A low carbon alkane dehydrogenation catalyst and its preparation method and application
By performing multiple impregnation and calcining on the alumina support, combined with oxychlorination and reduction treatment, the stability and number of active centers of the low-carbon alkane dehydrogenation catalyst are improved, the problem of fast catalyst deactivation is solved, and propylene is realized High selectivity and stability during preparation.
Patent Information
- Application Number
- CN202111290651.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-02
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-11-02
AI Technical Summary
In the existing propylene production process, the catalyst deactivation rate is fast, and high temperature will lead to an increase in propane cracking reaction and severe carbon deposits, making it difficult to meet the needs of high activity, high selectivity and high stability.
The preparation method of low-carbon alkane dehydrogenation catalyst containing alumina support is adopted. Through multiple impregnation and calcination processes, combined with oxychlorination and reduction treatment, the number of M2 active centers is increased, and the sintering and side reaction activities of Group VIII metals on the support are reduced. Center, improve catalyst stability.
The prepared catalyst has high number of active centers and stability, and is suitable for the process of dehydrogenation of low-carbon olefins to promote propylene, maintaining good product selectivity for the purpose.
Smart Images

Figure BDA0003334744860000131 
Figure BDA0003334744860000132
Abstract
Description
Technical Field
[0001] The invention relates to a low-carbon alkane dehydrogenation catalyst and a preparation method and application thereof. Background Art
[0002] Propylene is an important basic organic chemical raw material, widely used in the production of polypropylene, acetone, acrylonitrile, propylene oxide, acrylic acid and other chemical products. At present, the supply of propylene mainly comes from the by-products of naphtha cracking to produce ethylene and petroleum catalytic cracking process. Since the 1990s, with the continuous increase in the demand for propylene, the traditional propylene production process can no longer meet the demand of the chemical industry for propylene, and other alternative process technologies must be developed at a faster pace. Among them, the process of producing propylene by propane dehydrogenation has attracted the most attention. The process technologies for producing propylene by catalytic dehydrogenation of propane that have been industrialized mainly include UOP's Oleflex technology and Lummus's Catofin technology. The Oleflex process uses a moving bed reactor with continuous catalyst regeneration, with Pt-Sn / Al2O3 as the catalyst, and K or Li is added for modification; the Catofin process uses a fixed bed reactor with Cr2O3 / Al2O3 as the catalyst, and the catalyst deactivates quickly, requiring regeneration every 15 minutes.
[0003] The propane catalytic dehydrogenation reaction is limited by thermodynamic equilibrium, and high temperature and low pressure are conducive to the reaction. However, too high a reaction temperature will increase the propane cracking reaction, cause serious carbon deposition, and accelerate the catalyst deactivation rate. Therefore, the development of propane dehydrogenation catalysts with high activity, high selectivity and high stability has become the key to this technology.
[0004] Supported platinum-based catalysts are an important class of catalysts for dehydrogenation of low-carbon alkanes. US20180311645 discloses a method for preparing a linear light hydrocarbon dehydrogenation catalyst using a stable active metal complex. Due to the high reducibility of tin, platinum is easy to precipitate. In order to obtain a stable Pt-Sn complex solution, an organic solvent that can prevent tin reduction is used, and hydrochloric acid is added to provide an acidic environment. In order to increase the rate of penetration into the carrier, an organic acid is added. The organic solvent can be selected from any one or two of water, methanol, ethanol, butanol, acetone, ethyl acetate, acetonitrile, ethylene glycol, triethylene glycol, ethylene glycol ether, glycerol, sorbitol, xylitol, dialkyl ether, tetrahydrofuran, or can be used in combination. If the platinum-tin complex solution is exposed to air, platinum is easy to precipitate due to the high reducibility of tin. To ensure that the complex is stable, aging is required in an inert gas atmosphere. The inert gas is selected from nitrogen, argon and helium, and nitrogen is preferred.
