs.

[0015] The high-magnesium aluminum alloy plate for welding containers prepared in the present invention has increased Cr and Be element control compared to the plate prepared by the original method. The Cr element can improve the strength of the weld and reduce the tendency of welding hot cracking. The Be element can improve the formability of the ingot and reduce the generation of oxides in the material, which can greatly improve the plate flaw detection results. It has a better safety level for applications in welding containers, maritime and other fields. The flaw detection defect level of the plate is improved. Taking GB / T 6519-2013 as the detection standard, the flaw detection results of the aluminum alloy plate prepared by the present invention are all above grade A, and some can reach grade AA or AAA, while the flaw detection results of the plate obtained by the original preparation method are basically below grade B.

[0016] The invention is suitable for processing high-magnesium aluminum alloy plates for welding containers. DETAILED DESCRIPTION

[0017] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0018] Specific implementation method 1: This implementation method is a processing method for a high-magnesium aluminum alloy plate for a welded container, which is carried out in the following steps:

[0019] 1. According to the mass percentage of elements, Si: 0% to 0.4%, Fe: 0% to 0.35%, Cu: 0% to 0.1%, Mn: 0.50% to 0.80%, Mg: 5.80% to 6.80%, Cr: 0.05% to 0.15%, Zn: 0% to 0.20%, Ti: 0.02% to 0.10%, Be: 0.0001% to 0.005% and the balance is Al; respectively weigh an aluminum-manganese master alloy, an aluminum-chromium master alloy, an aluminum-titanium master alloy, anode magnesium and an aluminum ingot as raw materials, place the weighed raw materials in a dry smelting furnace for smelting, and obtain an aluminum alloy solution;

[0020] 2. The aluminum alloy solution is cast into an aluminum alloy square ingot by a semi-continuous water-cooling casting method, and after milling and sawing, it is placed in a push-type ingot heating furnace for uniform heating and integrated treatment to obtain a uniform heating and integrated aluminum alloy ingot that can be directly rolled;

[0021] 3. The above-mentioned directly rollable uniformly heated integrated aluminum alloy ingot is rolled to obtain a hot-rolled long plate, which is then temperature-controlled rolled to obtain a prefabricated plate. After precision sawing, a high-magnesium aluminum alloy plate for a welding container is obtained, thereby completing the processing method.

[0022] In the high-magnesium aluminum alloy plate for welding containers in the present embodiment, a single impurity is ≤0.05%, and all impurities should be less than 0.10%. Impurities within this range have no effect on the performance of the plate.

[0023] Specific embodiment 2: This embodiment is different from specific embodiment 1 in that the mass percentages of the elements in step 1 are Si: 0.1%, Cu: 0.05%, Mn: 0.60%, Mg: 5.90%, Cr: 0.08%, Zn: 0.05%, Ti: 0.05%, Be: 0.0001% and the balance is Al. The rest is the same as specific embodiment 1.

[0024] Specific embodiment 3: This embodiment is different from specific embodiment 1 in that the mass percentages of the elements in step 1 are Si: 0.25%, Fe: 0.2%, Cu: 0.05%, Mn: 0.65%, Mg: 6.5%, Cr: 0.1%, Zn: 0.1%, Ti: 0.06%, Be: 0.002% and the balance is Al. The other steps and parameters are the same as those in specific embodiment 1.

[0025] Specific embodiment 4: This embodiment differs from specific embodiment 1 in that the smelting in step 1 is: smelting at 700° C. to 750° C. for 5 h to 6 h. Other steps and parameters are the same as those in specific embodiment 1.

[0026] Specific embodiment 5: This embodiment is different from specific embodiment 4 in that the smelting in step 1 is carried out at 740° C. for 5.5 h. The other steps and parameters are the same as those in specific embodiment 4.

[0027] Specific embodiment 6: This embodiment is different from the specific embodiment 1 in that the process of the semi-continuous water-cooled casting method described in step 2 is: using a 30PPi+50PPi double-stage filtration device and a bipolar degassing device, a casting temperature of 690°C to 720°C, a casting speed of 50mm / min, a liquid level of 90mm, and a water flow rate of 120T / h. Other steps and parameters are the same as those of the specific embodiment 1.

[0028] Specific implementation example 7: This implementation example is similar to the specific implementation example in that the thickness of the aluminum alloy ingot in step 2 is 420 mm and the width is 1780 mm. The other steps and parameters are the same as those in the specific implementation example 1.

