A quaternary amine anion exchange resin coated fabric and preparation method thereof and application thereof in regulating carbon dioxide in air

By quaternary amine-type anion exchange resin-coated fabrics regulate the adsorption and desorption of carbon dioxide in the air, the problems of high energy consumption and low efficiency in air carbon dioxide capture technology are solved, and efficient and environmentally friendly carbon dioxide capture effect are achieved.

CN116043566BActive Publication Date: 2024-11-01SUZHOU UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310009733.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-04
Publication Date
2024-11-01
Estimated Expiration
2043-01-04

AI Technical Summary

Technical Problem

The existing air carbon dioxide capture technology has problems such as high energy consumption, high investment cost and low adsorption efficiency, especially when it is difficult to achieve efficient adsorption and desorption under normal temperature and pressure.

Method used

Using quaternary amine type anion exchange resin coated fabric, the loaded quaternary amine type anion exchange resin is contacted with different partial pressures of water vapor by adjusting the environmental dry and humidity and the drying/wetting method of the coated fabric, thereby achieving efficient carbon dioxide adsorption. and desorption.

Benefits of technology

It improves carbon dioxide adsorption efficiency and adsorption capacity, reduces regeneration energy consumption and capture costs, and the materials are environmentally friendly and circulating, suitable for large-scale carbon dioxide capture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116043566B_ABST
    Figure CN116043566B_ABST
Patent Text Reader

Abstract

The present invention relates to a quaternary amine anion exchange resin coated fabric, a preparation method and its application in regulating carbon dioxide in the air, and belongs to the technical field of carbon dioxide emission reduction. The present invention uses environmentally friendly coating technology to embed quaternary amine anion exchange resin to prepare a coated fabric with carbon fixation function, and by adjusting the environmental humidity and drying / wetting the coated fabric, the loaded quaternary amine anion exchange resin is exposed to different water vapor partial pressures to adsorb / desorb CO2, thereby achieving the purpose of regulating CO2 in the environment. Compared with traditional methods, the present invention is more accurate and efficient, and also solves the problems of large regeneration energy consumption, high capture cost, low adsorption efficiency, etc. of conventional adsorption materials, and can be applied to large-scale carbon dioxide capture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of carbon dioxide emission reduction, and in particular to a quaternary amine type anion exchange resin coated fabric, a preparation method and application thereof in regulating carbon dioxide in the air. Background Art

[0002] Since the 21st century, with the rapid economic growth of countries around the world, the huge energy consumption of human society has caused a large amount of CO2 to be discharged into the atmosphere. The current concentration of carbon dioxide in the air has exceeded 400ppm. In order to cope with the harm caused by large amounts of CO2 emissions to nature and human development, major economies have proposed the goals of "carbon reduction" and "carbon neutrality". The traditional pre-combustion and post-combustion carbon capture modes of capturing CO2 from large point sources are currently the main carbon fixation and emission reduction strategies, which help to slow down the increase in CO2 concentration in the atmosphere. However, to reduce the concentration of CO2 in the air, CO2 can only be directly removed from the air or directly captured by air (Direct Air Capture, DAC). The current methods for capturing carbon dioxide in the air mainly include physical adsorption technology, chemical absorption technology, and membrane separation technology. However, these methods all use temperature and pressure changes to achieve material regeneration, which have problems such as severe reaction conditions, high regeneration costs, large energy losses, and large losses of adsorption materials. DAC also faces huge challenges of high energy consumption and high investment and operating costs. Therefore, it is urgent to develop new DAC technologies.

[0003] In recent years, researchers have found that the use of quaternary amine polymer materials ionic functional groups ((CH3)4N +) has hydrophilicity and strong alkalinity. By adjusting the partial pressure of water vapor in the environment, the chemical adsorption capacity of the interface for CO2 can be controlled to achieve the purpose of adsorption / desorption, that is, variable humidity adsorption. Since this process is completed at room temperature and pressure, it is more suitable for DAC than the method that relies on temperature and pressure desorption. So far, a variety of quaternary amino ion exchange resins have been used as materials for variable humidity adsorption of CO2 for this study. Patent CN104475055A discloses a preparation method and product of an ultra-low concentration carbon dioxide adsorption membrane material, wherein a quaternary ammonium anion exchange resin is mixed with an organic solvent, polyethylene glycol, polyether sulfone, etc. are added to form a mixed suspension, and the mixed suspension is then coated on a substrate, and the initial membrane material is separated to obtain the initial membrane material. The membrane material can be used to capture low-concentration CO2. However, after the membrane material is hot-pressed, the resin particles are very tightly combined with the inert matrix, and there is no obvious pore structure, which is not conducive to the circulation of gas. The adsorption material has the problems of high water consumption and reduced adsorption efficiency. Patent CN113786818A discloses a resin-type adsorbent and preparation method for directly capturing carbon dioxide in the air. The quaternary amino resin is ground and added to an organic solution, heated and stirred into a gel state, and finally the solvent evaporates and solidifies to form spherical resin adsorption particles. The method is simple, but the volatilization of the organic solvent causes certain pollution to the environment. The particle size of the adsorption beads after solidification is large, and there is also the problem of low adsorption efficiency. In view of this, how to combine new materials and new processes to propose new research ideas is the key to achieving the rapid development of adsorption air CO2 capture technology. Summary of the invention

[0004] In order to solve the above technical problems, the present invention provides a quaternary amine anion exchange resin coated fabric and a preparation method and its application in the adsorption or desorption of carbon dioxide. It uses environmentally friendly coating technology to embed quaternary amine anion exchange resin to prepare a coated fabric with carbon fixation function. By adjusting the environmental humidity and drying / wetting the coated fabric, the loaded quaternary amine anion exchange resin is exposed to different water vapor partial pressures to adsorb / desorb CO2, thereby achieving the purpose of regulating CO2 in the environment. Compared with traditional methods, this will be more accurate and efficient, and also solve the problems of high regeneration energy consumption, high capture cost, and low adsorption efficiency of conventional adsorption materials, and can be applied to large-scale carbon dioxide capture.