[0005] US20200122125 and CN110603096 disclose a catalyst for the dehydrogenation of C3-C4 hydrocarbons and a preparation method thereof. Platinum and auxiliary metals exist in the form of an alloy in a single complex within a thickness of 300-500 μm from the outer edge of the catalyst. In the impregnation process, an organic solvent and an inert gas are used to protect aging to ensure the stable existence of the complex. In the catalyst reduction step, a rapid high-temperature reduction method is used for reduction, that is, the temperature is raised to a predetermined temperature under a nitrogen atmosphere, and hydrogen is injected for reduction when the predetermined temperature is reached.
[0006] CN108114717 discloses a C10-C13 long-chain normal alkane dehydrogenation catalyst and its preparation and application. The carrier γ-Al2O3 is prepared by forming an oil column or an oil-ammonia column using a vacuum complexation and one-step co-impregnation method, and is pre-vacuumed for 0.5-1.5 hours. The impregnation solution is water or a mixed solution of water and ethanol. During the impregnation, it is necessary to ensure that hydrochloric acid is added before the stannous chloride solution. The impregnation process is protected by N2 to prevent oxidation of the stannous chloride.
[0007] CN103785383 discloses a method for preparing a dehydrogenation catalyst, wherein a chloroplatinic acid ethylene glycol solution is mixed with a Sn-containing alumina carrier, heated, stirred and refluxed to help improve the Pt dispersion.
[0008] CN104549248 discloses a method for preparing a catalyst for dehydrogenation of low carbon alkanes. First, the carrier is impregnated with a potassium nitrate aqueous solution, and then impregnated with a chloroplatinic acid organic solvent solution after drying, and then dried by program temperature increase, roasted, and washed until the filtrate is free of Cl, and the organic solvent is selected from ethanol, ether or acetone. The purpose is to avoid hydrothermal dechlorination and avoid the aggregation of Pt.
[0009] CN109701529 discloses a highly dispersed dehydrogenation catalyst, a preparation method and a use method. Graphene is dispersed in an organic solvent, a metal salt of an active component is introduced, stirred and a certain amount of a reducing agent is added, and then microwave treatment is performed. The obtained insoluble matter is filtered, washed and dried to obtain a highly dispersed dehydrogenation catalyst. The organic solvent is selected from one or more of ethylene glycol, ethanol or glycerol. Summary of the invention
[0010] The purpose of the present invention is to provide a low-carbon alkane dehydrogenation catalyst and a preparation method and application thereof. The low-carbon alkane dehydrogenation catalyst prepared by the method has a relatively abundant number of M2 active centers, while reducing the sintering of Group VIII metal species on the carrier, reducing side reaction active centers, and the catalyst has higher stability.
[0011] In order to achieve the above object, the first aspect of the present invention provides a method for preparing a light alkane dehydrogenation catalyst, the method comprising:
[0012] S1, contacting an alumina carrier containing a Group IVA metal with a first impregnation solution for first impregnation, taking out a solid after the first impregnation and performing a first calcination to obtain a first solid;
[0013] The first impregnation solution contains a Group VIII metal compound, HCl and a weak polar solvent with a boiling point of 40-99°C; the amount of HCl is 0.1-5 wt% based on the dry weight of the alumina carrier; the content of the weak polar solvent with a boiling point of 40-99°C is 5-99 wt% based on the total weight of HCl and the weak polar solvent with a boiling point of 40-99°C;
[0014] S2, contacting the first solid with a second impregnation solution for a second impregnation, taking out the solid after the second impregnation and performing a second calcination to obtain a second solid; wherein the second impregnation solution contains a Group IA metal compound;
[0015] S3, subjecting the second solid to oxychlorination treatment and reduction treatment in sequence.
[0016] Optionally, in step S1, based on the dry weight of the alumina carrier, the amount of the Group VIII metal compound in the first impregnation solution is 0.1-1.0 wt % in terms of the Group VIII metal, and the amount of HCl in the first impregnation solution is 0.1-2.0 wt %.
[0017] Optionally, based on the total weight of HCl and the weak polar solvent with a boiling point of 40-99° C., the content of the weak polar solvent with a boiling point of 40-99° C. is 15-85% by weight.
[0018] Optionally, in step S1, the content of the Group IVA metal is 0.1-3.0 wt% based on the dry weight of the alumina carrier.