[0029] Specific embodiment eight: This embodiment is the same as the specific embodiment in that the process of the integrated treatment of equalizing heating in step two is as follows: 4 N-type or K-type galvanic couples are arranged in the pusher-type ingot heating furnace to measure the metal temperature, and the heating temperature is set to 560°C. When one of the 4 galvanic couples measures the highest metal temperature of 470°C, the heating temperature is set to 475°C. When one of the 4 galvanic couples measures the lowest metal temperature of 470°C, the furnace is kept warm for 41 hours, and the furnace is stopped to cool down. When one of the 4 galvanic couples measures the highest metal temperature below 470°C, an aluminum alloy ingot with equalizing heating integrated that can be directly rolled is obtained. The other steps and parameters are the same as those in the specific embodiment one.

[0030] The integrated uniform heating process in this embodiment can be named as "uniform heating integration".

[0031] Specific embodiment 9: This embodiment is the same as the specific embodiment in that the rolling temperature in step 3 is 430°C to 470°C, the maximum processing deformation is controlled to be 35% to 43%, the plate is rolled to 70% to 81% of the finished product thickness, and a thickness margin of 15% to 23% is reserved. Other steps and parameters are the same as those in specific embodiment 1.

[0032] Specific embodiment 10: This embodiment is the same as the specific embodiment in that the temperature-controlled rolling described in step 3: the hot rolling mill emulsion is used to spray-cool the hot-rolled long plate, the temperature of the hot-rolled long plate is controlled to be 150°C to 210°C, and the rolling is continued to complete the rolling of the reserved thickness margin, and a 100mm margin is reserved according to the finished product size length. The other steps and parameters are the same as those of the specific embodiment 1.

[0033] In this embodiment, a margin of 100 mm is reserved to facilitate subsequent precision sawing.

[0034] The beneficial effects of the present invention are verified by the following examples:

[0035] Example:

[0036] A method for processing a high-magnesium aluminum alloy plate for a welded container, which is carried out according to the following steps:

[0037] 1. According to the mass percentage of elements Si: 0.25%, Fe: 0.2%, Cu: 0.05%, Mn: 0.65%, Mg: 6.5%, Cr: 0.1%, Zn: 0.1%, Ti: 0.06%, Be: 0.002% and the balance is Al; aluminum-manganese master alloy, aluminum-chromium master alloy, aluminum-titanium master alloy, anode magnesium and aluminum ingot are weighed as raw materials respectively, and the weighed raw materials are placed in a dry melting furnace for melting to obtain an aluminum alloy solution;

[0038] 2. The aluminum alloy solution is cast into an aluminum alloy square ingot by a semi-continuous water-cooling casting method, and after milling and sawing, it is placed in a push-type ingot heating furnace for uniform heating and integrated treatment to obtain a uniform heating and integrated aluminum alloy ingot that can be directly rolled;

[0039] 3. The above-mentioned directly rollable uniformly heated integrated aluminum alloy ingot is rolled to obtain a hot-rolled long plate, which is then temperature-controlled rolled to obtain a prefabricated plate. After precision sawing, a high-magnesium aluminum alloy plate for a welding container is obtained, thereby completing the processing method.

[0040] The smelting described in step 1 of this embodiment is: smelting at 750° C. for 5 hours.

[0041] The process of the semi-continuous water-cooled casting method described in step 2 of this embodiment is: using a 30PPi+50PPi two-stage filtration device and a bipolar degassing device, a casting temperature of 710°C, a casting speed of 50mm / min, a liquid level of 90mm, and a water flow rate of 120T / h.

[0042] The aluminum alloy ingot described in step 2 of this embodiment has a thickness of 420 mm and a width of 1780 mm.

[0043] The process of integrated equalizing heating treatment described in step 2 of this embodiment is as follows: four N-type galvanic couples are arranged in the push-type ingot heating furnace to measure the metal temperature, and the heating temperature is set to 560°C. When one of the four galvanic couples measures the maximum metal temperature of 470°C, the heating temperature is set to 475°C. When one of the four galvanic couples measures the minimum metal temperature of 470°C, the furnace is kept warm for 41 hours, and then the furnace is stopped for cooling. When the maximum metal temperature measured by one of the four galvanic couples drops to below 470°C, an aluminum alloy ingot with integrated equalizing heating that can be directly rolled is obtained.

[0044] In step three of this embodiment, the rolling temperature is 450° C., the maximum processing deformation is controlled to be 40%, the plate is rolled to 75% of the finished product thickness, and a 20% thickness margin is retained.

[0045] The temperature-controlled rolling described in step three of this embodiment is: use the hot rolling mill emulsion to spray cool the hot-rolled long plate, control the temperature of the hot-rolled long plate to 200°C, continue rolling, complete the rolling of the retained thickness margin, and reserve a 100mm margin according to the finished product size length.

[0046] The high magnesium aluminum alloy plate for welded container prepared in this embodiment has a flaw detection result of AAA grade according to GB / T 6519-2013 as the testing standard, while the flaw detection result of the plate obtained by the original preparation method is basically below grade B.

