A comprehensive utilization method of coal gasification slag
Through the carbon ash separation process and acid-alkali leaching treatment, carbon, aluminum, silicon and other elements in coal gasification slag have been successfully extracted and utilized to prepare efficient carbon adsorption materials and water glass, solving the problems of coal gasification slag in the existing technology. The problem of low utilization rate is solved and efficient comprehensive utilization of resources is achieved.
Patent Information
- Application Number
- CN202111313546.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-11-08
AI Technical Summary
The existing technology cannot effectively utilize carbon, aluminum, silicon, iron, calcium and other elements in coal gasification slag, and the comprehensive utilization rate is low, and it cannot realize the utilization of all components of gasification slag.
The carbon ash separation process is used to obtain low-carbon slag with a loss on ignition of <5%, medium-carbon slag with a loss on ignition of 20-50%, and high-carbon slag with a loss on ignition of >80%, which are removed through acid leaching and alkali leaching respectively. Remove metal elements and prepare aluminum-based water purifiers, silicon-based water glass and carbon adsorption materials. Medium carbon slag is used for porous materials, geopolymers, etc., and high carbon slag is used to prepare carbon adsorption materials.
The separation of gasified slag carbon and other components is achieved. The prepared carbon adsorption material has a large specific surface area, high adsorption capacity, simple process, mild reaction, no secondary solid waste, small dosage of chemicals, low operating cost, and carbon High ash separation efficiency.
Smart Images

Figure CN116078348B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource utilization of inorganic chemical solid waste, and specifically relates to a comprehensive utilization method of coal gasification slag. Background Art
[0002] Coal gasification is one of the main ways to produce syngas products, mainly including fixed bed gasification technology, fluidized bed gasification technology and entrained bed gasification technology, which converts solid coal into gaseous syngas, while producing byproducts such as steam, tar (individual gasification technology) and ash. With the substantial growth in demand for syngas products, the byproduct inorganic ash is also discharged and stored in large quantities, causing serious environmental pollution problems.
[0003] In view of the physical properties of ash produced in the coal gasification process, CN106336164A discloses a method for preparing thermal insulation unburned bricks, using gasification slag as raw material, adding coal gangue, steel slag and boiler slag thereto, and obtaining unburned bricks after molding and curing; CN106467376A discloses a process for preparing unburned bricks, using gasification slag as raw material, adding cement and bean sand stone thereto, and obtaining unburned bricks after molding and curing.
[0004] In order to increase the added value of ash utilization, CN104774023A discloses a lightweight ceramsite prepared from fly ash and gasified slag, and its preparation method and application. After the gasified slag and sodium / potassium feldspar are mixed in a certain proportion, a small amount of additives are added to carry out molding, drying and sintering processes to obtain qualified lightweight ceramsite; CN105130487A discloses a composition for producing filter ceramics, filter ceramics, and its preparation method and application. Fly ash and gasified slag are used as raw materials, and grinding, molding and sintering are carried out in sequence to obtain qualified filter ceramics.
[0005] Based on the chemical composition characteristics of coal gasification slag, CN106800416A discloses a method for preparing low creep refractory bricks using gasification slag. The method uses gasification slag, cordierite, zirconium corundum, limestone, fly ash and feldspar as raw materials, adds additives such as boron carbide fiber and nano tungsten oxide, and obtains a refractory material with high mechanical properties, low creep and good seismic resistance through fine grinding-microwave high-temperature sintering-washing-drying and other processes.
[0006] Based on the high carbon content of coal gasification slag, CN102980195A discloses a method for treating coal chemical gasification slag, in which the gasification slag is evenly mixed with coal slime and then white mud slurry is added, and the mixture is sent to a fluidized bed boiler through a conveying pipeline for combustion, thereby improving the utilization efficiency of the carbon therein; CN108584971A discloses a method for preparing high modulus soluble silicate from coal gasification slag, in which the high modulus soluble silicate is obtained by the acid leaching-alkali leaching method, which has high quality and low production cost, but cannot realize the utilization of the carbon component in the gasification slag.
[0007] Coal gasification slag contains rich elements such as carbon, aluminum, silicon, iron, and calcium. The existing methods have failed to achieve effective extraction and utilization, and the comprehensive utilization rate is low, and the purpose of utilizing all components of the gasification slag has not been achieved.
[0008] Therefore, it is necessary to provide a new comprehensive utilization method of coal gasification slag to achieve effective extraction and utilization and improve comprehensive utilization efficiency. Summary of the invention
[0009] The object of the present invention is to provide a comprehensive utilization method of coal gasification slag. The comprehensive utilization method of coal gasification slag adopts a carbon ash separation process to obtain low-carbon slag with a loss on ignition of less than 5%, medium-carbon slag with a loss on ignition of 20-50%, and high-carbon slag with a loss on ignition of more than 80%. The aluminum, iron, and calcium metal elements in the low-carbon slag are removed by acid leaching, and the silicon element is removed by alkali leaching to obtain an aluminum-based water purifier and a silicon-based water glass. The medium-carbon slag is used as a raw material for porous materials, geopolymers, molecular sieves, microcrystalline glass or ceramsite, and the high-carbon slag is used to prepare carbon adsorption materials. The comprehensive utilization method of the present invention has a simple process, a mild reaction, and does not generate secondary solid waste. The prepared carbon adsorption material has a large specific surface area and a high adsorption capacity, and the separation of gasification slag carbon from other components is realized, the amount of reagents used is small, the operating cost is low, and the carbon ash separation efficiency is high.