[0019] Optionally, in step S1, the content of the Group IVA metal in the alumina support containing the Group IVA metal is 0.1-2.0 wt% based on the dry weight of the alumina support;
[0020] The Group IVA metal is tin and / or germanium.
[0021] Optionally, in step S2, the amount of the second impregnation liquid is 1.0-3.0 L relative to 1 kg of the first solid;
[0022] The content of the Group IA metal compound in the second impregnation solution is 0.1-3.0 wt % calculated as the Group IA metal, based on the dry weight of the alumina support.
[0023] Optionally, the weakly polar solvent with a boiling point of 40-99° C. is selected from one or more aqueous solutions of C1-C5 fatty alcohols, ethyl acetate and acetone;
[0024] The Group VIII metal compound is selected from one or more of chloroplatinic acid, ammonium chloroplatinate and platinum chloride;
[0025] The Group IA metal compound is selected from one or more of potassium hydroxide, lithium hydroxide, sodium hydroxide and cesium hydroxide.
[0026] Optionally, the first impregnation conditions include: a temperature of 25-60° C. and a time of 1-10 hours;
[0027] The first calcination conditions include: a temperature of 450-600° C. and a time of 1-10 hours;
[0028] The conditions of the second impregnation include: a temperature of 25-60°C and a time of 1-10 hours;
[0029] The second calcination conditions include: a temperature of 450-650° C. and a time of 1-10 hours;
[0030] The conditions of the oxychlorination treatment include: a temperature of 480-660° C., a time of 1-10 hours, and the oxychlorination treatment is carried out in an atmosphere containing water, oxygen and chlorine-containing gas;
[0031] The reduction treatment conditions include: a temperature of 450-650° C. and a time of 1-10 hours.
[0032] Optionally, the alumina support containing a Group IVA metal contains θ-alumina.
[0033] The second aspect of the present invention provides a low-carbon alkane dehydrogenation catalyst prepared by the method provided by the first aspect of the present invention.
[0034] The third aspect of the present invention provides a method for dehydrogenating low-carbon alkanes to produce olefins, the method comprising: contacting low-carbon alkanes with the catalyst provided by the second aspect of the present invention to carry out a dehydrogenation reaction.
[0035] Optionally, the conditions for the dehydrogenation reaction include: a temperature of 400-800°C, a pressure of 0.01-1.0 MPa, and a mass space velocity of 0.1-20 h -1 ;
[0036] The low carbon alkane is selected from C3-C5 alkanes, preferably propane, pentane, n-butane or isobutane.
[0037] In the preparation method of the present invention, HCl of a certain concentration and a weakly polar solvent with a boiling point of 40-99° C. are used in combination as an impregnation solvent, and an active component is impregnated on an alumina carrier containing a Group IVA metal to prepare a catalyst. A low-carbon alkane dehydrogenation catalyst with good active component dispersibility and high stability can be prepared, and the catalyst can be used in the process of dehydrogenating low-carbon olefins to produce propylene, and has good selectivity for the target product.
[0038] Other features and advantages of the present invention will be described in detail in the following detailed description. DETAILED DESCRIPTION
[0039] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0040] The first aspect of the present invention provides a method for preparing a light alkane dehydrogenation catalyst, the method comprising:
[0041] S1, contacting an alumina carrier containing a Group IVA metal with a first impregnation solution for first impregnation, taking out a solid after the first impregnation and performing a first calcination to obtain a first solid;
[0042] The first impregnation solution contains a Group VIII metal compound, HCl and a weak polar solvent with a boiling point of 40-99°C; the amount of HCl is 0.1-5 wt% based on the dry weight of the alumina carrier; the content of the weak polar solvent with a boiling point of 40-99°C is 5-99 wt% based on the total weight of HCl and the weak polar solvent with a boiling point of 40-99°C;
[0043] S2, contacting the first solid with a second impregnation solution for a second impregnation, taking out the solid after the second impregnation and performing a second calcination to obtain a second solid; wherein the second impregnation solution contains a Group IA metal compound;
[0044] S3, subjecting the second solid to oxychlorination treatment and reduction treatment in sequence.
