Metal-relaxor ferroelectric ceramic with micro-nano composite structure and preparation method thereof

By uniformly distributing metal Ag particles in BNT-BKT ceramics, forming a micro-nano composite structure, and controlling the sintering conditions, the problem of low depolarization temperature of BNT-based ceramics is solved, and the depolarization temperature and stability of the ceramics are improved.

CN116065075BActive Publication Date: 2024-11-15HARBIN INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310042651.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-28
Publication Date
2024-11-15
Estimated Expiration
2043-01-28

AI Technical Summary

Technical Problem

The depolarization temperature of BNT-based ceramics is low, which leads to the problem of limited use temperature range in practical applications.

Method used

A metal-relaxation ferroelectric ceramic with a micro-nano composite structure is adopted, and a micro-nano grain composite structure formed by 4-6 μm metal Ag particles uniformly distributed in nanoscale BNT-BKT ceramic grains, and is controlled by controlling Sintering temperature and insulation time increase the depolarization temperature of the ceramic. The specific steps include mixing and calcining the BNT-BKT pre-burning powder and silver oxide Ag2O powder, adding a binder and pressing into a wafer, sintering and gold plating and polarizing.

Benefits of technology

The depolarization temperature of BNT-BKT ceramics is increased to 170-185℃, which is 35-50℃ higher than the original ceramics, enhancing its stability and application temperature range at high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116065075B_ABST
    Figure CN116065075B_ABST
Patent Text Reader

Abstract

A metal-relaxor ferroelectric ceramic with a micro-nano composite structure and a preparation method thereof. The present invention belongs to the field of functional ceramic materials, and specifically relates to a metal-relaxor ferroelectric ceramic with a micro-nano composite structure and a preparation method thereof. The present invention aims to solve the problem of low depolarization temperature of existing BNT-based ceramics. The present invention prepares BNT-BKT / Ag ceramics with a micro-nano composite structure by controlling the sintering temperature and the holding time, wherein metal silver particles of 4 to 6 μm in size are uniformly distributed in nanoscale ceramic grains as a composite to form a micro-nano composite structure. Ag particles exert a large stress on ceramic grains during the heating process of the ceramic, thereby suppressing the depolarization behavior of the BNT-BKT ceramic, and obtaining sodium bismuth titanate-potassium bismuth titanate piezoelectric ceramics with a high depolarization temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of functional ceramic materials, and in particular relates to a metal-relaxor ferroelectric ceramic with a micro-nano composite structure and a preparation method thereof. Background Art

[0002] As a multifunctional material that can convert mechanical energy into electrical energy, piezoelectric ceramics are often used in electromechanical conversion devices. In recent years, with the improvement of people's ecological awareness and the demand for social sustainable development strategies, the production and use of lead-based piezoelectric ceramics and related devices have been restricted, and the research and development and use of lead-free piezoelectric ferroelectric ceramics have emerged. 0.5 Na 0.5 TiO3, BNT) as a lead-free relaxor ferroelectric, not only has good ferroelectric properties, but also has a Curie temperature (T m ~300℃), so the lead-free BNT system has attracted widespread attention.

[0003] The pure BNT system has low resistivity and high coercive field, making it difficult to fully polarize the ceramics, resulting in unsatisfactory piezoelectric properties. The piezoelectric constant d of BNT-based ceramics can be increased by constructing a trigonal-tetragonal quasi-modular phase boundary (MPB) in the BNT-based system through multi-component solid solution. 33 and the mechanical quality factor k p , such as 0.94BNT-0.06BT and 0.80BNT-0.20BKT systems. However, due to the existence of ferroelectric-relaxation phase transition, BNT-based piezoelectric ceramics have a depolarization temperature T before the Curie temperature. d , so this temperature is a key parameter that determines the actual use temperature range of ceramics. Recently, it has been found that quenching treatment can increase the depolarization temperature of BNT-based ceramics; however, due to the extremely high temperature during quenching, the sample is prone to cracks or even breakage, making it difficult to obtain complete and large ceramic pieces. Therefore, developing a new and stable preparation method to increase the depolarization temperature of BNT-based ceramics has extremely important research value and practical significance. Summary of the invention

[0004] The present invention aims to solve the problem of low depolarization temperature of existing BNT-based ceramics and provide a metal-relaxor ferroelectric ceramic with a micro-nano composite structure and a preparation method thereof.

