A method for starting up a wax oil hydrogenation unit
By using NO gas reduction catalyst in the wax oil hydrogenation device and increasing the end point temperature of the vulcanization, the problem of poor catalyst stability is solved, the device operation cycle is extended and the start-up process is simplified.
Patent Information
- Application Number
- CN202111271812.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-10-29
AI Technical Summary
The existing wax oil hydrogenation device has poor catalyst stability when treating low-sulfur wax oil, resulting in a short operating cycle of the device and is unable to operate stably for a long time.
The catalyst is moderately reduced by NO gas, the action force between the metal and the support is increased, and the catalyst is highly vulcanized by increasing the end point temperature of the vulcanization, and the device operation cycle is extended. The specific steps include controlling the volume flow rate of circulating hydrogen and the NO gas injection rate in the starting method, gradually increasing the reaction zone temperature, performing hydrogen replacement and vulcanization, and ensuring efficient vulcanization of the catalyst.
It improves the catalyst's sulfur loss resistance, extends the operation cycle of the device, simplifies the start-up process, and reduces the product adjustment time.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of wax oil hydrogenation, and in particular to a start-up method of a wax oil hydrogenation device. Background Art
[0002] Wax oil hydroprocessing technology was first applied in the 1970s. The original purpose was to produce low-sulfur fuel oil and reduce the sulfide emissions of the FCC unit regenerator to meet environmental regulations. In recent years, people have realized that nitrogen and aromatics in FCC feed are key factors affecting the efficiency of FCC units. Reducing the nitrogen and aromatic content of the feed can increase the gasoline yield of the unit, improve the stability of the catalyst, extend the unit operation cycle, and increase corporate benefits.
[0003] At present, China has more than ten sets of wax oil hydroprocessing industrial units in operation, and the technologies used are mainly provided by the two research institutes of FRIPP and RIPP under Sinopec. Although wax oil hydroprocessing technology can meet the production needs of enterprises to a certain extent, and the main catalyst technology and process technology level of wax oil hydroprocessing have fully reached the level of similar foreign technologies, in recent years, with the obvious trend of heavy and inferior crude oil, increasingly stringent environmental protection regulations, and accelerated upgrading of oil quality, the deficiencies and problems of processes and catalysts have gradually emerged in the production process and need to be solved urgently. The most obvious feature of China's wax oil composition that is different from that of foreign countries is that it has low sulfur and high nitrogen. When the wax oil hydroprocessing unit processes such raw oil for a long time, the catalyst is prone to sulfur loss, which seriously affects the stability of the catalyst and the operation cycle of the unit.
[0004] There are many reports on the start-up methods of wax oil hydrogenation units, but there are few reports on the start-up methods for improving the stability of wax oil hydrogenation units.
[0005] CN112742427A discloses a method for starting a hydrogenation catalyst, wherein the hydrogenation catalyst carrier is mixed with a thiomolybdate and / or thiotungstate solution, a nickel salt and / or a cobalt salt solution, respectively, and dried to obtain an intermediate hydrogenation catalyst; then a sulfiding agent is mixed evenly with the intermediate hydrogenation catalyst obtained above, and a phosphorus-containing substance is added; the material is dried to obtain a presulfurized catalyst; and the catalyst is loaded into a hydrogenation reactor and started. This method can solve the problem of high initial activity of the catalyst and poor safety.
[0006] CN111068795A discloses an off-site presulfurization method for a hydrogenation catalyst, in which a sulfiding agent is mixed evenly with an oxidized hydrogenation catalyst, and then heat-treated, and further supplemented with a material containing hydrogen sulfide for sulfurization. After hydrogen sulfide sulfurization, the intermediate material is loaded with excessive hydrocarbon oil to obtain a deeply sulfurized presulfurized catalyst. This method can effectively shorten the sulfurization start-up time.
[0007] The above existing technologies, when starting up, use off-site pre-sulfurization to save sulfurization time, and also directly develop sulfurized hydrogenation catalysts. However, none of them solves the problem that the hydrogenation unit cannot operate stably for a long period of time due to low hydrogen sulfide concentration and poor catalyst stability in the low-sulfur wax oil hydrogenation unit. Summary of the invention
[0008] In view of the shortcomings of the prior art, the present invention provides a start-up method for a wax oil hydrogenation device. The start-up method of the present invention can improve the stability of the catalyst and extend the operation period of the device.
