An EVS-10-based cerium-supported catalytic adsorbent for flue gas demercuration and denitrification, and its preparation method and application
By loading the CeO2 active component on the EVS-10 molecular sieve, an efficient EVS-10-based cerium-supported catalytic adsorbent is prepared, which solves the problems of low mercury and nitrogen oxide removal efficiency and easy agglomeration in the existing technology, and achieves Efficient flue gas collaborative removal and improved anti-sulfur poisoning performance are suitable for industrial applications.
Patent Information
- Application Number
- CN202111276215.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The existing EVS-10 molecular sieve catalyst has low efficiency in removing mercury and nitrogen oxides from the flue gas of coal-fired power stations, and is prone to agglomeration during repeated recycling processes, making it unsuitable for industrial applications.
By loading highly dispersed CeO2 active components on EVS-10 molecular sieves, an EVS-10-based cerium-supported catalytic adsorbent was prepared. Ultrasonic treatment and roasting were used to form the catalytic adsorbent to improve its mercury removal and denitration performance. .
It significantly improves the mercury removal efficiency and denitrification efficiency of the catalytic adsorbent, achieves the coordinated removal of elemental mercury and nitrogen oxides in coal-fired flue gas, improves the resistance to sulfur poisoning and service life, reduces the overall cost, and is suitable for industrialization Production and equipment upgrades.
Smart Images

Figure BDA0003330025970000091
Abstract
Description
Technical Field
[0001] The present disclosure relates to the technical field of environmental protection and air pollution control, and in particular to an EVS-10-based cerium-supported catalytic adsorbent for flue gas demercuration and denitrification, and a preparation method and application thereof. Background Art
[0002] The flue gas emitted by coal-fired power plants contains mercury, which is a toxic heavy metal that causes serious harm to human health and the ecological environment. Coal-fired power plants are considered to be the world's largest source of anthropogenic mercury emissions and one of the most important sources of anthropogenic mercury emissions. The mercury contained in the flue gas of coal-fired power plants mainly includes Hg 2+ , Hg p and Hg 0 There are three forms. Among them, Hg 2+ It is soluble in water, so it can be removed efficiently by using pollutant control equipment wet desulfurization device; Hg in flue gas p It is easy to combine with fly ash and can be removed by particulate matter control equipment, such as bag filters or electrostatic precipitators; while Hg 0 It is insoluble in water and highly volatile. It is quite stable at low temperatures and is difficult to be removed by existing pollutant control equipment. Therefore, it is directly discharged into the atmosphere during flue gas emission, causing environmental pollution and harming human health. Therefore, the key to removing mercury from flue gas in coal-fired power plants is to control Hg 0 emissions.
[0003] At present, the two main research directions of mercury removal are adsorbent demercuration and catalytic oxidation demercuration. 0 Through physical or chemical adsorption to the adsorbent surface, and then removed by the particulate matter control equipment; catalytic oxidation demercuration is to remove Hg 0 Highly efficient oxidation to Hg 2+ , and then removed by the wet desulfurization device. EVS-10 molecular sieve is a type of molecular sieve in which vanadium completely replaces the titanium in the titanium silicate molecular sieve ETS-10. It is mainly composed of vanadium oxygen octahedrons and silicon oxygen tetrahedrons, and is linked by common corner oxygen atoms to form a three-dimensional network structure. It is similar to industrial vanadium-supported catalysts and can catalyze the oxidation of elemental mercury. However, experimental test results show that the efficiency of catalytic oxidation of mercury by this material is low, about 48%.