[0005] A metal-relaxor ferroelectric ceramic with a micro-nano composite structure is a micro-nano grain composite structure formed by uniformly distributing metal Ag particles of 4 to 6 μm in the middle of nano-scale BNT-BKT ceramic grains.

[0006] A method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure is completed by the following steps:

[0007] 1. According to 0.8Bi 0.5 Na 0.5 TiO3-0.2Bi 0.5 K 0.5 Bi2O3, Na2CO3, K2CO3 and TiO2 are weighed, and the weighed Bi2O3, Na2CO3, K2CO3 and TiO2 are mixed and placed in a ball mill, and ball milled with anhydrous ethanol as a ball milling medium, and the wet material after ball milling is dried to obtain a dry mixture; the dry mixture is ground with a mortar to obtain a mixture powder, which is put into a corundum crucible and then placed in a box furnace for calcination to obtain a BNT-BKT pre-calcined powder with a pure perovskite structure;

[0008] 2. Weigh the BNT-BKT pre-calcined powder with a pure perovskite structure and the silver oxide Ag2O powder according to a molar ratio of 1:(0.025-0.125), put the weighed BNT-BKT pre-calcined powder with a pure perovskite structure and the silver oxide Ag2O powder into a mortar, mix and grind them to obtain a mixed powder;

[0009] 3. Add a binder to the mixed powder, grind it evenly, sieve it and press it into round tablets;

[0010] Fourth, three stacks of the formed discs are placed in a crucible covered with a platinum sheet, and the binder is removed at 500-650°C for 2-4 hours; then they are sintered at 1100-1200°C for 1-4 hours; metallic silver forms a liquid phase at its melting point of 962°C, and after flowing and agglomerating, it is evenly distributed among the BNT-BKT ceramic grains to obtain a metallic silver composite sodium bismuth titanate-potassium bismuth titanate ceramic sheet;

[0011] 5. The metal silver composite sodium bismuth titanate-bismuth potassium titanate ceramic sheet is gold-plated using a small metal sputtering coating machine, and the ceramic sheet is polarized using a DC high-voltage power supply. After the polarization is completed, the metal silver composite sodium bismuth titanate-bismuth potassium titanate piezoelectric ceramic is obtained.

[0012] Beneficial effects of the present invention: The present invention prepares BNT-BKT / Ag ceramics with a micro-nano composite structure by controlling the sintering temperature and the holding time, wherein the metal silver particles with a size of 4 to 6 μm are uniformly distributed in the nanoscale ceramic grains as a composite to form a micro-nano composite structure. The large thermal expansion coefficient and large-sized Ag particles exert stress on the nanoscale ceramic grains during the ceramic heating process, thereby increasing the depolarization temperature of the BNT-BKT ceramic; its depolarization temperature T d It is 170~185℃, which is 35~50℃ higher than BNT-BKT ceramics. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1XRD pattern of BNT-BKT / xAg (x=0, 0.15) ceramics;

[0014] Figure 2 Surface SEM image of BNT-BKT / 0.15Ag ceramic;

[0015] Figure 3 This is the elemental surface scanning spectrum of Ag in BNT-BKT / 0.15Ag ceramics;

[0016] Figure 4 This is the room temperature hysteresis loop of BNT-BKT / 0.15Ag ceramic;

[0017] Figure 5 The dielectric temperature spectrum of 0.80BNT-0.20BKT ceramics; 1 represents a frequency of 1kHz, 2 represents a frequency of 10kHz, and 3 represents a frequency of 100kHz;

[0018] Figure 6 It is the dielectric temperature spectrum of BNT-BKT / 0.15Ag ceramics; 1 represents the frequency of 1kHz, 2 represents the frequency of 10kHz, and 3 represents the frequency of 100kHz. DETAILED DESCRIPTION

[0019] The technical solution of the present invention is not limited to the specific implementation modes listed below, but also includes any combination of the specific implementation modes.

[0020] Specific implementation method 1: In this implementation method, a metal-relaxor ferroelectric ceramic with a micro-nano composite structure is a micro-nano grain composite structure formed by 4-6 μm metal Ag particles uniformly distributed in the middle of nano-scale BNT-BKT ceramic grains.