[0045] According to the present invention, "based on the dry weight of the alumina carrier" in step S1 means that the weight of the Group IVA metal in the alumina carrier containing the Group IVA metal is removed, and only the dry weight of the alumina carrier is used as the basis. In the method of the present invention, a certain concentration of HCl and a weak polar solvent with a boiling point of 40-99°C are used as the impregnation solvent to impregnate the alumina carrier containing the Group IVA metal. In the impregnation step, a catalyst with good dispersion of active components is obtained, which is conducive to constructing more M2 active centers and making the Group VIII metal species (such as Pt species) with good redispersion performance more located near the Group IVA metal oxide (such as SnO2). Through the subsequent activation step, the Group VIII metal species (such as Pt species) with good dispersion but poor stability on the carrier can be migrated to the nearby Group IVA metal oxide (such as SnO2), further increasing the number of M2 active centers, while reducing the sintering and side reaction active centers of the Group VIII metal species on the carrier, thereby improving the stability of the catalyst. The prepared catalyst also has good selectivity for the target product when used in the dehydrogenation of light olefins to propylene.
[0046] In a specific embodiment of the present invention, in step S1, based on the dry weight of the alumina carrier, the amount of the Group VIII metal compound in the first impregnation solution is 0.1-1.0 wt%, preferably 0.1-0.5 wt%, and the amount of HCl in the first impregnation solution is 0.1-2.0 wt%, preferably 0.3-2.0 wt%, and more preferably 0.5-1.5 wt%.
[0047] In a specific embodiment of the present invention, based on the total weight of HCl and the weak polar solvent with a boiling point of 40-99° C., the content of the weak polar solvent with a boiling point of 40-99° C. is 15-85% by weight, more preferably 35-75% by weight, or preferably 20-30% by weight.
[0048] In a specific embodiment of the present invention, in step S1, the content of the Group IVA metal is 0.1-3.0 wt % based on the dry weight of the alumina carrier.
[0049] In a specific embodiment of the present invention, in step S1, the content of the Group IVA metal in the alumina carrier containing the Group IVA metal is 0.1-2.0 wt% based on the dry weight of the alumina carrier; the Group IVA metal is selected from tin and / or germanium.
[0050] In a specific embodiment of the present invention, in step S2, the amount of the second impregnation solution is 1.0-3.0 L, preferably 1.2-2.0 L, relative to 1 kg of the first solid; based on the dry weight of the alumina carrier, the amount of the Group IA metal compound in the second impregnation solution is 0.1-3.0 wt. % calculated as the Group IA metal.
[0051] In a specific embodiment of the present invention, the weak polar solvent with a boiling point of 40-99°C is selected from one or more aqueous solutions of C1-C5 fatty alcohols, ethyl acetate and acetone, and the C1-C5 fatty alcohols may include but are not limited to methanol, ethanol, propanol, n-butanol, isobutanol, n-pentanol, etc.; the Group VIII metal compound is selected from one or more of chloroplatinic acid, ammonium chloroplatinate and platinum chloride; the Group IA metal compound is selected from one or more of potassium hydroxide, lithium hydroxide, sodium hydroxide and cesium hydroxide.
[0052] According to the present invention, impregnation is a technical means conventionally adopted by those skilled in the art during the preparation of the catalyst, which refers to immersing the carrier in a solution containing an active component (and / or a co-catalyst). In a specific embodiment of the present invention, in step S1, the conditions for the first impregnation include: a temperature of 25-60°C and a time of 1-10 hours. Calcination is also a technical means conventionally adopted by those skilled in the art, for example, it can be carried out in a muffle furnace or a tubular furnace. The present invention does not limit the atmosphere for calcination, for example, it can be an air atmosphere. In one embodiment, the conditions for the first calcination include: a temperature of 450-600°C and a time of 1-10 hours, preferably, a temperature of 480-580°C and a time of 2-8 hours.
[0053] In a specific embodiment of the present invention, the conditions of the second impregnation include: temperature of 25-60°C, time of 1-10 hours; the conditions of the second calcination include: temperature of 450-650°C, time of 1-10 hours, preferably, temperature of 480-600°C, time of 2-8 hours.