[0004] In addition to elemental mercury, nitrogen oxides are also a common air pollutant produced by coal combustion, which can cause acid rain and the greenhouse effect. x) has a high proportion of NO, accounting for more than 95%. Therefore, efficient removal of NO is the key to achieving the removal of nitrogen oxides. At present, the most effective and widely used technology for removing NO from coal-fired flue gas is NH3 selective catalytic reduction (SCR) technology. The SCR catalysts currently studied are mainly prepared by loading metal oxides such as V2O5, CuO, Cr2O3, CeO2, Fe2O3, MnOx, Co2O3, etc. on carriers such as Al2O3, SiO2, TiO2, ZrO2, carbon materials and molecular sieves. However, the existing EVS-10 molecular sieve has a certain ability to remove mercury, but its catalytic denitrification performance is poor, with a removal efficiency of only 14%, and it is impossible to achieve the effects of efficient mercury removal and denitrification at the same time; and it is easy to agglomerate into larger particles during repeated recycling, which is not conducive to the repeated recycling of molecular sieves. Summary of the invention
[0005] The purpose of the present disclosure is to provide an EVS-10-based cerium-supported catalytic adsorbent for flue gas demercuration and denitrification, and a preparation method and application thereof, wherein the catalytic adsorbent can achieve the synergistic removal of mercury and nitrogen oxides.
[0006] In order to achieve the above-mentioned objectives, the first aspect of the present disclosure provides an EVS-10-based cerium-supported catalytic adsorbent for flue gas demercurization and denitrification, the catalytic adsorbent comprising a carrier and an active component supported on the carrier; wherein the carrier comprises an EVS-10 molecular sieve, and the active component comprises CeO2.
[0007] Optionally, based on the total weight of the catalytic adsorbent, the mass fraction of the carrier is 85 to 99 weight %, and the mass fraction of the active component is 1 to 15 weight %.
[0008] The second aspect of the present disclosure provides a method for preparing the catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure, comprising the following steps: (1) mixing EVS-10 molecular sieve, a cerium source and water to obtain a raw material mixture; (2) adding an alkaline solution to the raw material mixture; and then adding alcohol to obtain a colloidal precursor; and (3) calcining the colloidal precursor.
[0009] Optionally, in step (1), the weight ratio of the EVS-10 molecular sieve, the cerium source and water is (90-95): (13-18);
[0010] Optionally, the cerium source is a soluble cerium salt, preferably one or more selected from cerium acetate, cerium chloride and cerium nitrate.
[0011] Optionally, step (1) further comprises: ultrasonically treating the EVS-10 molecular sieve in water for 5 to 30 minutes, and then adding the cerium source and an optional dispersing aid to mix to obtain the raw material mixture; preferably, the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, and more preferably polymethacrylic acid.
[0012] Optionally, the weight ratio of the dispersing aid to the cerium source is (34-68): (13-18).
[0013] Optionally, in step (2), the alkaline solution includes aqueous ammonia; the alcohol includes ethanol; and further preferably, the volume ratio of the aqueous ammonia to the alcohol is (4-8):(60-70).
[0014] Optionally, step (2) further includes:
[0015] Adding the alkaline solution to the raw material mixture obtained in step (1) and then ultrasonically treating for 5 to 30 minutes; and
[0016] Before the calcination treatment, the colloidal precursor is subjected to ultrasonic treatment for 5 to 30 minutes and then evaporated at 70 to 100°C.
[0017] Optionally, in step (3), the conditions of the calcination treatment include: a calcination temperature of 350 to 600° C. and a calcination time of 1 to 4 hours;
[0018] Optionally, step (3) further comprises: cooling the calcined product and then screening it, taking the sieve material to obtain the catalytic adsorbent.
[0019] The third aspect of the present disclosure provides application of the catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure in the field of mercury removal and denitrification of flue gas in coal-fired power plants.
[0020] Through the above technical scheme, the present disclosure provides an EVS-10-based cerium-supported catalytic adsorbent for flue gas demercuration and denitrification, and a preparation method and application thereof. The present disclosure loads a highly dispersed active component containing CeO2 on the EVS-10 molecular sieve, so that the catalytic adsorbent has good mercury removal efficiency and high denitrification efficiency, and has a good application effect in the synergistic removal of elemental mercury and nitrogen oxides in coal-fired flue gas; the catalytic adsorbent is relatively simple to synthesize and can be recycled, which greatly reduces the overall cost and is suitable for industrial production; and the catalytic adsorbent has improved anti-sulfur poisoning performance, good process adaptability and compatibility, and is suitable for use in series with dust removal and desulfurization equipment, and is particularly suitable for enterprises with desulfurization and dust removal equipment to expand the upgrade and transformation for demercuration, reducing equipment installation and use costs, and has industrial application prospects.