[0005] The present invention is achieved through the following technical solutions:

[0006] The first object of the present invention is to provide a quaternary amine anion exchange resin coated fabric, which comprises a coating liquid containing a quaternary amine anion exchange resin and a fabric; the quaternary amine anion exchange resin is dispersed in the fiber gaps of the fabric.

[0007] In one embodiment of the present invention, the coating liquid containing quaternary amine anion exchange resin is prepared by the following method:

[0008] The silk fibroin solution and the organic solvent are mixed to obtain a mixed solution; the pretreated quaternary ammonium anion exchange resin is added to the mixed solution and stirred to obtain a coating solution containing the quaternary ammonium anion exchange resin.

[0009] In one embodiment of the present invention, the silk fibroin solution is prepared by the following method:

[0010] S1. dissolving an alkaline reagent in boiling water, adding raw silk, and continuing to boil, stir, and knead the raw silk so that the sericin on the surface of the raw silk is fully removed, and then drying to obtain dried silk;

[0011] S2. The dried silk obtained in S1 is dissolved in a lithium bromide solution, dialyzed, and centrifuged to obtain the silk fibroin solution.

[0012] In one embodiment of the present invention, the organic solvent is selected from one or more of glycerol, PEG and ethanol.

[0013] In one embodiment of the present invention, the mass concentration of the silk fibroin solution is 1%-6%.

[0014] In one embodiment of the present invention, the mass ratio of the silk fibroin solution to the organic solvent is 20:1-3:1; the mass ratio of the treated quaternary ammonium anion exchange resin to the mixed solution is 1:40-1:5.

[0015] In one embodiment of the present invention, the pretreated quaternary amine anion exchange resin is prepared by the following method:

[0016] The quaternary ammonium anion exchange resin is ground to an average particle size of ≤30 μm, then alkali washed and dried to obtain the pretreated quaternary ammonium anion exchange resin.

[0017] In one embodiment of the present invention, the fabric is selected from one or more of cotton fabric, polyester fabric and polyester-cotton blended fabric.

[0018] The second object of the present invention is to provide the use of the quaternary amine anion exchange resin coated fabric in the regulation of carbon dioxide in the air.

[0019] In one embodiment of the present invention, the carbon dioxide regulation is carried out under the condition of humidity of 10%-99%.

[0020] In one embodiment of the present invention, the adsorption of CO2 in the carbon dioxide regulation is carried out under the condition of humidity of 10%-70%.

[0021] In one embodiment of the present invention, desorption of CO2 in the carbon dioxide regulation is carried out under a humidity of 70%-99% or soaking condition.

[0022] The third object of the present invention is to provide a method for preparing a quaternary amine type anion exchange resin coated fabric, which specifically comprises the following steps:

[0023] The coating liquid containing quaternary amine anion exchange resin is coated on the fabric after alkali treatment, and the quaternary amine anion exchange resin coated fabric is obtained by impregnation, pressing and drying.

[0024] Mechanism of the present invention:

[0025] (1) The adsorbent used in the present invention is a macroporous strongly alkaline anion exchange resin, which is washed with a Na2CO3 solution to perform ion exchange, and the Cl in the resin is removed. - Converted into CO3 2- Only anion exchange resins of this type have the ability to absorb CO2. The original resin is in a non-porous smooth spherical shape in an absolutely dry state, and it is difficult for CO2 to continue to diffuse into the interior after being adsorbed on the outer surface. The reduced particle size of the resin particles after grinding and crushing and the fully exposed inner surface of the particles can significantly increase the specific surface area of ​​the material.

[0026] (2) Organic solvents such as glycerol, PEG, and ethanol are added to the silk fibroin solution to make it gel. The polarity of the organic solvent can destroy the hydrogen bonds and electrostatic binding effects within the silk fibroin molecular chain, allowing the molecular chain to stretch while forming hydrophobic macromolecular segments with a β-folded structure. The segments are adjusted and rearranged to form a three-dimensional network structure to form a hydrogel. The gel can be used to bond the resin well and coat it on the fabric. Furthermore, silk fibroin is rich in serine and alanine and has a high CO2 affinity, which can further promote the adsorption of carbon dioxide by the coated fabric.

[0027] The technical solution of the present invention has the following advantages:

[0028] (1) The present invention breaks with previous research ideas. By changing the ambient humidity or wetting / drying the coated fabric, the loaded quaternary ammonium anion exchange resin particles are exposed to different water vapor partial pressures, thereby achieving the effect of regulating CO2 adsorption / desorption. This is more accurate and efficient than traditional methods.