[0009] The invention provides a start-up method for a wax oil hydrogenation device, comprising: after completing catalyst loading, air tightness inspection and establishment of a circulating hydrogen system for the wax oil hydrogenation device, controlling the hourly volume flow rate of circulating hydrogen to be 100 to 800 times of the total catalyst loading volume, injecting NO gas into the inlet of a reaction zone of the wax oil hydrogenation device, wherein the volume injection rate of NO is 10% to 30% of the volume flow rate of circulating hydrogen, raising the inlet temperature of the reaction zone to 200 to 240° C., stopping the injection of NO gas when the volume fraction of NO2 in the circulating hydrogen is 5% to 30%, then sequentially performing hydrogen replacement and sulfurization, and introducing raw oil for normal production after the sulfurization is completed.
[0010] Furthermore, the volumetric injection rate of NO is 10% to 30% of the volumetric flow rate of circulating hydrogen, wherein the volumetric injection rate of NO and the volumetric flow rate of circulating hydrogen are both measured in hours.
[0011] Furthermore, the process of the air tightness inspection and establishment of the circulating hydrogen system is carried out by conventional methods in the art, and there is no particular limitation in the present invention. After the air tightness inspection and establishment of the circulating hydrogen system, the high pressure is controlled to the design pressure, which is generally 5.0 to 10.0 MPa.
[0012] Furthermore, the hydrogen replacement is completed when the hydrogen gas volume fraction in the circulating hydrogen is adjusted to 95% to 99%. The hydrogen replacement process can introduce new hydrogen into the circulating hydrogen, and introduce a wax oil hydrogenation device at the entrance of the reaction zone to replace the gas in the system until the hydrogen gas volume fraction in the circulating hydrogen reaches 95% to 99%, and the hydrogen replacement is completed.
[0013] Furthermore, before hydrogen replacement, the inlet temperature of the reaction zone may be lowered to 150-170° C., and then hydrogen replacement may be performed.
[0014] Furthermore, the vulcanization process adopts wet vulcanization or dry vulcanization, preferably dry vulcanization.
[0015] Furthermore, the dry sulfidation includes a first sulfidation stage and a second sulfidation stage, wherein the first sulfidation stage is to increase the inlet temperature of the reaction zone to a first constant temperature of 230 to 250°C at a heating rate of ≯10°C / h, preferably 3 to 10°C / h, and then maintain the temperature at the first constant temperature for 4 to 10 hours. In the first sulfidation stage, the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 1000 to 5000 ppm; the second sulfidation stage is to increase the inlet temperature of the reaction zone to a second constant temperature of 350 to 390°C at a heating rate of ≯10°C / h, preferably 3 to 10°C / h, and the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to reach 5000 to 10000 ppm during the heating period, and then maintain the temperature at the second constant temperature for 2 to 6 hours. During the second constant temperature period, the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to reach 10000 to 20000 ppm.
[0016] Furthermore, in the dry sulfurization, before entering the first sulfurization stage, a sulfurizing agent is gradually injected into the wax oil hydrogenation unit, and the temperature is gradually increased and the catalyst bed temperature in the reaction zone is controlled not to exceed 230°C until hydrogen sulfide penetrates the entire catalyst bed; preferably, the conditions for hydrogen sulfide to penetrate the entire catalyst bed are as follows: the mass concentration of hydrogen sulfide in the circulating hydrogen reaches more than 1000ppm, and more preferably 1000-10000pm.
[0017] Further, the catalyst comprises a hydrorefining catalyst. The reaction zone is filled with a hydrorefining catalyst. The hydrorefining catalyst comprises a hydrogenation active metal component, a carrier and a binder. The hydrogenation active metal comprises at least one of a Group VIB metal (such as tungsten and / or molybdenum) and a Group VIII metal (such as nickel and / or cobalt); the carrier comprises at least one of alumina, silicon oxide and amorphous silicon aluminum; the binder is alumina and / or silicon oxide. Based on the weight of the catalyst, the content of the Group VIB metal oxide is 15% to 35%, preferably 18% to 30%, and the content of the Group VIII metal oxide is 2% to 10%, preferably 4% to 8%. The hydrorefining catalyst can be prepared according to existing methods, or an industrial catalyst can be used, such as FF-34, FF-24, FF-14 and FF-66 developed by Dalian Petrochemical Research Institute.
[0018] Furthermore, the vulcanizing agent is a commonly used vulcanizing agent in industry and / or an environmentally friendly vulcanizing agent. The commonly used vulcanizing agent in industry is at least one of dimethyl disulfide (DMDS) and carbon disulfide (CS2) commonly used in industry.