[0054] According to the present invention, the oxychlorination treatment and reduction treatment of the catalyst are well known to those skilled in the art. In a specific embodiment of the present invention, the conditions of the oxychlorination treatment include: a temperature of 480-660° C. and a time of 1-10 hours. The oxychlorination treatment is carried out in an atmosphere containing water, oxygen and chlorine-containing gas, wherein the chlorine-containing gas may include but is not limited to hydrogen chloride, chloroform, tetrachloroethylene, dichloroethylene and carbon tetrachloride. The content of chlorine-containing gas in the atmosphere containing water, oxygen and chlorine-containing gas may be 0.0001-10% by volume, and the content of oxygen may be 0.0001-10% by volume.
[0055] In a specific embodiment of the present invention, the conditions of the reduction treatment include: a temperature of 450-650°C and a time of 1-10 hours, preferably a temperature of 460-560°C and a time of 1-6 hours. The reduction treatment is carried out in a reducing atmosphere, and the reducing atmosphere may contain a reducing gas such as hydrogen, or a mixture of hydrogen and an inert gas. Under the above conditions, the catalyst is subjected to oxychlorination and reduction treatment, which can achieve the migration of highly dispersed Group VIII metals (such as platinum) on the carrier to Group IVA metal oxides (such as tin oxide), and the interaction between Group VIII metals and Group IVA metal species is strengthened by reduction.
[0056] According to the present invention, the Group IVA metal in the alumina carrier containing the Group IVA metal is introduced during carrier molding. In a specific embodiment of the present invention, the aluminum sol containing the Group IVA metal compound is molded into a ball drop using an oil-ammonia column or a hot oil column to obtain an alumina wet ball containing the Group IVA metal compound, and the alumina wet ball containing the Group IVA metal compound is subjected to a third calcination at 450-1100°C to obtain an alumina carrier containing the Group IVA metal. In one embodiment, the wet ball obtained by the ball drop molding is dried, and then calcined at 450-650°C to make the alumina in the carrier ball γ-Al2O3, and then calcined at 900-1100°C, and the calcination time is preferably 1-20 hours, and finally a θ-alumina carrier containing the Group IVA metal can be prepared. Preferably, the γ-Al2O3 is treated with air containing 2-10 volume % of water at 450-650°C for 2-8 hours, and then calcined at 900-1100°C for 2-8 hours.
[0057] Among them, the oil-ammonia column or hot oil column drop ball forming is a method well known to those skilled in the art.
[0058] In a specific embodiment, the method for preparing the aluminum sol used for the drop ball can be to react aluminum chloride and ammonia water at a temperature of 50-90°C, preferably 50-80°C, then filter and wash with water, and add an acid solution to the filter cake to form an aluminum sol; or directly add water to aluminum hydroxide powder to form a slurry, and then add acid to the slurry to form an aluminum sol. The acid used is preferably nitric acid or hydrochloric acid, and an organic acid such as acetic acid or citric acid can also be added. If preparing alumina containing macropores, it is necessary to add an appropriate amount of urea, kerosene, fatty alcohol polyoxyethylene ether and other pore-enlarging agents to the aluminum sol.
[0059] According to the present invention, the Group IVA metal in the alumina carrier containing the Group IVA metal is introduced by impregnation or ion exchange after the carrier is formed. In a specific embodiment of the present invention, the alumina carrier is contacted with a third impregnation solution containing a Group IVA metal compound for a third impregnation, and the solid product after the third impregnation is taken out and subjected to a fourth calcination at 500-630°C. Preferably, the alumina carrier has a carbon content of 50-160 m 2 / g and a specific surface area of 0.1-1.0cm 3 The alumina carrier can be prepared by a sol-gel method, a coprecipitation method or a hydrothermal synthesis method, or directly using metal oxides.
[0060] According to the present invention, the Group IVA metal compound is selected from one or more of tin chlorides, bromides, nitrates, alkoxides and organic complexes; preferably, the Group IVA metal compound is selected from one or more of stannous bromide, stannous chloride, tin tetrachloride, tin tetrachloride pentahydrate and tetrabutyltin.
[0061] In one embodiment of the present invention, the alumina support containing a Group IVA metal contains θ-alumina.
[0062] The second aspect of the present invention provides a low-carbon alkane dehydrogenation catalyst prepared by the method provided by the first aspect of the present invention.