[0029] (2) The present invention changes the partial pressure of water vapor that the loaded quaternary amine groups are exposed to by the hydrophilicity and hydrophobicity of the fabric. No additional heat source or power source is required, and the adsorption / desorption of the material can be achieved at room temperature and pressure. Compared with conventional adsorption methods such as temperature and pressure changes, this method solves the problems of high capture cost and high regeneration energy consumption, and provides a new strategy and technology for carbon fixation.

[0030] (3) The present invention increases the adsorption area by uniformly dispersing the quaternary amine anion exchange resin between the pores of the fibers. Compared with the original resin particles, the adsorption efficiency and adsorption capacity of the adsorbent for carbon dioxide are effectively improved.

[0031] (4) The silk protein coating liquid used in the present invention is a biodegradable, green and environmentally friendly material, and may also be a green reagent such as chitosan and sodium alginate; the coated fabric can be recycled multiple times, meeting the requirements of a low-carbon and environmentally friendly new energy system.

[0032] (5) The preparation process of the present invention is simple and has high feasibility. It has broad application prospects, and its coated fabric can be used for clothing, indoor curtains, tablecloths, car awnings, etc. The adsorption / desorption of CO2 can be cycled by wetting and drying. For example, it can adsorb carbon dioxide in a dry state during the day, spray it at night, and adsorb it again after drying the next day.

[0033] (6) The present invention can realize the recycling of resources. The coated fabric can be combined with biological utilization technology to use the desorbed carbon dioxide for biological photosynthesis. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:

[0035] Figure 1 is a diagram of fabrics coated with different particle sizes in Example 1 of the present invention;

[0036] Figure 2 is a SEM image of the original fabric and the quaternary amine type anion exchange resin cotton fabric coating in Example 2 of the present invention;

[0037] Figure 3 is the contact angle of the polyester coating, polyester-cotton blended coating and cotton fabric coating in Test Example 1 of the present invention;

[0038] Figure 4 is a graph showing the adsorption test results of different fabric coatings in Test Example 2 of the present invention;

[0039] Figure 5 is a test graph of air permeability of silk protein polyester coated fabrics with different concentrations in Test Example 3 of the present invention;

[0040] Figure 6 This is a test diagram of the adsorption performance of silk protein polyester coated fabrics with different concentrations in Test Example 4 of the present invention;

[0041] Figure 7 is an adsorption diagram of the polyester coated fabric in Test Example 5 of the present invention under different humidity conditions;

[0042] Figure 8-Ais a graph showing the desorption test results by adjusting the humidity in Test Example 3 of the present invention;

[0043] Figure 8-B is a graph showing the desorption test results of the coated fabric by wetting in Test Example 3 of the present invention;

[0044] Fig. 9 4 is a graph showing the test results of the regeneration adsorption efficiency of the coated fabric in Test Example 4 of the present invention. DETAILED DESCRIPTION

[0045] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.

[0046] Example 1

[0047] Pretreatment of quaternary amine anion exchange resin

[0048] Soak D290 resin in deionized water at 90°C for 4h-8h, dry the treated sample in an oven above 60°C, then grind the resin and sieve it into particles of two different sizes: 30μm<d≤500μm and d≤30μm, wash the ground resin particles with Na2CO3 solution, rinse the sample with deionized water after each washing; collect the solution and washing liquid and titrate with silver nitrate until the titration method detects that there is no chlorine in the solution, dry it, and obtain the pretreated quaternary ammonium anion exchange resin.

[0049] (2) Preparation of silk fibroin solution

[0050] Use an analytical balance to weigh 30g of raw silk and 25.44g of anhydrous sodium carbonate for use, measure 12L of deionized water and pour it into a steel barrel, and heat it with an induction cooker. When the deionized water is about to boil, add the weighed anhydrous sodium carbonate, continue to heat it to boiling so that the anhydrous sodium carbonate is fully dissolved, then add 30g of raw silk and cook for 40min, stirring every 10min to dissolve the sericin on the surface of the raw silk. Rub the degummed raw silk with deionized water for 3 times to fully remove the sericin on the surface of the raw silk, and finally place it in a fume hood to dry overnight. The next day, weigh 25g of dry silk and dissolve it in 100mL, 9.3mol / L lithium bromide solution, and place it in a 60℃ oven. During this period, stir once an hour to allow the cooked silk to be fully dissolved. After 4h, take the dissolved silk solution out of the oven, cool it to room temperature, pour it into a dialysis bag, dialyze it with deionized water for 40h, and change the deionized water every 5h. The dialyzed silk solution was centrifuged twice using a high-speed centrifuge (9000rpm, 20min) to remove impurities for later use. The concentration of the purified silk fibroin solution was measured by the following method: the mass of the dry culture dish was weighed and recorded as W0 (g). Then 1mL of silk fibroin solution was dripped into the culture dish and weighed to obtain the mass W1 (g). The culture dish containing the silk fibroin solution was placed in an oven for drying and then taken out and weighed to obtain the mass W2 (g). The concentration (C) of the silk fibroin solution was calculated according to the following formula:

[0051] Concentration (%) = [(W2-W0) / (W1-W0)] × 100

[0052] (3) Fabric pretreatment

[0053] The cotton fabric was soaked in 10% NaOH solution for 1 hour, and the treated fabric was soaked in deionized water to remove excess alkali solution, and then dried for storage.