[0019] Furthermore, the feedstock oil is selected from low-sulfur wax oil, the initial distillation point of the feedstock oil is 300-400°C, the final distillation point is 550-650°C, the sulfur mass content is below 5000ppm, and the nitrogen mass content is 1500-4000ppm.
[0020] Furthermore, the specific operation of introducing the crude oil is as follows: lowering the inlet temperature of the reaction zone to 280-320° C., starting to introduce the crude oil, the initial introduction amount is 20%-40% of the designed processing load, and after stabilization, the crude oil feed amount is adjusted to 60%-100%. Adjust the reaction temperature until the wax oil product quality is qualified.
[0021] Furthermore, during the normal production, the reaction conditions are as follows:
[0022] The reaction pressure is 5.0~10.0MPa, the reaction temperature is 280~410℃, and the volume space velocity of hydrogenation refining liquid is 0.5~6.0h -1 Preferably, the reaction pressure is 6.0-8.0 MPa, the reaction temperature is 340-400°C, and the volume space velocity during hydrogenation of the refined liquid is 0.6-2.0 h -1 .
[0023] Furthermore, after the feedstock oil is mixed with hydrogen, it contacts with a catalyst in a hydrorefining reaction zone to undergo desulfurization, denitrogenation and dearomatization reactions, and the resulting hydrorefining effluent passes through a separation system to obtain a wax oil product.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] (1) The start-up method of the present invention uses NO gas as a reducing gas before the start of the sulfurization of the wax oil hydrogenation catalyst, firstly appropriately reduces the catalyst, thereby increasing the interaction between the metal and the carrier and reducing some of the hexacoordinated active metals in the catalyst with high hydrogenation activity but poor stability to tetracoordinated active metals with good stability. Subsequently, by increasing the sulfurization endpoint temperature, the purpose of highly sulfurized catalyst is finally achieved, thereby improving the catalyst's ability to resist desulfurization and extending the device operation cycle.
[0026] (2) The start-up process involved in the start-up method of the present invention is simple and controllable, there is no risk of temperature runaway, and the product adjustment time is short. DETAILED DESCRIPTION
[0027] The start-up method provided by the present invention will be further described below in conjunction with embodiments to compare and reflect the effects and advantages of the start-up method of the present invention, but the present invention is not limited thereto.
[0028] In the present invention, unless otherwise specified, percentages refer to mass fractions.
[0029] The feedstock oil involved in the following examples and comparative examples is low sulfur wax oil, and its properties are shown in Table 1. The main physical properties of various catalysts are shown in Table 2. The refining reactor in the examples and comparative examples is filled with FF-34 hydrorefining catalyst, and the main evaluation conditions are shown in Table 3. The evaluation effect ratio of the examples is shown in Table 4, and the evaluation effect ratio of the comparative examples is shown in Table 5.
[0030] Example 1
[0031] After completing the catalyst loading, air tightness inspection and establishment of the circulating hydrogen system for the wax oil hydrogenation unit, the high-pressure is controlled to the design pressure (7MPa), the hourly volume flow rate of circulating hydrogen is controlled to 400 times the total catalyst loading volume, NO gas is injected into the reaction zone inlet, and the volume injection rate of NO is 10% of the circulating hydrogen volume flow rate. The reaction zone inlet temperature is increased to 200°C. When the volume fraction of NO2 in the circulating hydrogen is 15%, the introduction of NO gas is stopped, and the reaction zone inlet temperature is reduced to 170°C.
[0032] New hydrogen begins to be introduced into the circulating hydrogen and is passed from the reaction zone into the wax oil hydrogenation unit to replace the gas in the reaction system. When the hydrogen gas volume fraction in the circulating hydrogen reaches 98%, the hydrogen replacement is completed.
[0033] Start the sulfur injection pump and gradually inject the sulfiding agent DMDS into the reaction zone. Gradually increase the temperature and control the catalyst bed temperature in the reaction zone not to exceed 230°C, until the mass concentration of hydrogen sulfide in the circulating hydrogen is maintained at more than 1000ppm and the hydrogen sulfide penetrates the catalyst bed. Then enter the first sulfidation stage and increase the inlet temperature of the reaction zone to 230°C at a rate of 5°C / h. Constant temperature sulfidation is carried out for 8 hours, during which the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 2000-3000ppm.
[0034] After the constant temperature of 230℃, the second sulfurization stage begins, and the inlet temperature of the reaction zone is steadily increased to 360℃ at a rate of 5℃ / h, during which the concentration of hydrogen sulfide is controlled to be 5000-10000ppm. The constant temperature sulfurization is carried out at 360℃ for 5h, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 10000-15000ppm.