[0063] In a specific embodiment of the present invention, the low-carbon alkane dehydrogenation catalyst contains an alumina carrier and an active component, wherein the active component contains 0.1-5 wt. % of Group VIII metal, 0.1-3 wt. % of Group IVA metal, 0.1-3 wt. % of Group IA metal, and 0.1-3 wt. % of Group VIIA element, based on the dry weight of the alumina carrier; preferably, the active component contains 0.1-0.5 wt. % of Group VIII metal, 0.1-1.5 wt. % of Group IVA metal, 0.1-1.5 wt. % of Group IA metal, and 0.1-1.5 wt. % of Group VIIA element, based on the dry weight of the alumina carrier.
[0064] The third aspect of the present invention provides a method for dehydrogenating low-carbon alkanes to produce olefins, the method comprising: contacting low-carbon alkanes with the catalyst provided by the second aspect of the present invention to carry out a dehydrogenation reaction.
[0065] In a specific embodiment of the present invention, the conditions of the dehydrogenation reaction include: a temperature of 400-800°C, a pressure (absolute pressure) of 0.01-1.0 MPa, preferably, a temperature of 550-650°C, a pressure of 0.01-0.3 MPa; a mass space velocity of light alkanes of 0.1-20 h -1, preferably 0.5 to 10 hours -1 The low carbon alkane is selected from C3 to C5 alkanes, preferably propane, pentane, n-butane or isobutane.
[0066] In a specific embodiment of the present invention, water vapor, argon, methane, ethane, carbon dioxide, nitrogen, etc. can also be used as diluent gas for the dehydrogenation reaction and mixed with the low carbon alkane and introduced into the reactor, preferably the diluent gas is hydrogen. When hydrogen is selected, the molar ratio of hydrogen to low carbon alkane is preferably (0.1-10):1, more preferably (0.3-3):1.
[0067] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.
[0068] The raw materials used in the following examples and comparative examples were commercially available unless otherwise specified. The alumina carrier was produced by Sasol of Germany and had a specific surface area of 120 m 2 / g, and the pore volume is 0.65 ml / g.
[0069] The catalyst compositions of the embodiments and comparative examples were detected by ICP-OES method.
[0070] The Sn-containing θ-alumina carrier 1 used in Examples 1-6 was prepared by an impregnation method: the alumina carrier 1 was contacted and impregnated with an impregnation solution having a tin element concentration of 0.35 wt% at a liquid-to-solid ratio of 2.0 mL / g, and the impregnated solid was taken out and calcined at 650°C for 5 hours to obtain a Sn-containing θ-alumina carrier, wherein the Sn content was 0.35 wt% based on the dry basis weight of the alumina carrier.
[0071] The preparation method of the Sn-containing θ-alumina carrier 2 used in Example 5 is similar to the preparation method of the Sn-containing θ-alumina carrier 1, with the only difference being that the impregnation solution used is an impregnation solution with a tin element concentration of 2.2 wt%. Based on the dry weight of the alumina carrier, the Sn content is 2.2 wt%.
[0072] Example 1
[0073] S1. Take a spherical Sn-containing θ-alumina carrier 1, impregnate it with an impregnation solution containing chloroplatinic acid, hydrochloric acid and ethanol at 40°C for 2 hours, dry the solid at 100°C for 12 hours after impregnation, and then calcine it at 550°C for 4 hours to obtain a first solid.
[0074] Among them, ethanol in the impregnation solution accounts for 55 weight% of the total mass of hydrochloric acid and ethanol; based on the dry weight of the alumina carrier, the amount of hydrochloric acid used is 1.2 weight%, and the amount of chloroplatinic acid in the impregnation solution calculated as platinum is 0.35 weight%.
[0075] S2. The first solid is immersed in a potassium hydroxide solution at 40°C for 2 hours. After the immersed solid is dried at 100°C for 12 hours, it is calcined at 600°C for 2 hours to obtain a second solid.
[0076] The potassium hydroxide solution contained 1.3% potassium hydroxide by weight based on the dry weight of the alumina support, and the liquid / solid ratio was 2.0 mL / g. The second solid contained 0.35% platinum, 0.8% chlorine, and 1.3% potassium.