[0054] (4) Preparation of coating liquid

[0055] After 2% silk fibroin solution and PEG-400 were mixed in a ratio of 3:1, the resin powders of different particle sizes treated in (1) were added to the mixed solution (their mass ratio was 1:40) and stirred by magnetic force for 10 hours to make them mixed evenly.

[0056] (5) Preparation of coated fabrics

[0057] The coating liquid prepared in (4) was poured onto the cotton fabric, pressed back and forth with a glass rod, and dried in an oven at 60°C to obtain cotton fabrics coated with quaternary ammonium anion exchange resins of different particle sizes. Figure 1 shown.

[0058] Table 1 Resin coated cotton fabric

[0059]

[0060] Example 2

[0061] (1) Pretreatment of quaternary amine anion exchange resin

[0062] Soak D290 resin in deionized water at 90°C for 4h-8h, dry the treated sample in an oven above 60°C, grind and sieve into particles with an average particle size of ≤30μm, and alkaline wash the ground resin particles with Na2CO3 solution. Rinse the sample with deionized water after each washing. Collect the solution and washing liquid and titrate with silver nitrate until the titration method detects that there is no chlorine in the solution, dry it, and obtain the pretreated quaternary ammonium anion exchange resin.

[0063] (2) Preparation of silk fibroin solution

[0064] Use an analytical balance to weigh 30g of raw silk and 25.44g of anhydrous sodium carbonate for use, measure 12L of deionized water and pour it into a steel barrel, and heat it with an induction cooker. When the deionized water is about to boil, add the weighed anhydrous sodium carbonate, continue to heat it to boiling so that the anhydrous sodium carbonate is fully dissolved, then add 30g of raw silk and cook for 40min, stirring every 10min to dissolve the sericin on the surface of the raw silk. Rub the degummed raw silk with deionized water for 3 times to fully remove the sericin on the surface of the raw silk, and finally place it in a fume hood to dry overnight. The next day, weigh 25g of dry silk and dissolve it in 100mL, 9.3mol / L lithium bromide solution, and place it in a 60℃ oven. During this period, stir once an hour to allow the cooked silk to be fully dissolved. After 4h, take the dissolved silk solution out of the oven, cool it to room temperature, pour it into a dialysis bag, dialyze it with deionized water for 40h, and change the deionized water every 5h. The dialyzed silk solution was centrifuged twice using a high-speed centrifuge (9000rpm, 20min) to remove impurities for later use. The concentration of the purified silk fibroin solution was measured by the following method: the mass of the dry culture dish was weighed and recorded as W0 (g). Then 1mL of silk fibroin solution was dripped into the culture dish and weighed to obtain the mass W1 (g). The culture dish containing the silk fibroin solution was placed in an oven for drying and then taken out and weighed to obtain the mass W2 (g). The concentration (C) of the silk fibroin solution was calculated according to the following formula:

[0065] Concentration (%) = [(W2-W0) / (W1-W0)] × 100

[0066] (3) Fabric pretreatment

[0067] The cotton fabric was soaked in 10% NaOH solution for 1 hour, and the treated fabric was soaked in deionized water to remove excess alkali solution, and then dried for storage.

[0068] (4) Preparation of coating liquid

[0069] After 2% silk fibroin solution and glycerol were mixed evenly in a ratio of 3:1, the resin powder treated in (1) was added to the mixed solution (the mass ratio was 1:40), and magnetic stirring was used for 10 hours to make the mixture evenly mixed.

[0070] (5) Preparation of coated fabrics

[0071] The coating liquid prepared in (4) was poured onto the cotton fabric, pressed back and forth with a glass rod, and dried in an oven at 60° C. to obtain a quaternary amine type anion exchange resin coated cotton fabric (cotton fabric coating).

[0072] The original cotton fabric and the quaternary amine anion exchange resin coated fabric were characterized, and their SEM images are shown in Figure 2 shown by Figure 2 It can be seen that the quaternary amine anion exchange resin was successfully embedded between the fibers of the cotton fabric through the coating technology.

[0073] (6) CO2 adsorption performance test

[0074] The adsorption performance test is carried out in a dryer at room temperature and a certain humidity. After the carbon dioxide concentration in the dryer is stable, the carbon dioxide detector and the dried quaternary amine anion exchange resin coated fabric are placed in the dryer, and the dryer is sealed for adsorption test. After adsorption saturation, the humidity in the dryer is adjusted. When the relative humidity increases to 80%, the carbon dioxide adsorbed on the cotton fabric is desorbed, and the carbon dioxide concentration in the dryer rises. After drying again, the adsorption cycle is repeated.

[0075] Example 3

[0076] (1) Pretreatment of quaternary amine anion exchange resin

[0077] The D290 resin is soaked in deionized water at 90°C for 4h-8h, the treated sample is dried in an oven at 60°C, and then ground and sieved into particles of a certain size. The ground resin particles are alkaline washed with a Na2CO3 solution, and the sample is rinsed with deionized water after each washing; the solution and the washing liquid are collected and titrated with silver nitrate until the titration method detects that there is no chlorine in the solution, and then dried to obtain the pretreated quaternary ammonium anion exchange resin.