[0035] After the 360°C constant temperature was completed, the inlet temperature of the reaction zone was lowered to 300°C, and the crude oil was introduced, with the initial introduction amount being 30% of the designed processing load. After stabilization, the crude oil feed amount was adjusted to 80% of the designed processing load. Subsequently, the reaction temperature was adjusted, and the product was produced according to the conditions in Table 3 and the catalyst was evaluated over a long period of time.
[0036] Example 2
[0037] After completing the catalyst loading, air tightness inspection and establishment of the circulating hydrogen system for the wax oil hydrogenation unit, the high-pressure is controlled to the design pressure (7MPa), the hourly volume flow rate of circulating hydrogen is controlled to 600 times the total catalyst loading volume, NO gas is injected into the reaction zone inlet, and the volume injection rate of NO is 15% of the circulating hydrogen volume flow rate. The reaction zone inlet temperature is increased to 210°C. When the volume fraction of NO2 in the circulating hydrogen is 20%, the introduction of NO gas is stopped, and the reaction zone inlet temperature is reduced to 170°C.
[0038] New hydrogen begins to be introduced into the circulating hydrogen and is passed from the reaction zone into the wax oil hydrogenation unit to replace the gas in the reaction system. When the hydrogen gas volume fraction in the circulating hydrogen reaches 97%, the hydrogen replacement is completed.
[0039] Start the sulfur injection pump and gradually inject the sulfiding agent DMDS into the reaction zone. Gradually increase the temperature and control the catalyst bed temperature in the reaction zone not to exceed 230°C, until the mass concentration of hydrogen sulfide in the circulating hydrogen is maintained at more than 1000ppm and the hydrogen sulfide penetrates the catalyst bed. Increase the inlet temperature of the reaction zone to 250°C at a rate of 5°C / h. Keep the sulfiding at a constant temperature for 10 hours, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 4000-5000ppm.
[0040] After the constant temperature of 250℃, the second sulfurization stage begins, and the inlet temperature of the reaction zone is steadily increased to 360℃ at a rate of 8℃ / h, during which the hydrogen sulfide concentration is controlled to be 6000-8000ppm. The constant temperature sulfurization is carried out at 360℃ for 3h, during which the hydrogen sulfide concentration in the circulating hydrogen is controlled to be maintained at 13000-15000ppm.
[0041] After the constant temperature of 360°C was completed, the inlet temperature of the reaction zone was lowered to 320°C, and the feedstock oil was introduced, with the initial introduction amount being 35% of the designed processing load. After stabilization, the feedstock oil feed amount was adjusted to 70% of the designed processing load. Subsequently, the reaction temperature was adjusted, and the product was produced according to the conditions in Table 3 and the catalyst was evaluated over a long period of time.
[0042] Example 3
[0043] After the wax oil hydrogenation unit is completed with catalyst loading, air tightness inspection, and establishment of the circulating hydrogen system, the high pressure is controlled to the design pressure (7MPa), the hourly volume flow rate of circulating hydrogen is controlled to 800 times the total catalyst loading volume, and NO gas is injected into the inlet of the reaction zone, and the volume injection rate of NO is 30% of the volume flow rate of circulating hydrogen. The inlet temperature of the reaction zone is increased to 200°C. When the volume fraction of NO2 in the circulating hydrogen is 30%, the introduction of NO gas is stopped, and the inlet temperature of the reaction zone is reduced to 150°C.
[0044] New hydrogen begins to be introduced into the circulating hydrogen and is passed from the reaction zone into the wax oil hydrogenation unit to replace the gas in the reaction system. When the hydrogen gas volume fraction in the circulating hydrogen reaches 98%, the hydrogen replacement is completed.
[0045] Start the sulfur injection pump and gradually inject the sulfiding agent DMDS into the reaction zone. Gradually increase the temperature and control the catalyst bed temperature in the reaction zone not to exceed 230°C, until the mass concentration of hydrogen sulfide in the circulating hydrogen is maintained at above 2000ppm and the hydrogen sulfide penetrates the catalyst bed. Then enter the first sulfidation stage and increase the inlet temperature of the reaction zone to 240°C at a rate of 7°C / h. Constant temperature sulfidation is carried out for 8 hours, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 3000-4000ppm.