[0021] Specific embodiment 2: This embodiment is different from the specific embodiment 1 in that the chemical formula of the metal-relaxor ferroelectric ceramic with a micro-nano composite structure is 0.8Bi 0.5 Na 0.5 TiO3-0.2Bi 0.5 K 0.5 TiO3 / xAg, denoted as BNT-BKT / xAg, wherein x is the molar ratio of Ag to BNT-BKT, 0.05≤x≤0.25. Others are the same as those in the first embodiment.

[0022] Specific implementation method three: In this implementation method, a preparation method of a metal-relaxor ferroelectric ceramic with a micro-nano composite structure is completed by the following steps:

[0023] 1. According to 0.8Bi 0.5 Na 0.5 TiO3-0.2Bi 0.5 K0.5 Bi2O3, Na2CO3, K2CO3 and TiO2 are weighed, and the weighed Bi2O3, Na2CO3, K2CO3 and TiO2 are mixed and placed in a ball mill, and ball milled with anhydrous ethanol as a ball milling medium, and the wet material after ball milling is dried to obtain a dry mixture; the dry mixture is ground with a mortar to obtain a mixture powder, which is put into a corundum crucible and then placed in a box furnace for calcination to obtain a BNT-BKT pre-calcined powder with a pure perovskite structure;

[0024] 2. Weigh the BNT-BKT pre-calcined powder with a pure perovskite structure and the silver oxide Ag2O powder according to a molar ratio of 1:0.025-0.125, put the weighed BNT-BKT pre-calcined powder with a pure perovskite structure and the silver oxide Ag2O powder into a mortar, mix and grind them to obtain a mixed powder;

[0025] 3. Add a binder to the mixed powder, grind it evenly, sieve it and press it into round tablets;

[0026] Fourth, three stacks of the formed discs are placed in a crucible covered with a platinum sheet, and the binder is removed at 500-650°C for 2-4 hours; then they are sintered at 1100-1200°C for 1-4 hours; metallic silver forms a liquid phase at its melting point of 962°C, and after flowing and agglomerating, it is evenly distributed among the BNT-BKT ceramic grains to obtain a metallic silver composite sodium bismuth titanate-potassium bismuth titanate ceramic sheet;

[0027] 5. The metal silver composite sodium bismuth titanate-bismuth potassium titanate ceramic sheet is gold-plated using a small metal sputtering coating machine, and the ceramic sheet is polarized using a DC high-voltage power supply. After the polarization is completed, the metal silver composite sodium bismuth titanate-bismuth potassium titanate piezoelectric ceramic is obtained.

[0028] The depolarization temperature test of the metal silver composite sodium bismuth titanate-bismuth potassium titanate piezoelectric ceramic prepared in this embodiment is carried out: the polarized metal silver composite sodium bismuth titanate-bismuth potassium titanate ceramic sheet is placed in a dielectric temperature spectrum tester, and its dielectric properties are tested in the temperature range of 20 to 450°C to determine the depolarization temperature of the BNT-BKT / Ag ceramic.

[0029] Specific embodiment 4: This embodiment differs from specific embodiment 3 in that: the parameters of the ball milling in step 1 are: the ball-to-material ratio is (1.2-1.5):1, the rotation speed is 180-230 rpm, the ball milling time is 24-48h, and the drying temperature is 80-130°C. Others are the same as specific embodiment 3.

[0030] Specific embodiment 5: This embodiment differs from specific embodiment 3 or 4 in that the calcination parameters in step 1 are: calcination temperature is 800-900°C, heating rate is 2-10°C / min, calcination time is 2-6h. Others are the same as specific embodiment 3 or 4.

[0031] Specific embodiment 6: This embodiment is different from specific embodiments 3 to 5 in that: the mixed grinding in step 2 is to add anhydrous ethanol at a mass ratio of 1: (1.2 to 1.5) and grind by hand for 10 to 30 minutes, and after the alcohol evaporates and dries, add the same amount of anhydrous ethanol again and grind until the alcohol is completely evaporated. Others are the same as specific embodiments 3 to 5.