[0078] (2) Preparation of silk fibroin solution

[0079] Use an analytical balance to weigh 30g of raw silk and 25.44g of anhydrous sodium carbonate for use, measure 12L of deionized water and pour it into a steel barrel, and heat it with an induction cooker. When the deionized water is about to boil, add the weighed anhydrous sodium carbonate, continue to heat it to boiling so that the anhydrous sodium carbonate is fully dissolved, then add 30g of raw silk and cook for 40min, stirring every 10min to dissolve the sericin on the surface of the raw silk. Rub the degummed raw silk with deionized water for 3 times to fully remove the sericin on the surface of the raw silk, and finally place it in a fume hood to dry overnight. The next day, weigh 25g of dry silk and dissolve it in 100mL, 9.3mol / L lithium bromide solution, and place it in a 60℃ oven. During this period, stir once an hour to allow the cooked silk to be fully dissolved. After 4h, take the dissolved silk solution out of the oven, cool it to room temperature, pour it into a dialysis bag, dialyze it with deionized water for 40h, and change the deionized water every 5h. The dialyzed silk solution was centrifuged twice using a high-speed centrifuge (9000rpm, 20min) to remove impurities for later use. The concentration of the purified silk fibroin solution was measured by the following method: the mass of the dry culture dish was weighed and recorded as W0 (g). Then 1mL of silk fibroin solution was dripped into the culture dish and weighed to obtain the mass W1 (g). The culture dish containing the silk fibroin solution was placed in an oven for drying and then taken out and weighed to obtain the mass W2 (g). The concentration (C) of the silk fibroin solution was calculated according to the following formula:

[0080] Concentration (%) = [(W2-W0) / (W1-W0)] × 100

[0081] (3) Polyester fabric pretreatment

[0082] The polyester fabric was soaked in a 10% NaOH solution and treated in a 60°C water bath for 1 hour. The treated fabric was soaked in deionized water to remove excess alkali solution and then dried for storage.

[0083] (4) Preparation of coating liquid

[0084] After 2% silk fibroin solution and glycerol were mixed evenly in a ratio of 3:1, the resin powder treated in (1) was added to the mixed solution (the mass ratio was 1:40), and magnetic stirring was used for 10 hours to make the mixture evenly mixed.

[0085] (5) Preparation of coated fabrics

[0086] The coating liquid prepared in (4) was poured onto the fabric, pressed back and forth with a glass rod, and dried in an oven at 60° C. to obtain a quaternary amine type anion exchange resin coated polyester fabric (2% SF polyester fabric coating).

[0087] (6) CO2 adsorption performance test

[0088] The adsorption performance test was conducted in a dryer at room temperature and a relative humidity of 30%. After the carbon dioxide concentration in the dryer stabilized, the carbon dioxide detector and the dried coated fabric were placed in the dryer, and the dryer was sealed for adsorption testing. After adsorption saturation, the humidity in the dryer was adjusted. When the relative humidity increased to 85%, only part of the carbon dioxide adsorbed on the fabric was desorbed, indicating that the hydrophobicity of the polyester fabric hindered the full combination of water vapor and resin under high humidity.

[0089] Example 4

[0090] (1) Pretreatment of quaternary amine anion exchange resin

[0091] The D290 resin is soaked in deionized water at 90°C for 4h-8h, the treated sample is dried in an oven at 60°C, and then ground and sieved into particles of a certain size. The ground resin particles are alkaline washed with a Na2CO3 solution, and the sample is rinsed with deionized water after each washing; the solution and the washing liquid are collected and titrated with silver nitrate until the titration method detects that there is no chlorine in the solution, and then dried to obtain the pretreated quaternary ammonium anion exchange resin.

[0092] (2) Preparation of silk fibroin solution

[0093] Use an analytical balance to weigh 30g of raw silk and 25.44g of anhydrous sodium carbonate for use, measure 12L of deionized water and pour it into a steel barrel, and heat it with an induction cooker. When the deionized water is about to boil, add the weighed anhydrous sodium carbonate, continue to heat it to boiling so that the anhydrous sodium carbonate is fully dissolved, then add 30g of raw silk and cook for 40min, stirring every 10min to dissolve the sericin on the surface of the raw silk. Rub the degummed raw silk with deionized water for 3 times to fully remove the sericin on the surface of the raw silk, and finally place it in a fume hood to dry overnight. The next day, weigh 25g of dry silk and dissolve it in 100mL, 9.3mol / L lithium bromide solution, and place it in a 60℃ oven. During this period, stir once an hour to allow the cooked silk to be fully dissolved. After 4h, take the dissolved silk solution out of the oven, cool it to room temperature, pour it into a dialysis bag, dialyze it with deionized water for 40h, and change the deionized water every 5h. The dialyzed silk solution was centrifuged twice using a high-speed centrifuge (9000rpm, 20min) to remove impurities for later use. The concentration of the purified silk fibroin solution was measured by the following method: the mass of the dry culture dish was weighed and recorded as W0 (g). Then 1mL of silk fibroin solution was dripped into the culture dish and weighed to obtain the mass W1 (g). The culture dish containing the silk fibroin solution was placed in an oven for drying and then taken out and weighed to obtain the mass W2 (g). The concentration (C) of the silk fibroin solution was calculated according to the following formula:

[0094] Concentration (%) = [(W2-W0) / (W1-W0)] × 100

[0095] (3) Polyester fabric pretreatment

[0096] The polyester fabric was soaked in a 10% NaOH solution and treated in a 60°C water bath for 1 hour. The treated fabric was soaked in deionized water to remove excess alkali solution and then dried for storage.