[0046] After the constant temperature of 240℃, the second sulfurization stage begins, and the inlet temperature of the reaction zone is steadily increased to 360℃ at a rate of 8℃ / h, during which the hydrogen sulfide concentration is controlled to be 7000-9000ppm. The constant temperature sulfurization is carried out at 360℃ for 4h, during which the hydrogen sulfide concentration in the circulating hydrogen is controlled to be maintained at 12000-14000ppm.
[0047] After the 360°C constant temperature was completed, the inlet temperature of the reaction zone was lowered to 310°C, and the crude oil was introduced, with the initial introduction amount being 40% of the designed processing load. After stabilization, the crude oil feed amount was adjusted to 95% of the designed processing load. Subsequently, the reaction temperature was adjusted, and the product was produced according to the conditions in Table 3 and the catalyst was evaluated over a long period of time.
[0048] Example 4
[0049] After the catalyst loading, air tightness inspection and establishment of the circulating hydrogen system of the wax oil hydrogenation unit are completed, the high pressure is controlled to the design pressure (7MPa), the hourly volume flow rate of circulating hydrogen is controlled to 500 times the total catalyst loading volume, and NO gas is injected into the inlet of the reaction zone, and the volume injection rate of NO is 15% of the volume flow rate of circulating hydrogen. The inlet temperature of the reaction zone is increased to 210°C. When the volume fraction of NO2 in the circulating hydrogen is 15%, the introduction of NO gas is stopped, and the inlet temperature of the reaction zone is reduced to 160°C.
[0050] New hydrogen begins to be introduced into the circulating hydrogen and is passed from the reaction zone into the wax oil hydrogenation unit to replace the gas in the reaction system. When the hydrogen gas volume fraction in the circulating hydrogen reaches 99%, the hydrogen replacement is completed.
[0051] Start the sulfur injection pump and gradually inject the sulfiding agent DMDS into the reaction zone. Gradually increase the temperature and control the catalyst bed temperature in the reaction zone not to exceed 230°C, until the mass concentration of hydrogen sulfide in the circulating hydrogen is maintained at above 3000ppm and the hydrogen sulfide penetrates the catalyst bed. Then enter the first sulfidation stage and increase the inlet temperature of the reaction zone to 235°C at a rate of 7°C / h. Constant temperature sulfidation is carried out for 10 hours, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 3000-4000ppm.
[0052] After the constant temperature of 235℃, the second sulfurization stage was entered, and the inlet temperature of the reaction zone was steadily increased to 390℃ at a rate of 9℃ / h, during which the hydrogen sulfide concentration was controlled to be 8000-10000ppm. The constant temperature sulfurization was carried out at 390℃ for 6h, during which the hydrogen sulfide concentration in the circulating hydrogen was controlled to be maintained at 14000-15000ppm.
[0053] After the constant temperature at 390°C was completed, the inlet temperature of the reaction zone was lowered to 310°C, and the crude oil was introduced, with the initial introduction amount being 25% of the designed processing load. After stabilization, the crude oil feed amount was adjusted to 95% of the designed processing load. Subsequently, the reaction temperature was adjusted, and the product was produced according to the conditions in Table 3 and the catalyst was evaluated over a long period of time.
[0054] Comparative Example 1
[0055] After completing the catalyst loading, air tightness inspection and establishment of the circulating hydrogen system for the wax oil hydrogenation unit, the high-pressure is controlled to the design pressure (7MPa), the hourly volume flow rate of circulating hydrogen is controlled to 400 times the total catalyst loading volume, and the inlet temperature of the reaction zone is controlled to 170°C.
[0056] The sulfiding agent DMDS is gradually injected into the reaction zone through a high-pressure sulfur injection pump, and the temperature is gradually increased and the catalyst bed temperature in the reaction zone is controlled not to exceed 230°C, until the mass concentration of hydrogen sulfide in the circulating hydrogen is maintained at more than 1000ppm, and the hydrogen sulfide penetrates the catalyst bed. Then, the first sulfidation stage is entered, and the inlet temperature of the reaction zone is increased to 230°C at a rate of 5°C / h. Constant temperature sulfidation is carried out for 8 hours, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 2000-3000ppm.
[0057] After the constant temperature at 230°C is completed, the inlet temperature of the reaction zone is steadily increased to 360°C at a rate of 5°C / h, during which the concentration of hydrogen sulfide is controlled to be 5000-10000ppm. Constant temperature sulfidation is performed at 360°C for 5h, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 10000-15000ppm.