[0010] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0011] The object of the present invention is to provide a comprehensive utilization method of coal gasification slag, which comprises the following steps:
[0012] (1) separating the coal gasification slag into carbon ash to obtain a first high-carbon slag, a medium-carbon slag and a low-carbon slag;
[0013] (2) subjecting the low carbon slag obtained in step (1) to acid leaching to obtain an acid leaching solution and an acid leaching slag; and subjecting the acid leaching slag to alkali leaching to obtain a second high carbon slag and an alkali leaching solution;
[0014] (3) activating the first high carbon slag in step (1) and the second high carbon slag in step (2) to obtain a carbon adsorption material;
[0015] The first high carbon slag and the second high carbon slag are both carbon slags with a loss on ignition greater than 80%, the medium carbon slag is carbon slag with a loss on ignition of 20-50%, and the low carbon slag is carbon slag with a loss on ignition less than 5%.
[0016] The comprehensive utilization method of coal gasification slag of the present invention adopts a carbon ash separation process to obtain low-carbon slag with a loss on ignition of less than 5%, medium-carbon slag with a loss on ignition of 20-50%, and high-carbon slag with a loss on ignition of more than 80%. The aluminum, iron, and calcium metal elements in the low-carbon slag are removed by acid leaching, and the silicon element is removed by alkali leaching to obtain an aluminum-based water purifier and a silicon-based water glass. The medium-carbon slag is used as a raw material for porous materials, geopolymers, molecular sieves, microcrystalline glass or ceramsite, and the high-carbon slag is used to prepare carbon adsorption materials. The comprehensive utilization method of the present invention has a simple process, mild reaction, and does not generate secondary solid waste. The prepared carbon adsorption material has a large specific surface area and a high adsorption capacity, and the separation of gasification slag carbon from other components is realized, the amount of reagents used is small, the operating cost is low, and the carbon ash separation efficiency is high.
[0017] It is worth noting that in the process of carbon ash separation described in the present invention, 5%-20% carbon slag and 50%-80% carbon slag will not be produced. In actual application, if 5%-20% carbon slag and 50%-80% carbon slag appear, the carbon ash separation will be repeated until there is no 5%-20% carbon slag and 50%-80% carbon slag.
[0018] As a preferred technical solution of the present invention, the carbon ash separation in step (1) includes classification, gravity separation and flotation performed in sequence.
[0019] Preferably, the classification equipment comprises any one of a vibrating screen, a cyclone or a spiral classifier, or a combination of at least two of them. The combination typically but not limitedly comprises a combination of a vibrating screen and a cyclone, a combination of a vibrating screen and a spiral classifier, and a combination of a cyclone and a spiral classifier.
[0020] Preferably, the re-selection equipment comprises a sorting cyclone and / or a spiral chute.
[0021] Preferably, the flotation equipment comprises a flotation machine and / or a flotation column.
[0022] Preferably, during the flotation process, a regulator, a collector and a frother are added in sequence.
[0023] Preferably, the adjusting agent comprises sodium hexametaphosphate and / or water glass.
[0024] Preferably, the dosage of the adjusting agent is 0.5-2kg / t, for example, it can be 0.5kg / t, 0.6kg / t, 0.7kg / t, 0.8kg / t, 0.9kg / t, 1kg / t, 1.1kg / t, 1.2kg / t, 1.3kg / t, 1.4kg / t, 1.5kg / t, 1.6kg / t, 1.7kg / t, 1.8kg / t, 1.9kg / t, 2kg / t, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0025] Preferably, the collector comprises a composite solution of oleic acid, linoleic acid and kerosene.
[0026] Preferably, the sum of the contents of oleic acid and linoleic acid in the composite solution is 5-50wt%, for example, it can be 5wt%, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%, 35wt%, 40wt%, 45wt%, 50wt% and the like, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0027] Preferably, the kerosene content in the composite solution is 50-95wt%, for example, it can be 50wt%, 55wt%, 60wt%, 65wt%, 70wt%, 75wt%, 80wt%, 85wt%, 90wt%, 95wt%, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0028] Preferably, the dosage of the collector is 1-20 kg / t, for example, it can be 1 kg / t, 2 kg / t, 4 kg / t, 6 kg / t, 8 kg / t, 10 kg / t, 12 kg / t, 14 kg / t, 16 kg / t, 8 kg / t, 20 kg / t, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0029] Preferably, the blowing agent comprises methyl isobutyl carbinol.