[0097] (4) Preparation of coating liquid

[0098] After 3% silk fibroin solution and glycerol were mixed evenly in a ratio of 3:1, the resin powder treated in (1) was added to the mixed solution (the mass ratio was 1:40), and magnetic stirring was used for 10 hours to make the mixture evenly mixed.

[0099] (5) Preparation of coated fabrics

[0100] The coating liquid prepared in (4) was poured onto the fabric, pressed back and forth with a glass rod, and dried in an oven at 60° C. to obtain a quaternary amine type anion exchange resin coated polyester fabric (3% SF polyester fabric coating).

[0101] (6) CO2 adsorption performance test

[0102] The adsorption performance test was conducted in a dryer at room temperature and a certain humidity. After the carbon dioxide concentration in the dryer stabilized, the carbon dioxide detector and the dried coated fabric were placed in the dryer, and the dryer was sealed for adsorption test. After adsorption saturation, the humidity in the dryer was adjusted. When the relative humidity increased to 84%, only part of the carbon dioxide adsorbed on the fabric was desorbed, indicating that the hydrophobicity of the polyester fabric hindered the full combination of water vapor and resin under high humidity.

[0103] Example 5

[0104] (1) Pretreatment of quaternary amine anion exchange resin

[0105] The D290 resin is soaked in deionized water at 90°C for 4h-8h, the treated sample is dried in an oven at 60°C, and then ground and sieved into particles of a certain size. The ground resin particles are alkaline washed with a Na2CO3 solution, and the sample is rinsed with deionized water after each washing; the solution and the washing liquid are collected and titrated with silver nitrate until the titration method detects that there is no chlorine in the solution, and then dried to obtain the pretreated quaternary ammonium anion exchange resin.

[0106] (2) Preparation of silk fibroin solution

[0107] Use an analytical balance to weigh 30g of raw silk and 25.44g of anhydrous sodium carbonate for use, measure 12L of deionized water and pour it into a steel barrel, and heat it with an induction cooker. When the deionized water is about to boil, add the weighed anhydrous sodium carbonate, continue to heat it to boiling so that the anhydrous sodium carbonate is fully dissolved, then add 30g of raw silk and cook for 40min, stirring every 10min to dissolve the sericin on the surface of the raw silk. Rub the degummed raw silk with deionized water for 3 times to fully remove the sericin on the surface of the raw silk, and finally place it in a fume hood to dry overnight. The next day, weigh 25g of dry silk and dissolve it in 100mL, 9.3mol / L lithium bromide solution, and place it in a 60℃ oven. During this period, stir once an hour to allow the cooked silk to be fully dissolved. After 4h, take the dissolved silk solution out of the oven, cool it to room temperature, pour it into a dialysis bag, dialyze it with deionized water for 40h, and change the deionized water every 5h. The dialyzed silk solution was centrifuged twice using a high-speed centrifuge (9000rpm, 20min) to remove impurities for later use. The concentration of the purified silk fibroin solution was measured by the following method: the mass of the dry culture dish was weighed and recorded as W0 (g). Then 1mL of silk fibroin solution was dripped into the culture dish and weighed to obtain the mass W1 (g). The culture dish containing the silk fibroin solution was placed in an oven for drying and then taken out and weighed to obtain the mass W2 (g). The concentration (C) of the silk fibroin solution was calculated according to the following formula:

[0108] Concentration (%) = [(W2-W0) / (W1-W0)] × 100

[0109] (3) Polyester fabric pretreatment

[0110] The polyester fabric was soaked in a 10% NaOH solution and treated in a 60°C water bath for 1 hour. The treated fabric was soaked in deionized water to remove excess alkali solution and then dried for storage.

[0111] (4) Preparation of coating liquid

[0112] After 5% silk fibroin solution and glycerol were mixed evenly in a ratio of 3:1, the resin powder treated in (1) was added to the mixed solution (the mass ratio was 1:40), and magnetic stirring was used for 10 hours to make the mixture evenly mixed.

[0113] (5) Preparation of coated fabrics

[0114] The coating liquid prepared in (4) was poured onto the fabric, pressed back and forth with a glass rod, and dried in an oven at 60° C. to obtain a quaternary amine type anion exchange resin coated polyester fabric (5% SF polyester fabric coating).

[0115] (6) CO2 adsorption performance test

[0116] The adsorption performance test was conducted in a dryer at room temperature and a certain humidity. After the carbon dioxide concentration in the dryer stabilized, the carbon dioxide detector and the dried coated fabric were placed in the dryer, and the dryer was sealed for adsorption test. After adsorption saturation, the humidity in the dryer was adjusted. When the relative humidity increased to 85%, only part of the carbon dioxide adsorbed on the fabric was desorbed, indicating that the hydrophobicity of the polyester fabric hindered the full combination of water vapor and resin under high humidity.

[0117] Example 6

[0118] (1) Pretreatment of quaternary amine anion exchange resin

[0119] The D290 resin was soaked in deionized water at 90°C for 4h-8h, the treated sample was dried in an oven at 60°C, then ground and sieved into particles with an average particle size of ≤30μm, the ground resin particles were alkaline washed with Na2CO3 solution, and the sample was rinsed with deionized water after each washing; the solution and washing liquid were collected and titrated with silver nitrate until the titration method detected that there was no chlorine in the solution, and then dried to obtain the pretreated quaternary ammonium anion exchange resin.