[0032] The mass ratio refers to the mass ratio of the total mass of the BNT-BKT pre-calcined powder with a pure perovskite structure and the silver oxide Ag2O powder to anhydrous ethanol, which is 1:(1.2-1.5).

[0033] Specific implementation 7: This implementation is different from Specific implementations 3 to 6 in that the adhesive in step 3 is PVA, and the amount of the adhesive added is 7% of the mass of the mixed powder. The rest is the same as Specific implementations 3 to 6.

[0034] Specific embodiment 8: This embodiment differs from specific embodiments 3 to 7 in that: the mesh size of the sieving in step 3 is 80 to 120 meshes; the pressing into round tablets is performed at a pressure of 4 to 8 MPa. The rest is the same as specific embodiments 3 to 7.

[0035] Specific embodiment 9: This embodiment is different from any one of specific embodiments 3 to 8 in that the heating rate of the sintering in step 4 is 2 to 6°C / min, and the cooling rate is 4 to 10°C / min. The rest is the same as any one of specific embodiments 3 to 8.

[0036] Specific embodiment 10: This embodiment differs from any one of specific embodiments 3 to 9 in that two layers of crucibles are placed on the stacked wafers in step 4. The rest is the same as any one of specific embodiments 3 to 9.

[0037] This embodiment can reduce element volatilization.

[0038] Specific embodiment 11: This embodiment differs from specific embodiments 3 to 10 in that: the gold plating time in step 5 is 5 to 15 minutes; the electric field intensity of the polarization treatment is 30 to 70 kV / cm, and the polarization time is 30 to 60 minutes. The rest is the same as specific embodiments 3 to 10.

[0039] Specific embodiment 12: This embodiment differs from specific embodiments 3 to 11 in that the diameter of the Ag particles in the metal silver composite sodium bismuth titanate-potassium bismuth titanate piezoelectric ceramic in step 5 is 4 to 6 μm, and the grain size of the BNT-BKT ceramic is 300 to 600 nm. Other aspects are the same as those of specific embodiments 3 to 11.

[0040] The following examples are used to verify the beneficial effects of the present invention:

[0041] Embodiment 1:

[0042] A method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure is completed by the following steps:

[0043] 1. According to 0.8Bi 0.5 Na 0.5 TiO3-0.2Bi 0.5 K 0.5 TiO3 proportion: Bi2O3, Na2CO3, K2CO3 and TiO2 are weighed, and the weighed Bi2O3, Na2CO3, K2CO3 and TiO2 are mixed and anhydrous ethanol is added in a mass ratio of 1:1.3, and then placed in a ball mill, and ball milled for 30 hours at a speed of 200 rpm, and the wet material after ball milling is dried at 110°C to obtain a dry mixture; the dry mixture is ground with a mortar to obtain a mixture powder, which is loaded into a corundum crucible and placed in a box furnace, and calcined at 830°C for 4 hours at a heating rate of 5°C / min to obtain a BNT-BKT pre-calcined powder with a pure perovskite structure;

[0044] 2. Weigh the BNT-BKT calcined powder with a pure perovskite structure and the silver oxide Ag2O powder in a molar ratio of 1:0.075, put the weighed BNT-BKT calcined powder with a pure perovskite structure and the silver oxide Ag2O powder into a mortar, add anhydrous ethanol in a mass ratio of 1:1.3 and grind for 15 minutes until the alcohol is completely evaporated, add anhydrous ethanol again in the same mass ratio and grind until the alcohol evaporates and dry to obtain a mixed powder;

[0045] 3. Add a binder to the mixed powder, grind it evenly, sieve it through 80 mesh, and press it into a disc with a diameter of 10 mm under a pressure of 6 MPa without holding the pressure; the binder is PVA, and the amount of the binder added is 7% of the mass of the mixed powder;

[0046] Fourth, three stacked discs are placed in a crucible covered with platinum sheets, covered with two layers of crucibles to reduce element volatilization, and the binder is removed at 550°C for 3 hours, while ensuring that Ag2O is completely separated into Ag and O2; then they are sintered at 1120°C, with a holding time of 1 hour, a heating rate of 2°C / min, and a cooling rate of 4°C / min; metallic silver forms a liquid phase at its melting point of 962°C, and after flowing and aggregation, it is evenly distributed among the BNT-BKT ceramic grains to obtain BNT-BKT / 0.15Ag ceramic sheets.