[0077] S3. The second solid product was subjected to oxychlorination treatment at 550° C. for 6 hours in an atmosphere containing water, oxygen and carbon tetrachloride, and then subjected to reduction treatment at 550° C. for 2 hours to obtain Catalyst A. Based on the dry weight of the alumina carrier, the catalyst contained 0.35% by weight of platinum, 0.35% by weight of tin, 1.4% by weight of potassium and 1.3% by weight of chlorine. The evaluation results are shown in Table 1.
[0078] Example 2
[0079] Catalyst B was prepared by the same method as in Example 1, except that in step S1, ethanol accounted for 25 weight % of the total mass of hydrochloric acid and ethanol.
[0080] The catalyst contained 0.35 wt% platinum, 0.35 wt% tin, 1.4 wt% potassium and 1.3 wt% chlorine based on the dry weight of the alumina carrier. The evaluation results are shown in Table 1.
[0081] Example 3
[0082] Catalyst C was prepared by the same method as in Example 1, except that in step S1, ethanol accounted for 85 weight % of the total mass of hydrochloric acid and ethanol.
[0083] The catalyst contained 0.35 wt% platinum, 0.35 wt% tin, 1.4 wt% potassium and 1.3 wt% chlorine based on the dry weight of the alumina carrier. The evaluation results are shown in Table 1.
[0084] Example 4
[0085] Catalyst D was prepared by the same method as in Example 1, except that in step S1, the amount of hydrochloric acid used was 2.2 wt % based on the dry weight of the alumina carrier.
[0086] The catalyst contained 0.35 wt% platinum, 0.35 wt% tin, 1.4 wt% potassium and 1.6 wt% chlorine based on the dry weight of the alumina carrier. The evaluation results are shown in Table 1.
[0087] Comparative Example 1
[0088] Catalyst DA was prepared by the same method as in Example 1, except that the impregnation solution in step S1 did not contain ethanol.
[0089] The catalyst contained 0.35 wt% platinum, 0.35 wt% tin, 1.4 wt% potassium and 1.3 wt% chlorine based on the dry weight of the alumina carrier. The evaluation results are shown in Table 1.
[0090] Comparative Example 2
[0091] Catalyst DB was prepared by the same method as in Example 1, except that in step S1, the θ-alumina carrier was impregnated with an impregnation solution containing chloroplatinic acid, stannous chloride, hydrochloric acid and ethanol at 40°C for 2 hours, the solid was dried at 100°C for 12 hours after impregnation, and then calcined at 550°C for 4 hours to obtain a first solid, and the amount of stannous chloride in the impregnation solution was 0.35% by weight, calculated as tin.
[0092] The catalyst contained 0.35 wt% platinum, 0.35 wt% tin, 1.4 wt% potassium and 1.3 wt% chlorine based on the dry weight of the alumina carrier. The evaluation results are shown in Table 1.
[0093] Test Case
[0094] In the microreactor, 2 mL of catalyst was loaded, and a mixture of hydrogen and propane was used as the raw material. The reaction temperature was 615 °C, 0.21 MPa (absolute pressure), and the propane feed mass space velocity was 9.0 h -1 The reaction was carried out for 16 hours under the condition of a hydrogen / propane molar ratio of 0.33:1. Samples were taken every hour for chromatographic analysis. The propane conversion rate and propylene selectivity were calculated and the deactivation rate constant (kd, h -1 ) to evaluate catalyst stability, deactivation rate constant (kd, h -1 ) is calculated by the following equation. initial and X final are the propane conversion rates at the beginning and end of the reaction, respectively, and t is the reaction time. The results are shown in Table 1.
[0095]
[0096] Table 1
[0097]
[0098] It can be seen from Table 1 that the low-carbon alkane dehydrogenation catalyst prepared by the method of the present invention has better catalyst stability and at the same time maintains good selectivity to propylene.
[0099] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, a variety of simple modifications can be made to the technical solution of the present invention, and these simple modifications all belong to the protection scope of the present invention.
[0100] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0101] In addition, various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.