[0058] After the 360°C constant temperature was completed, the inlet temperature of the reaction zone was lowered to 300°C, and the feedstock oil was introduced, with the initial introduction amount being 30% load. After stabilization, the feedstock oil feed amount was adjusted to 80% load. Subsequently, the reaction temperature was adjusted, and the product was produced and the catalyst was evaluated over a long period of time according to the conditions in Table 3.
[0059] Comparative Example 2
[0060] After the catalyst loading, air tightness inspection and establishment of the circulating hydrogen system of the wax oil hydrogenation unit are completed, the high pressure is controlled to the design pressure (7MPa), and the hourly volume flow rate of circulating hydrogen is controlled to 400 times the total catalyst loading volume. The inlet temperature of the reaction zone is increased to 270°C. When the volume of water generated by the high pressure separator is 10% of the catalyst loading amount, measured by volume, the inlet temperature of the reaction zone is reduced to 170°C.
[0061] The sulfiding agent DMDS is gradually injected into the reaction zone through a high-pressure sulfur injection pump, and the temperature is gradually increased and the catalyst bed temperature in the reaction zone is controlled not to exceed 230°C, until the mass concentration of hydrogen sulfide in the circulating hydrogen is maintained at more than 1000ppm, and the hydrogen sulfide penetrates the catalyst bed. Then, the first sulfidation stage is entered, and the inlet temperature of the reaction zone is increased to 230°C at a rate of 5°C / h. Constant temperature sulfidation is carried out for 8 hours, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 2000-3000ppm.
[0062] After the constant temperature at 230°C is completed, the inlet temperature of the reaction zone is steadily increased to 360°C at a rate of 5°C / h, during which the concentration of hydrogen sulfide is controlled to be 5000-10000ppm. Constant temperature sulfidation is performed at 360°C for 5h, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 10000-15000ppm.
[0063] After the 360°C constant temperature was completed, the inlet temperature of the reaction zone was lowered to 300°C, and the feedstock oil was introduced, with the initial introduction amount being 30% load. After stabilization, the feedstock oil feed amount was adjusted to 80% load. Subsequently, the reaction temperature was adjusted, and the product was produced and the catalyst was evaluated over a long period of time according to the conditions in Table 3.
[0064] Comparative Example 3
[0065] After the catalyst loading, air tightness inspection and establishment of the circulating hydrogen system of the wax oil hydrogenation unit are completed, the high pressure is controlled to the design pressure (7MPa), and the hourly volume flow rate of circulating hydrogen is controlled to be 1000 times the total catalyst loading volume. The inlet temperature of the reaction zone is increased to 280°C. When the volume of water generated by the high pressure separator is 20% of the catalyst loading amount, the inlet temperature of the reaction zone is reduced to 170°C.
[0066] The sulfiding agent DMDS is gradually injected into the reaction zone through a high-pressure sulfur injection pump, and the temperature is gradually increased and the catalyst bed temperature in the reaction zone is controlled not to exceed 230°C, until the mass concentration of hydrogen sulfide in the circulating hydrogen is maintained at more than 1000ppm, the hydrogen sulfide penetrates the catalyst bed, and then enters the first sulfidation stage, the reaction zone inlet temperature is increased to 230°C at a rate of 5°C / h, and constant temperature sulfidation is carried out for 8 hours, during which the hydrogen sulfide concentration in the circulating hydrogen is controlled to be maintained at 2000-3000ppm.
[0067] After the constant temperature at 230°C is completed, the inlet temperature of the reaction zone is steadily increased to 360°C at a rate of 5°C / h, during which the concentration of hydrogen sulfide is controlled to be 5000-10000ppm. Constant temperature sulfidation is performed at 360°C for 5h, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 10000-15000ppm.
[0068] After the 360°C constant temperature was completed, the inlet temperature of the reaction zone was lowered to 300°C, and the feedstock oil was introduced, with the initial introduction amount being 30% load. After stabilization, the feedstock oil feed amount was adjusted to 80% load. Subsequently, the reaction temperature was adjusted, and the product was produced and the catalyst was evaluated over a long period of time according to the conditions in Table 3.
[0069] Comparative Example 4
[0070] After the wax oil hydrogenation unit has completed the catalyst loading, air tightness inspection, and establishment of the circulating hydrogen system, the high pressure is controlled to the design pressure (7MPa), the hourly volume flow rate of circulating hydrogen is controlled to 600 times the total catalyst loading volume, and NO gas is injected into the reaction zone inlet, and the volume injection rate of NO is 15% of the circulating hydrogen volume flow rate. The reaction zone inlet temperature is increased to 210°C. When the NO2 volume fraction in the circulating hydrogen is 2%, the NO gas is stopped from being introduced, and the reaction zone inlet temperature is reduced to 170°C.