[0021] Other features and advantages of the present disclosure will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0022] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0023] The inventors of the present disclosure have found in their research that loading an active component containing CeO2 on the EVS-10 molecular sieve can not only greatly improve the mercury removal efficiency of the EVS-10 molecular sieve (from about 48% to 97%), but also enable the molecular sieve loaded with CeO2 to have good nitrogen oxide removal performance (about 86%); the inventors further conducted long-term tests on the molecular sieve loaded with the CeO2 active component in a complex SO2 flue gas environment, and there was no obvious attenuation in performance, indicating that the molecular sieve loaded with the CeO2 active component has improved resistance to sulfur poisoning and service life.
[0024] In a first aspect, the present disclosure provides an EVS-10-based cerium-supported catalytic adsorbent for flue gas demercuration and denitrification, the catalytic adsorbent comprising a carrier and an active component supported on the carrier; wherein the carrier comprises an EVS-10 molecular sieve, and the active component comprises CeO2.
[0025] The present invention loads highly dispersed active components including CeO2 on the EVS-10 molecular sieve, so that the catalytic adsorbent has good mercury removal efficiency and high denitrification efficiency, and has good application effect in the synergistic removal of elemental mercury and nitrogen oxides in coal-fired flue gas; the catalytic adsorbent is relatively simple to synthesize and can be recycled, which greatly reduces the overall cost and is suitable for industrial production; and the catalytic adsorbent has improved anti-sulfur poisoning performance, good process adaptability and compatibility, and is suitable for use in series with dust removal and desulfurization equipment, and is particularly suitable for enterprises with desulfurization and dust removal equipment to expand the upgrade and transformation for mercury removal, reducing equipment installation and use costs, and has industrial application prospects.
[0026] In the present disclosure, the EVS-10 molecular sieve has high hydrothermal stability, large specific surface area, fast heat and mass transfer, and is an excellent catalyst and carrier. In the present disclosure, CeO2 is loaded on the EVS-10 molecular sieve to obtain a catalytic adsorbent, wherein the molecular sieve framework contains vanadium, which can catalytically oxidize part of elemental mercury; and CeO2 has good denitrification performance and can also catalytically oxidize elemental mercury. The vanadium in the framework and the loaded CeO2 can achieve synergistic demercurization and denitrification.
[0027] In one embodiment, based on the total weight of the catalytic adsorbent, the mass fraction of the carrier is 85-99 weight percent, and the mass fraction of the active component is 1-15 weight percent. When the content of each component in the catalytic adsorbent provided by the present disclosure is within the range of this embodiment, the obtained catalytic adsorbent can achieve a good synergistic removal effect of elemental mercury and nitrogen oxides.
[0028] In one embodiment, the carrier is an EVS-10 molecular sieve, and the molar ratio of Si:Na:K:V in the EVS-10 molecular sieve is 3.92:1.39:0.48:1, based on the molar amount of the elements. Specifically, the chemical composition of the EVS-10 molecular sieve can be determined by XRF spectroscopy.
[0029] The second aspect of the present disclosure provides a method for preparing the catalytic adsorbent for mercury removal and denitrification according to the first aspect of the present disclosure, comprising the following steps:
[0030] (1) mixing EVS-10 molecular sieve, a cerium source and water to obtain a raw material mixture;
[0031] (2) adding an alkaline solution to the raw material mixture, and then adding alcohol to obtain a colloidal precursor;
[0032] (3) calcining the colloidal precursor.
[0033] The synthesis method provided by the present disclosure is stable and reliable, the comprehensive use cost of the catalytic adsorbent is low, and it has good prospects for industrial application.
[0034] Specifically, the amount of raw material added or the weight ratio between different raw materials in the present disclosure, such as the amount or weight ratio of EVS-10 molecular sieve and cerium source, is obtained by adjusting the mass fraction of each component in the catalytic adsorbent provided in the first aspect of the present disclosure. The EVS-10 molecular sieve can be prepared according to existing methods, for example, according to the method disclosed in the document Zijian Zhou, Tiantian Cao, et al. "Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elemental mercury removal from flue gas". Journal of Hazardous Materials, 375 (2019) 1-8.