[0047] The high-magnesium aluminum alloy plate material of the welded container prepared in this embodiment was tested, and its tensile strength was 351 MPa, the yield strength was 177 MPa, and the elongation was 22.6%.

Claims

1. A method for processing high magnesium aluminum alloy sheet for welding container, characterized in that It proceeds as follows:

1. According to the mass percentage of elements, Si: 0% to 0.4%, Fe: 0% to 0.35%, Cu: 0% to 0.1%, Mn: 0.50% to 0.80%, Mg: 5.80% to 6.80%, Cr: 0.05% to 0.15%, Zn: 0% to 0.20%, Ti: 0.02% to 0.10%, Be: 0.0001% to 0.005% and the balance is Al; respectively weighing an aluminum-manganese master alloy, an aluminum-chromium master alloy, an aluminum-titanium master alloy, anode magnesium and an aluminum ingot as raw materials, placing the weighed raw materials in a dry melting furnace for melting to obtain an aluminum alloy solution; Second, the aluminum alloy solution is cast into an aluminum alloy ingot by a semi-continuous water-cooling casting method, and after milling and sawing, the ingot is placed in a pusher-type ingot heating furnace for uniform heating and integrated treatment to obtain a uniform heating and integrated aluminum alloy ingot that can be directly rolled; 3. The above-mentioned directly rollable, soaking-heated integrated aluminum alloy ingot is rolled to obtain a hot-rolled long plate, which is then temperature-controlled rolled to obtain a prefabricated plate. After precision sawing, a high-magnesium aluminum alloy plate for a welded container is obtained, thereby completing the processing method; Melting in step 1: melting at 700°C to 750°C for 5h to 6h; The semi-continuous water-cooled casting process in step 2 is as follows: a 30PPi+50PPi double-stage filtration device and a bipolar degassing device are used, the casting temperature is 690°C to 720°C, the casting speed is 50mm / min, the liquid level is 90mm, and the water flow rate is 120T / h; The thickness of the aluminum alloy ingot in step 2 is 420 mm and the width is 1780 mm; The process of the integrated equalizing heating treatment in step 2 is as follows: 4 N-type or K-type galvanic couples are arranged in the pusher-type ingot heating furnace to measure the metal temperature, and the heating temperature is set to 560°C. When one of the four galvanic couples measures the maximum metal temperature of 470°C, the heating temperature is set to 475°C. When one of the four galvanic couples measures the minimum metal temperature of 470°C, the furnace is kept warm for 41 hours, and then the furnace is stopped and cooled. When the maximum metal temperature measured by one of the four galvanic couples drops below 470°C, an aluminum alloy ingot with integrated equalizing heating that can be directly rolled is obtained. The rolling temperature in step 3 is 430° C. to 470° C., the maximum processing deformation is controlled at 35% to 43%, and the plate is rolled to 70% to 81% of the finished product thickness, with a thickness margin of 15% to 23% remaining; The temperature-controlled rolling described in step three: use the hot rolling mill emulsion to spray cool the hot-rolled long plate, control the temperature of the hot-rolled long plate to 150°C ~ 210°C, continue rolling, complete the remaining thickness margin, and reserve a margin of 100mm according to the finished product size length.

2. The method for processing a high-magnesium aluminum alloy sheet for a welded container according to claim 1, characterized in that The mass percentages of the elements in step 1 are Si: 0.1%, Cu: 0.05%, Mn: 0.60%, Mg: 5.90%, Cr: 0.08%, Zn: 0.05%, Ti: 0.05%, Be: 0.0001% and the balance is Al.

3. The method for processing a high-magnesium aluminum alloy sheet for a welded container according to claim 1, characterized in that The mass percentages of the elements in step 1 are Si: 0.25%, Fe: 0.2%, Cu: 0.05%, Mn: 0.65%, Mg: 6.5%, Cr: 0.1%, Zn: 0.1%, Ti: 0.06%, Be: 0.002% and the balance is Al.

4. The method for processing a high-magnesium aluminum alloy sheet for a welded container according to claim 1, characterized in that Melting as described in step 1: Melting at 740°C for 5.5h.

Citation Information

Patent Citations

  • Production process of aluminum alloy hot rolling medium plate

    CN101538668A

  • 5A06H14 sheet metal with thickness of 8.5mm, and preparation method thereof

    CN102899541A

  • Method for preparing alumium alloy plate for automobiles

    CN103194700A

  • Method for producing high-magnesium aluminum alloy sheets

    CN104233129A

  • Preparation process of medium-strength anti-corrosion high-magnesium aluminum alloy plate

    CN104357690A