[0047] Comparative Example:

[0048] A method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure is completed by the following steps:

[0049] 1. According to 0.8Bi 0.5 Na 0.5 TiO3-0.2Bi 0.5 K 0.5 TiO3 proportion: Bi2O3, Na2CO3, K2CO3 and TiO2 are weighed, and the weighed Bi2O3, Na2CO3, K2CO3 and TiO2 are mixed and anhydrous ethanol is added in a mass ratio of 1:1.3, and then placed in a ball mill, and ball milled for 30 hours at a speed of 200 rpm, and the wet material after ball milling is dried at 110°C to obtain a dry mixture; the dry mixture is ground with a mortar to obtain a mixture powder, which is loaded into a corundum crucible and placed in a box furnace, and calcined at 830°C for 4 hours at a heating rate of 5°C / min to obtain a BNT-BKT pre-calcined powder with a pure perovskite structure;

[0050] 2. Put the BNT-BKT calcined powder with a pure perovskite structure into a mortar, add anhydrous ethanol at a mass ratio of 1:1.3 and grind for 15 minutes until the alcohol is completely evaporated, add anhydrous ethanol again at the same mass ratio and grind until the alcohol evaporates and dry to obtain a mixed powder;

[0051] 3. Add a binder to the mixed powder, grind it evenly, sieve it through 80 mesh, and press it into a disc with a diameter of 10 mm under a pressure of 6 MPa without holding the pressure; the binder is PVA, and the amount of the binder added is 7% of the mass of the mixed powder;

[0052] 4. Stack three formed discs in a crucible covered with platinum sheets, cover with two layers of crucibles to reduce element volatilization, and remove the binder at 550°C for 2 hours; then sinter at 1160°C, keep warm for 2 hours, heat up at a rate of 3°C / min, and cool down at a rate of 5°C / min; obtain 0.80BNT-0.20BKT ceramic sheets.

[0053] The ceramics in Example 1 and Comparative Example were ground into fine powders, and their X-ray diffraction spectra were tested at room temperature. Figure 1 As shown in the figure, the x=0 sample presents a pure perovskite structure, while the x=0.15 sample shows a small amount of second phase of metal Ag, and the overall performance is a composite phase of perovskite and metal Ag. In addition, both are in a pseudo-cubic phase in the unpolarized state.

[0054] After gold electrode sputtering was performed on the surface of the BNT-BKT / 0.15Ag ceramic sample, the morphology of the ceramic surface was observed by scanning electron microscopy, and element scanning detection was performed, such as Figure 2 , Figure 3 The morphology shows a composite structure of larger micron-sized particles and nano-sized grains. The elemental surface scanning spectrum shows that the particles with a size of 4 to 6 μm are metallic Ag, while the grain size of BNT-BKT ceramics is 300 to 600 nm. It can be seen that the Ag particles are evenly distributed in the ceramic grains and form a micro-nano composite structure.

[0055] The ferroelectric properties of BNT-BKT / 0.15Ag ceramics were tested. The hysteresis loop was tested at room temperature with an electric field strength of 60kV / cm and a frequency of 1Hz. Figure 4 BNT-BKT / 0.15Ag ceramics show a typical saturation hysteresis loop shape, with a coercive electric field Ec of 35kV / cm and a residual polarization intensity Pr of 26μC / cm 2 , indicating that the ceramic is a ferroelectric.

[0056] After sputtering gold electrodes on the ceramics in Example 1 and the comparative example, a DC high voltage power supply was used to polarize the ceramic sheets at room temperature at an electric field of 50 kV / cm for 30 minutes. After the polarization was completed, polarized BNT-BKT / xAg (x=0, 0.15) piezoelectric ceramics were obtained.