[0035] The EVS-10 molecular sieve used in the present disclosure can be prepared by a hydrothermal method. In a specific embodiment, the steps include: dissolving sodium silicate in deionized water; then adding NaOH, KCl, NaF and NaCl to the solution to obtain solution A. Then VOSO4 is dissolved in deionized water to obtain solution B. Solution A and solution B are mixed and stirred, and aged at room temperature. The aged mixture is transferred to an autoclave for further aging. The synthesized product is washed with deionized water and dried to obtain an EVS-10 molecular sieve. During the preparation process, the amount of each reactant and the reaction conditions can be adjusted according to actual needs.
[0036] In one embodiment, in step (1), the weight ratio of the EVS-10 molecular sieve, the cerium source and water is (90-95): (13-18); optionally, the cerium source is a soluble cerium salt, preferably one or more of cerium acetate, cerium chloride and cerium nitrate.
[0037] In a preferred embodiment, step (1) further comprises: ultrasonically treating the EVS-10 molecular sieve in water for 5 to 30 minutes, and then adding the cerium source and an optional dispersing aid to mix to obtain the raw material mixture; preferably, the weight ratio of the dispersing aid to the cerium source is (34 to 68): (13 to 18).
[0038] In a preferred embodiment, the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride, and polymethacrylic acid is further preferred. The inventors of the present disclosure have found in their research that when introducing cerium element into EVS-10 molecular sieve, adding one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride into the raw material mixture can improve the dispersion of cerium ions and further improve the mercury removal and denitrification performance of the finally prepared catalytic adsorbent.
[0039] The present invention adopts a dispersing aid to form a complex with Ce ions in a solution, so that the Ce ions are uniformly dispersed in the system in the form of a complex. When an alkaline solution (such as ammonia water) is subsequently added, a uniformly dispersed Ce(OH)4 complex can be obtained, further avoiding agglomeration; after adding alcohol, the complex in the system forms a dispersing aid-Ce polymer particle (such as PMAA-Ce polymer particle) on the surface of the EVS-10 molecular sieve, and the electrostatic repulsion between the particles makes the system stable, ensuring the dispersion of Ce ions in the preparation system, so that the particle size of CeO2 loaded in the finally synthesized catalytic adsorbent is small and uniformly distributed.
[0040] In one embodiment, in step (2), the alkaline solution includes aqueous ammonia; the alcohol includes ethanol; and more preferably, the volume ratio of the aqueous ammonia to the alcohol is (4-8):(60-70).
[0041] In one embodiment, step (2) further comprises: adding the alkaline solution to the raw material mixture obtained in step (1) and then ultrasonically treating for 5 to 30 minutes; and
[0042] Before the calcination treatment, the colloidal precursor is subjected to ultrasonic treatment for 5 to 30 minutes and then evaporated at 70 to 100° C. The ultrasonic treatment in the present disclosure refers to ultrasonic treatment using a conventional ultrasonic instrument to make the materials mixed or dispersed more uniformly.
[0043] In one embodiment, in step (3), the conditions of the calcination treatment include: a calcination temperature of 350 to 600° C. and a calcination time of 1 to 4 hours;
[0044] Optionally, step (3) further comprises: cooling the calcined product and then screening it, taking the sieve residue to obtain the catalytic adsorbent. For example, after cooling to room temperature, screening it with a 100-mesh sieve, taking the sieve residue as the final catalytic adsorbent.
[0045] The third aspect of the present disclosure provides application of the catalytic adsorbent described in the first aspect of the present disclosure in the field of flue gas demercurization and denitrification; optionally, the flue gas is flue gas from a coal-fired power plant.
[0046] The present invention is further described below in conjunction with specific embodiments, but the scope of protection claimed by the present invention is not limited to the scope described in the embodiments.
[0047] The chemicals used in each example can be obtained through public commercial channels.