Claims
1. A method for preparing a catalyst for dehydrogenation of light alkanes, the method comprising: include: S1, contacting an alumina carrier containing a Group IVA metal with a first impregnation solution for first impregnation, taking out a solid after the first impregnation and performing a first calcination to obtain a first solid; The first impregnation solution contains a Group VIII metal compound, HCl and a boiling point of 40-99 o C of weakly polar solvent; based on the dry weight of the alumina carrier, the amount of HCl is 0.1-5% by weight; HCl and boiling point of 40-99 o The total weight of the weak polar solvent of C is taken as the basis, and the boiling point is 40-99 o The content of the weak polar solvent of C is 5-99% by weight; S2, contacting the first solid with a second impregnation solution for a second impregnation, taking out the solid after the second impregnation and performing a second calcination to obtain a second solid; wherein the second impregnation solution contains a Group IA metal compound; S3, subjecting the second solid to oxychlorination treatment and reduction treatment in sequence.
2. The method according to claim 1, in, In step S1, based on the dry weight of the alumina support, the amount of the Group VIII metal compound in the first impregnation solution is 0.1-1.0 wt % in terms of the Group VIII metal, and the amount of HCl in the first impregnation solution is 0.1-2.0 wt %.
3. The method according to claim 1, in, With HCl and boiling point of 40-99 o The total weight of the weak polar solvent of C is taken as the basis, and the boiling point is 40-99 o The content of the weakly polar solvent in C is 15-85% by weight.
4. The method according to claim 1, in, In step S1, the content of the Group IVA metal is 0.1-3.0 wt % based on the dry weight of the alumina carrier.
5. The method according to claim 1, in, In step S1, the content of the Group IVA metal in the alumina support containing the Group IVA metal is 0.1-2.0% by weight based on the dry weight of the alumina support; The Group IVA metal is tin and / or germanium.
6. The method according to claim 1, in, In step S2, the amount of the second impregnation liquid is 1.0-3.0 L relative to 1 kg of the first solid; The content of the Group IA metal compound in the second impregnation solution is 0.1-3.0 wt % calculated as the Group IA metal, based on the dry weight of the alumina support.
7. The method according to claim 1, in, The boiling point is 40-99 o The weakly polar solvent C is selected from one or more aqueous solutions of C1-C5 fatty alcohol, ethyl acetate and acetone; The Group VIII metal compound is selected from one or more of chloroplatinic acid, ammonium chloroplatinate and platinum chloride; The Group IA metal compound is selected from one or more of potassium hydroxide, lithium hydroxide, sodium hydroxide and cesium hydroxide.
8. The method according to claim 1, in, The conditions of the first impregnation include: a temperature of 25-60° C. and a time of 1-10 hours; The first calcination conditions include: a temperature of 450-600° C. and a time of 1-10 hours; The conditions of the second impregnation include: a temperature of 25-60°C and a time of 1-10 hours; The second calcination conditions include: a temperature of 450-650° C. and a time of 1-10 hours; The conditions of the oxychlorination treatment include: a temperature of 480-660° C., a time of 1-10 hours, and the oxychlorination treatment is carried out in an atmosphere containing water, oxygen and chlorine-containing gas; The reduction treatment conditions include: a temperature of 450-650° C. and a time of 1-10 hours.
9. The method according to claim 1, in, The alumina support containing a Group IVA metal contains θ-alumina.
10. A light alkane dehydrogenation catalyst prepared by the method according to any one of claims 1 to 9.
11. A method for dehydrogenating low-carbon alkanes to produce olefins, the method comprising: include: A dehydrogenation reaction is carried out by contacting a low carbon alkane with the catalyst according to claim 10.
12. The method according to claim 11, in, The conditions of the dehydrogenation reaction include: temperature of 400-800°C, pressure of 0.01-1.0 MPa, mass space velocity of light alkanes of 0.1-20 h -1 ; The low carbon alkane is selected from C 3 ~C 5 of alkanes.
13. The method according to claim 12, in, The low carbon alkane is selected from propane, pentane, n-butane or isobutane.
Citation Information
Cited By
Metal self-dispersed low-carbon alkane dehydrogenation catalyst as well as preparation method and application thereof
CN120079417A