[0071] New hydrogen begins to be introduced into the circulating hydrogen and is passed from the reaction zone into the wax oil hydrogenation unit to replace the gas in the reaction system. When the hydrogen gas volume fraction in the circulating hydrogen reaches 97%, the hydrogen replacement is completed.
[0072] The sulfiding agent DMDS is gradually injected into the reaction zone through a high-pressure sulfur injection pump, and the temperature is gradually increased and the catalyst bed temperature in the reaction zone is controlled not to exceed 230°C, until the mass concentration of hydrogen sulfide in the circulating hydrogen is maintained at more than 1000ppm, and the hydrogen sulfide penetrates the catalyst bed. Then, the first sulfidation stage is entered, and the inlet temperature of the reaction zone is increased to 250°C at a rate of 5°C / h. Constant temperature sulfidation is carried out for 10 hours, during which the concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 4000-5000ppm.
[0073] After the constant temperature at 250°C is completed, the inlet temperature of the reaction zone is steadily increased to 360°C at a rate of 8°C / h, during which the hydrogen sulfide concentration is controlled to be 6000-8000ppm. The constant temperature sulfidation is carried out at 360°C for 3h, during which the hydrogen sulfide concentration in the circulating hydrogen is controlled to be maintained at 13000-15000ppm.
[0074] After the constant temperature of 360°C was completed, the inlet temperature of the reaction zone was lowered to 320°C, and the feedstock oil was introduced, with the initial introduction amount being 35% load. After stabilization, the feedstock oil feed amount was adjusted to 70% load. Subsequently, the reaction temperature was adjusted, and the product was produced according to the conditions in Table 3 and the catalyst was evaluated over a long period of time.
[0075] Table 1 Raw oil properties
[0076] Raw oil name Low sulfur wax oil <![CDATA[Density (20 °C), g·cm -3 (GB / T 1884)]]> 0.9235 Distillation range, ℃ (ASTM D1160) IBP / 10% 350 / 371 30% / 50% 401 / 425 70% / 90 483 / 525 95% / EBP 539 / 568 Sulfur content, ppm 4500 Nitrogen content, ppm 2000
[0077] Table 2 Industrial Catalysts
[0078] Industrial Agents FF-34 Physical and chemical properties Pore diameter / nm 2~10nm <![CDATA[Pore volume / mL·g -1 > ≥0.35 <![CDATA[Specific surface area / m 2 ·g -1 > ≥120 shape Shamrock <![CDATA[Loading heap ratio, g / cm 3 > 0.75
[0079] Table 3 Evaluation conditions
[0080] High pressure, MPa 7.0 <![CDATA[Volume space velocity during refining liquid, h -1 > 1.0 Sulfur content of wax oil, ppm ~2500 Hydrogen to oil volume ratio at hydrotreating inlet 400:1 Running time, h 2500
[0081] Table 4 Example test results
[0082] project Example 1 Example 2 Example 3 Example 4 Hydrogen consumption, wt% 0.90 0.92 0.95 0.93 Refined catalyst deactivation rate, ℃ / d 0.04 0.06 0.05 0.08 Average reaction temperature of 2500h refining, ℃ 380 382 381 384
[0083] Table 5 Comparative Example Test Results
[0084] project Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Hydrogen consumption, wt% 1.09 1.03 1.06 1.00 Refined catalyst deactivation rate, ℃ / d 0.19 0.15 0.16 0.12 Average reaction temperature of 2500h refining, ℃ 397 393 395 388
[0085] It can be seen from the above examples and comparative examples that, under the condition of controlling the same sulfur content in wax oil, the start-up method of the present invention not only has low hydrogen consumption but also slows down the catalyst deactivation rate.