[0048] The EVS-10 molecular sieve used in the following examples and comparative examples was prepared according to the method disclosed in Zijian Zhou, Tiantian Cao, et al. "Vanadium silicate (EVS)-supported silver nanoparticles: A novel catalytic sorbent for elemental mercury removal from flue gas". Journal of Hazardous Materials, 375 (2019) 1-8.
[0049] The 25% ammonia water used in the following examples, comparative examples and comparative examples is ammonia water having an NH3·H2O content of 25% by weight.
[0050] Ultrasonic treatment uses conventional ultrasonic equipment to make the materials mixed or dispersed more uniformly.
[0051] Example 1
[0052] (1) 9.0 g of EVS-10 molecular sieve was dispersed in 50 mL of deionized water, and after ultrasonic treatment for 15 minutes, 1.8 g of (CH3CO2)3Ce hydrate and 6.8 g of polymethacrylic acid were added;
[0053] (2) Add 8 mL of 25% ammonia water and perform ultrasonic treatment for 15 minutes, then add 70 mL of ethanol to form a colloidal precursor. After continuing the ultrasonic treatment for 30 minutes, evaporate the sample at 80°C, and finally calcine the sample at 500°C in a muffle furnace for 2 hours. After cooling to room temperature, sieve the sample with a 100-mesh sieve and take the particles under the sieve to obtain a catalytic adsorbent loaded with CeO2, which is recorded as sample 1.
[0054] Comparative Example 1
[0055] The catalytic adsorbent was prepared by similar steps to Example 1, except that the EVS-10 molecular sieve was replaced with the commercially available ETS-10 molecular sieve. The other preparation steps were the same as those in Example 1, and a catalytic adsorbent loaded with CeO2 was obtained, which was recorded as sample D-1.
[0056] Example 2
[0057] (1) 9.5 g of EVS-10 molecular sieve was dispersed in 60 mL of deionized water, and then ultrasonicated for 15 min and then 1.3 g of Ce(NO3)3·6H2O and 3.4 g of polymethacrylic acid were added;
[0058] (2) Add 4 mL of 25% ammonia water and ultrasonically treat for 15 minutes, then add 60 mL of ethanol to form a colloidal precursor. After continuing the ultrasonic treatment for 30 minutes, evaporate the sample at 80°C, and finally calcine the sample at 600°C in a muffle furnace for 2 hours. After cooling to room temperature, sieve with a 100-mesh sieve, take the particles under the sieve, and obtain a catalytic adsorbent loaded with CeO2, which is recorded as sample 2.
[0059] Example 3
[0060] The catalytic adsorbent was prepared by the steps similar to those in Example 1, except that no polymethacrylic acid dispersing aid was added in step (1), and the other preparation processes and reaction conditions were the same as those in Example 1. A catalytic adsorbent loaded with CeO2 was obtained, which was recorded as Sample 3.
[0061] Comparative Example 2
[0062] Weigh 4.3 g of AgNO3 and dissolve it in 100 ml of deionized water, then add 10 g of EVS-10 molecular sieve, stir it magnetically in a dark environment for 6 h, then filter it, rinse it repeatedly with deionized water, dry it at 80 ° C, and then bake it in a tube furnace at 250 ° C in a nitrogen atmosphere for 1 hour. The catalytic adsorbent loaded with only silver nanoparticles is obtained, which is recorded as sample D-2.
[0063] The mass fractions of the carrier molecular sieve and CeO2 in the samples obtained from the above embodiments and comparative examples are listed in Table 1.
[0064] Table 1
[0065]
[0066] Simulated smoke test example
[0067] The samples synthesized in the above examples and comparative examples were placed in a simulated flue gas experimental system to test the demercuration and denitrification performance. The simulated flue gas conditions are as follows: 5% O2, 12% CO2, 400ppm NO, 400ppm NH3, 600ppm SO2, 30ppm HCl, Hg 0 Concentration: 110 μg / m 3 The balance gas is N2, the flow rate is 500 mL / min, and the test temperature is 250° C. The results of the mercury removal and denitrification tests are listed in Table 2 below.