[0120] (2) Preparation of silk fibroin solution

[0121] Use an analytical balance to weigh 30g of raw silk and 25.44g of anhydrous sodium carbonate for use, measure 12L of deionized water and pour it into a steel barrel, and heat it with an induction cooker. When the deionized water is about to boil, add the weighed anhydrous sodium carbonate, continue to heat it to boiling so that the anhydrous sodium carbonate is fully dissolved, then add 30g of raw silk and cook for 40min, stirring every 10min to dissolve the sericin on the surface of the raw silk. Rub the degummed raw silk with deionized water for 3 times to fully remove the sericin on the surface of the raw silk, and finally place it in a fume hood to dry overnight. The next day, weigh 25g of dry silk and dissolve it in 100mL, 9.3mol / L lithium bromide solution, and place it in a 60℃ oven. During this period, stir once an hour to allow the cooked silk to be fully dissolved. After 4h, take the dissolved silk solution out of the oven, cool it to room temperature, pour it into a dialysis bag, dialyze it with deionized water for 40h, and change the deionized water every 5h. The dialyzed silk solution was centrifuged twice using a high-speed centrifuge (9000rpm, 20min) to remove impurities for later use. The concentration of the purified silk fibroin solution was measured by the following method: the mass of the dry culture dish was weighed and recorded as W0 (g). Then 1mL of silk fibroin solution was dripped into the culture dish and weighed to obtain the mass W1 (g). The culture dish containing the silk fibroin solution was placed in an oven for drying and then taken out and weighed to obtain the mass W2 (g). The concentration (C) of the silk fibroin solution was calculated according to the following formula:

[0122] Concentration (%) = [(W2-W0) / (W1-W0)] × 100

[0123] (3) Fabric pretreatment

[0124] The polyester-cotton blended fabric was soaked in a 10% NaOH solution and treated in a 60° C. water bath for 1 h. The treated fabric was soaked in deionized water to remove excess alkali solution and then dried for storage.

[0125] (4) Preparation of coating liquid

[0126] After 2% silk fibroin solution and glycerol were mixed evenly in a ratio of 3:1, the resin powder treated in (1) was added to the mixed solution (the mass ratio was 1:40), and magnetic stirring was used for 10 hours to make the mixture evenly mixed.

[0127] (5) Preparation of coated fabrics

[0128] The coating liquid prepared in (4) was poured onto the fabric, pressed back and forth with a glass rod, and dried in an oven at 60° C. to obtain a quaternary amine type anion exchange resin coated polyester-cotton blended fabric (polyester-cotton blended fabric coating).

[0129] (6) CO2 adsorption / desorption performance test

[0130] The adsorption performance test was conducted in a dryer at room temperature and a certain humidity. After the carbon dioxide concentration in the dryer stabilized, the carbon dioxide detector and the dried coated fabric were placed in the dryer, and the dryer was sealed for adsorption test. After adsorption saturation, the humidity in the dryer was adjusted. When the relative humidity increased to 80%, most of the carbon dioxide adsorbed on the fabric was desorbed. Its desorption amount was between that of cotton coated fabric and polyester coated fabric.

[0131] Test Example 1

[0132] In this test example, the hydrophilicity and hydrophobicity of the polyester coated fabric, polyester-cotton blended coated fabric and cotton coated fabric obtained in Examples 2, 3 and 6 were tested by contact angle test. The specific results are as follows: Figure 3 As shown by Figure 3 It can be seen that polyester coated fabric has better hydrophobicity, cotton fabric has better hydrophilicity, and the hydrophilicity of polyester-cotton blended coated fabric is between the two.

[0133] Test Example 2

[0134] In this test example, the cotton fabric coating, polyester fabric coating, polyester-cotton blended fabric coating and control group (D290 resin) obtained in Examples 2, 3 and 6 were subjected to adsorption tests: the adsorption performance test was conducted in a dryer at room temperature and a relative humidity of 30%. After the carbon dioxide concentration in the dryer stabilized, the carbon dioxide detector and the dried coated fabric were placed in the dryer, and the dryer was sealed for adsorption test. The test results are shown in FIG. Figure 4 shown by Figure 4The results showed that the three coated fabrics adsorbed CO2 in a dry state, which reduced the CO2 concentration in the dryer. Compared with the adsorption efficiency of the resin particles in the control group, the adsorption efficiency of the coated fabrics was significantly improved.

[0135] Test Example 3

[0136] The concentration of silk protein will directly affect the air permeability of the coated fabric. In order to explore the effect of adsorption of different silk protein concentrations, the polyester coated fabrics with different concentrations of silk protein in Examples 3, 4, and 5 were selected as test objects, and the original polyester fabric was used as a control. The air permeability of the fabric was tested by a fully automatic air permeability measuring instrument. The test results are as follows: Figure 5 As shown. Figure 5 It can be seen that 2% SF coating has no obvious effect on the air permeability of the fabric, but with the increase of silk protein concentration, the air permeability of the coated fabric decreases.

[0137] Test Example 4

[0138] The concentration of silk protein will directly affect the air permeability of the coated fabric, and the air permeability will also directly affect its adsorption efficiency. Therefore, this test selected the polyester coated fabrics with different concentrations of silk protein in Examples 3, 4, and 5 as the test objects, and conducted the adsorption performance test in a dryer at room temperature and a relative humidity of 30%. After the carbon dioxide concentration in the dryer stabilized, the carbon dioxide detector and the dried coated fabric were placed in the dryer, and the dryer was sealed for adsorption test. The test results are shown in Figure 2. Figure 6 As shown. Figure 6 It can be seen that as the silk protein concentration increases, the adsorption efficiency of the coated fabric decreases, which is consistent with the change in air permeability in Test Example 3.