[0057] The polarized BNT-BKT / xAg ceramic sheet was subjected to dielectric temperature spectrum test. The dielectric constant and dielectric loss at different temperatures were measured at different test frequencies. Figure 5 is the dielectric temperature spectrum of BNT-BKT ceramics, Figure 6 The dielectric temperature spectrum of BNT-BKT / 0.15Ag ceramics. First, both ceramics show frequency dispersion and temperature dispersion, indicating that both are relaxor ferroelectric ceramics; and the frequency dispersion degree of BNT-BKT / 0.15Ag ceramics in the low temperature zone is lower than that of BNT-BKT ceramics. Secondly, the first dielectric abnormal peak of BNT-BKT ceramics is T d peak, indicating that the depolarization temperature of the ceramic is 136°C; while the T d The peak is around 179℃, which is 43℃ ​​higher than that of BNT-BKT ceramics.

Claims

1. A method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure, Features The preparation method of the metal-relaxor ferroelectric ceramic with a micro-nano composite structure is completed by the following steps:

1. According to 0.8Bi 0.5 Na 0.5 TiO 3 -0.2Bi 0.5 K 0.5 TiO 3 Weigh Bi 2 O 3 、Na 2 CO 3 , K 2 CO 3 and TiO 2 , the weighed Bi 2 O 3 、Na 2 CO 3 , K 2 CO 3 and TiO 2 The mixture is mixed and placed in a ball mill, and ball milled with anhydrous ethanol as a ball milling medium, and the wet material after ball milling is dried to obtain a dry mixture; the dry mixture is ground with a mortar to obtain a mixture powder, which is placed in a corundum crucible and then placed in a box furnace for calcination to obtain a BNT-BKT pre-calcined powder with a pure perovskite structure; 2. Pre-sintering BNT-BKT powder with pure perovskite structure and silver oxide Ag 2 O powder was weighed in a molar ratio of 1:(0.025-0.125), and the weighed BNT-BKT pre-calcined powder with a pure perovskite structure and silver oxide Ag were mixed. 2 The O powder is put into a mortar and mixed and ground to obtain a mixed powder; 3. Add a binder to the mixed powder, grind it evenly, sieve it and press it into round tablets; Fourth, three stacks of the formed discs are placed in a crucible covered with a platinum sheet, and the binder is removed at 500-650°C for 2-4 hours; then they are sintered at 1100-1200°C for 1-4 hours; metallic silver forms a liquid phase at its melting point of 962°C, and after flowing and agglomerating, it is evenly distributed among the BNT-BKT ceramic grains to obtain a metallic silver composite sodium bismuth titanate-potassium bismuth titanate ceramic sheet; 5. The metal silver composite sodium bismuth titanate-potassium bismuth titanate ceramic sheet is gold-plated by a small metal sputtering coating machine, and the ceramic sheet is polarized by a DC high-voltage power supply. After the polarization is completed, the metal silver composite sodium bismuth titanate-potassium bismuth titanate piezoelectric ceramic is obtained; the Ag particle diameter in the metal silver composite sodium bismuth titanate-potassium bismuth titanate piezoelectric ceramic is 4-6μm, and the BNT-BKT ceramic grain size is 300-600nm.

2. A method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure according to claim 1, Features The parameters of the ball milling in step 1 are as follows: the ball-to-material ratio is (1.2-1.5):1, the rotation speed is 180-230 rpm, and the ball milling time is 24-48 h; the drying temperature is 80-130° C.

3. A method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure according to claim 1, Features The calcination parameters in step 1 are as follows: calcination temperature is 800-900° C., heating rate is 2-10° C. / min, and calcination time is 2-6 h.

4. The method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure according to claim 1, Features The mixed grinding described in step 2 is to add anhydrous ethanol in a mass ratio of 1: (1.2-1.5) and grind by hand for 10-30 minutes. After the alcohol is evaporated and dried, the same amount of anhydrous ethanol is added again and ground until all the alcohol is evaporated.

5. The method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure according to claim 1, Features The adhesive in step 3 is PVA, and the amount of the adhesive added is 7% of the mass of the mixed powder.

6. The method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure according to claim 1, Features The mesh number of the sieving in step 3 is 80-120 meshes; and the pressing into round tablets is performed under a pressure of 4-8 MPa.

7. The method for preparing a metal-relaxor ferroelectric ceramic having a micro-nano composite structure according to claim 1, Features The gold plating time in step 5 is 5 to 15 minutes; the electric field intensity of the polarization treatment is 30 to 70 kV / cm, and the polarization time is 30 to 60 minutes.