[0068] Table 2
[0069] sample <![CDATA[Hg 0 Removal efficiency (%)]]> <![CDATA[NO x Removal efficiency (%)]]> 1 97 86 D-1 74 67 2 93 84 3 83 67 D-2 100 21
[0070] According to Table 2 above, compared with the commercially available ETS-10 molecular sieve used in Comparative Example 1, the Hg content of the catalyst prepared by using EVS-10 molecular sieve in Example 1 of the present disclosure is 0 Removal efficiency and NO x The removal efficiency is better.
[0071] Comparing Examples 1 to 3 of the present disclosure with Comparative Example 2, although Comparative Example 2 can achieve a good elemental mercury removal efficiency, the nitrogen oxide removal efficiency is extremely low, only 21%. The catalytic adsorbent samples prepared by the method provided by the present disclosure in Examples 1 to 3 have high elemental mercury removal efficiency and nitrogen oxide removal efficiency, achieving synergistic removal of Hg 0 and NO x .
[0072] Further comparison of Examples 1 to 3 shows that when the dispersing aid is added in Examples 1 to 2, the obtained catalytic adsorbent has a higher Hg 0 Removal efficiency and NO x Removal efficiency.
[0073] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0074] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0075] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. An EVS-10-based cerium-supported catalytic adsorbent for flue gas demercuration and denitrification, characterized in that: The catalytic adsorbent comprises a carrier and an active component loaded on the carrier; wherein the carrier comprises EVS-10 molecular sieve, and the active component comprises CeO2; based on the total weight of the catalytic adsorbent, the mass fraction of the carrier is 85-99% by weight, and the mass fraction of the active component is 1-15% by weight; The catalytic adsorbent is prepared by a method comprising the following steps: (1) mixing EVS-10 molecular sieve, cerium source and water to obtain a raw material mixture; (2) adding an alkaline solution to the raw material mixture; and then adding alcohol to obtain a colloidal precursor; (3) calcining the colloidal precursor; Step (1) further comprises: ultrasonically treating the EVS-10 molecular sieve in water for 5 to 30 minutes, and then adding the cerium source and a dispersing aid to mix to obtain the raw material mixture; the dispersing aid is selected from one or more of polymethacrylic acid, polyacrylic acid and hydrolyzed polymaleic anhydride.
2. The catalytic adsorbent according to claim 1, characterized in that: In step (1), the weight ratio of the EVS-10 molecular sieve, the cerium source and water is (90-95): (13-18); The cerium source is a soluble cerium salt.
3. The catalytic adsorbent according to claim 2, characterized in that: The cerium source is selected from one or more of cerium acetate, cerium chloride and cerium nitrate.
4. The catalytic adsorbent according to claim 1, characterized in that: The dispersing aid is polymethacrylic acid.
5. The catalytic adsorbent according to claim 1, characterized in that: The weight ratio of the dispersing aid to the cerium source is (34-68): (13-18).
6. The catalytic adsorbent according to claim 1, characterized in that: In step (2), the alkaline solution includes aqueous ammonia; and the alcohol includes ethanol.
7. The catalytic adsorbent according to claim 6, characterized in that: In step (2), the volume ratio of the added ammonia water to the added alcohol is (4-8):(60-70).
8. The catalytic adsorbent according to claim 1, characterized in that: Step (2) also includes: Adding the alkaline solution to the raw material mixture obtained in step (1) and subjecting the mixture to ultrasonic treatment for 5 to 30 minutes; and Prior to the calcination treatment, the colloidal precursor is subjected to ultrasonic treatment for 5 to 30 minutes and then evaporated at 70 to 100°C.
9. The catalytic adsorbent according to claim 1, characterized in that: In step (3), the conditions for the calcination treatment include: a calcination temperature of 350-600° C. and a calcination time of 1-4 hours.
10. The catalytic adsorbent according to claim 9, characterized in that: Step (3) also includes: cooling the calcined product and then screening it, taking the sieve material to obtain the catalytic adsorbent.
11. Use of the catalytic adsorbent according to any one of claims 1 to 10 in the field of flue gas demercurization and denitrification.
12. The use according to claim 11, characterized in that: The flue gas is flue gas from a coal-fired power plant.