[0139] Test Example 5

[0140] The quaternary ammonium ion resin adsorbent material achieves the regeneration cycle of the adsorbent material by regulating the partial pressure of ambient water vapor. The change of ambient relative humidity will affect the CO2 adsorption hydration process and have a significant impact on the saturated adsorption capacity and adsorption rate. In order to explore the effect of relative humidity on the kinetic properties of the adsorbent, this test selected the polyester coated fabric in Example 6 as the test object, and conducted adsorption experiments under relative humidity conditions of 10% RH, 30% RH and 70% RH at room temperature. The test results are as follows: Figure 7 As shown. Figure 7 It can be seen that the change of environmental relative humidity has a significant effect on the CO2 adsorption rate. With the increase of relative humidity, the adsorption rate and adsorption capacity of the coated fabric decrease significantly.

[0141] Test Example 6

[0142] In this test example, the cotton fabric coating, polyester fabric coating, polyester-cotton blended fabric coating and the control group (D290 resin) obtained in Examples 2, 3 and 6 were subjected to CO2 desorption test by adjusting the humidity: after the coated fabric in Test Example 2 was saturated with adsorption, the relative humidity in the dryer was adjusted to above 80%, and the CO2 concentration in the dryer was detected at this time. The results are as follows: Figure 8-A shown.

[0143] The CO2 desorption test was performed by wetting the saturated coated fabric in Test Example 2, and the results are as follows: Figure 8-B shown.

[0144] Depend on Figure 8-A and Figure 8-B The results show that when adjusting the ambient humidity, the coated fabric actively absorbs water vapor from the environment. Cotton fabric has a higher affinity for water vapor than polyester due to its good hygroscopic properties, and the most carbon dioxide is desorbed on cotton fabric. Polyester is hydrophobic, so the water vapor in the environment is blocked and it is difficult to completely contact the surface of the quaternary ammonium resin. Therefore, even under high humidity, only a small amount of CO2 is desorbed from the fabric. The polyester-cotton blended coated fabric is in between the two. When the coated fabric is completely wetted, the loaded quaternary ammonium resin is fully in contact with water, so that the carbon dioxide adsorbed by the three fabrics is fully released.

[0145] Test Example 7

[0146] The regeneration adsorption efficiency of the coated fabric obtained in Example 6 was tested by drying adsorption-wetting desorption-drying adsorption-wetting desorption, and the test results were as follows: Fig. 9 shown by Fig. 9 The test results show that the material's ability to adsorb carbon dioxide has not significantly diminished after multiple cycles.

[0147] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.

Claims

1. A quaternary amine type anion exchange resin coated fabric, characterized in that: The coating liquid containing quaternary amine anion exchange resin is coated on the fabric after alkali treatment, and the quaternary amine anion exchange resin coated fabric is obtained by impregnation, pressing and drying; the quaternary amine anion exchange resin is dispersed in the fiber gaps of the fabric; The coating liquid containing quaternary amine anion exchange resin is prepared by the following method: The silk fibroin solution is mixed with an organic solvent to obtain a mixed solution; the pretreated quaternary ammonium anion exchange resin is added to the mixed solution and stirred to obtain a coating solution containing the quaternary ammonium anion exchange resin; The pretreated quaternary amine anion exchange resin is prepared by the following method: The quaternary ammonium anion exchange resin is ground to an average particle size of ≤30 μm, then alkali washed and dried to obtain the pretreated quaternary ammonium anion exchange resin.

2. The quaternary amine type anion exchange resin coated fabric according to claim 1, characterized in that: The silk fibroin solution is prepared by the following method: S1. dissolving an alkaline reagent in boiling water, adding raw silk, and continuing to boil, stir, and knead the raw silk so that the sericin on the surface of the raw silk is fully removed, and then drying to obtain dried silk; S2. The dried silk obtained in S1 is dissolved in a lithium bromide solution, dialyzed, and centrifuged to obtain the silk fibroin solution.

3. The quaternary amine type anion exchange resin coated fabric according to claim 1, characterized in that: The organic solvent is selected from one or more of glycerol, PEG and ethanol.

4. The quaternary amine type anion exchange resin coated fabric according to claim 1, characterized in that: The mass concentration of the silk protein solution is 1%-6%.

5. The quaternary amine type anion exchange resin coated fabric according to claim 1, characterized in that: The fabric is selected from one or more of cotton fabric, polyester fabric and polyester-cotton blended fabric.

6. Use of the quaternary amine anion exchange resin coated fabric according to claim 1 in regulating carbon dioxide in the air.

7. The use according to claim 6, characterized in that: The carbon dioxide regulation is carried out under the condition of humidity of 10%-99%.

8. The method for preparing a quaternary amine type anion exchange resin coated fabric according to any one of claims 1 to 5, characterized in that: The specific steps include: The coating liquid containing quaternary amine type anion exchange resin is coated on the fabric after alkali treatment, and the quaternary amine type anion exchange resin coated fabric is obtained by impregnation, pressing and drying.