Claims
1. A method for starting up a wax oil hydrogenation unit, comprising: After the wax oil hydrogenation unit has completed the catalyst loading, air tightness inspection, and establishment of the circulating hydrogen system, the hourly volume flow rate of the circulating hydrogen is controlled to be 100-800 times the total catalyst loading volume, and NO gas is injected into the inlet of the reaction zone of the wax oil hydrogenation unit. The volume injection rate of NO is 10%-30% of the circulating hydrogen volume flow rate. The inlet temperature of the reaction zone is increased to 200-240°C. When the volume fraction of NO2 in the circulating hydrogen is 5%-30%, the injection of NO gas is stopped, and then hydrogen replacement and sulfurization are carried out in sequence. After the sulfurization is completed, the feedstock oil is introduced for normal production; The vulcanization adopts dry vulcanization, and the dry vulcanization includes a first vulcanization stage and a second vulcanization stage, wherein the first vulcanization stage is to increase the inlet temperature of the reaction zone to a first constant temperature of 230-250°C at a heating rate of ≯10°C / h, and then maintain the first constant temperature for 4-10 hours, and the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 1000-5000ppm in the first vulcanization stage; the second vulcanization stage is to increase the inlet temperature of the reaction zone to a second constant temperature of 350-390°C at a heating rate of ≯10°C / h, and the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to reach 5000-10000ppm during the heating period, and then maintain the second constant temperature for 2-6 hours, and the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to reach 10000-20000ppm during the second constant temperature period.
2. The start-up method according to claim 1, characterized in that: The hydrogen replacement is completed when the hydrogen gas volume fraction in the circulating hydrogen is adjusted to 95% to 99%.
3. The start-up method according to claim 1 or 2, characterized in that: Before hydrogen replacement, the inlet temperature of the reaction zone is lowered to 150~170℃, and then hydrogen replacement is carried out.
4. The start-up method according to claim 1, characterized in that: In the dry vulcanization, the first vulcanization stage is to increase the temperature of the reaction zone inlet to a first constant temperature of 230-250° C. at a heating rate of 3-10° C. / h, and then maintain the temperature at the first constant temperature for 4-10 hours. In the first vulcanization stage, the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to be maintained at 1000-5000 ppm; the second vulcanization stage is to increase the temperature of the reaction zone inlet to a second constant temperature of 350-390° C. at a heating rate of 3-10° C. / h, and the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to reach 5000-10000 ppm during the heating period, and then maintain the temperature at the second constant temperature for 2-6 hours. During the second constant temperature period, the mass concentration of hydrogen sulfide in the circulating hydrogen is controlled to reach 10000-20000 ppm.
5. The start-up method according to claim 4, characterized in that: In the dry sulfidation, before entering the first sulfidation stage, the sulfiding agent is gradually injected into the wax oil hydrogenation unit, and the temperature is gradually increased and the catalyst bed temperature in the reaction zone is controlled not to exceed 230° C. until hydrogen sulfide penetrates the entire catalyst bed.
6. The start-up method according to claim 5, characterized in that: The conditions for hydrogen sulfide to penetrate the entire catalyst bed are as follows: the mass concentration of hydrogen sulfide in the circulating hydrogen reaches more than 1000 ppm.
7. The start-up method according to claim 6, characterized in that: The conditions for hydrogen sulfide to penetrate the entire catalyst bed are as follows: the mass concentration of hydrogen sulfide in the circulating hydrogen reaches 1000~10000pm.
8. The start-up method according to claim 4, characterized in that: The reaction zone is filled with a hydrotreating catalyst; the hydrotreating catalyst, based on the weight of the catalyst, has a content of 15% to 35% in terms of Group VIB metal oxides and a content of 2% to 10% in terms of Group VIII metal oxides.
9. The start-up method according to claim 8, characterized in that: The hydrorefining catalyst has a content of 18% to 30% of Group VIB metal oxides and a content of 4% to 8% of Group VIII metal oxides based on the weight of the catalyst.
10. The start-up method according to claim 1 or 4, characterized in that: The vulcanizing agent used in the vulcanization is at least one of dimethyl disulfide and carbon disulfide.
11. The start-up method according to claim 1, characterized in that: The initial distillation point of the feedstock oil is 300-400° C., the final distillation point is 550-650° C., the sulfur content is below 5000 ppm, and the nitrogen content is 1500-4000 ppm.
12. The start-up method according to claim 1, characterized in that: The specific operation of introducing the crude oil is as follows: lowering the inlet temperature of the reaction zone to 280-320°C, starting to introduce the crude oil, with the initial introduction amount being 20%-40% of the designed processing load. After stabilization, the crude oil feed amount is adjusted to 60%-100%, and the reaction temperature is adjusted until the wax oil product quality is qualified.
13. The start-up method according to claim 1, characterized in that: During normal production, the reaction conditions are as follows: reaction pressure 5.0-10.0 MPa, reaction temperature 280-410°C, volume space velocity of 0.5-6.0 h-10 -1 .
14. The start-up method according to claim 13, characterized in that: During normal production, the reaction conditions are as follows: reaction pressure 6.0-8.0 MPa, reaction temperature 340-400°C, volume space velocity of 0.6-2.0 h -1 .