[0030] Preferably, the dosage of the foaming agent is 1-20 kg / t, for example, it can be 1 kg / t, 2 kg / t, 4 kg / t, 6 kg / t, 8 kg / t, 10 kg / t, 12 kg / t, 14 kg / t, 16 kg / t, 8 kg / t, 20 kg / t, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0031] Preferably, the flotation comprises roughing, cleaning and scavenging which are performed sequentially.
[0032] Preferably, the rough selection is performed 1-2 times, for example, 1 time or 2 times.
[0033] Preferably, the number of times of selection is 1-3 times, for example, it can be 1 time, 2 times or 3 times.
[0034] Preferably, the scanning is performed 1-3 times, for example, 1 time, 2 times or 3 times.
[0035] As a preferred technical solution of the present invention, the concentration of the acid leaching solution used in the acid leaching in step (2) is 3-10 mol / L, for example, it can be 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, 5.5 mol / L, 6 mol / L, 6.5 mol / L, 7 mol / L, 7.5 mol / L, 8 mol / L, 8.5 mol / L, 9 mol / L, 9.5 mol / L, 10 mol / L, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0036] Preferably, the solute of the acid leaching solution includes any one of hydrochloric acid, nitric acid or sulfuric acid, or a combination of at least two of them. The combination typically but not limitedly includes a combination of hydrochloric acid and nitric acid, a combination of hydrochloric acid and sulfuric acid, and a combination of nitric acid and sulfuric acid.
[0037] Preferably, the mass ratio of the acid leaching solution to the low carbon slag is (2-8):1, for example, it can be 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1, 5:1, 5.5:1, 6:1, 6.5:1, 7:1, 7.5:1, 8:1, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0038] Preferably, the acid leaching temperature in step (2) is 20-100°C, for example, it can be 20°C, 30°C, 40°C, 50°C, 60°C, 0°C, 80°C, 90°C, 100°C, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0039] Preferably, the acid leaching time in step (2) is 30-200 min, for example, it can be 30 min, 50 min, 70 min, 90 min, 100 min, 120 min, 140 min, 160 min, 80 min, 200 min, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0040] As a preferred technical solution of the present invention, the comprehensive utilization method further comprises: controlling the pH of the acid leaching solution in step (2) to obtain the ferroalloy and the water purifier.
[0041] The acid leaching solution in step (2) of the present invention can also be mixed with the medium carbon slag in step (1) to be used as a raw material for porous materials and / or ceramic materials.
[0042] Preferably, the reagent used for pH control includes any one of potassium hydroxide, sodium hydroxide, calcium aluminate or carbide slag, or a combination of at least two of them.
[0043] Preferably, the endpoint pH of the pH regulation is 3-5, for example, it can be 3, 3.5, 4, 4.5, 5, etc., but it is not limited to the listed values, and other values not listed in the above numerical range are also applicable.
[0044] As a preferred technical solution of the present invention, the concentration of the alkali leaching solution used in the alkali leaching in step (2) is 0.5-5 mol / L, for example, it can be 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0045] Preferably, the solute of the alkaline leaching solution includes sodium hydroxide and / or potassium hydroxide.
[0046] Preferably, the temperature of the alkali leaching in step (2) is 60-180°C, for example, it can be 60°C, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0047] Preferably, the alkali leaching time in step (2) is 60-240 min, for example, it can be 60 min, 100 min, 120 min, 150 min, 180 min, 200 min, 220 min, 240 min, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0048] Preferably, the stirring speed of the alkali leaching in step (2) is 200-500rpm, for example, it can be 200rpm, 230rpm, 250rpm, 280rpm, 300rpm, 330rpm, 350rpm, 370rpm, 400rpm, 420rpm, 450rpm, 480rpm, 500rpm, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0049] As a preferred technical solution of the present invention, the comprehensive utilization method also includes: using the medium carbon slag in step (1) as a raw material for porous materials and / or ceramic materials; and using the alkaline leaching solution in step (2) as a raw material for water glass.
[0050] As a preferred technical solution of the present invention, before the activation in step (3), the first high carbon slag and the second high carbon slag are sequentially mixed, impregnated once and dried once.
[0051] Preferably, the first high carbon slag and the second high carbon slag are mixed to obtain high carbon slag.
[0052] The high carbon slag of the present invention can be activated to prepare carbon adsorption material, and can also be used as thermal coal.
[0053] Preferably, the primary impregnation liquid used in the primary impregnation comprises a potassium hydroxide solution.
[0054] Preferably, the concentration of the primary impregnation solution is 3-5 mol / L, for example, it can be 3 mol / L, 3.2 mol / L, 3.4 mol / L, 3.6 mol / L, 3.8 mol / L, 4 mol / L, 4.2 mol / L, 4.4 mol / L, 4.6 mol / L, 4.8 mol / L, 5 mol / L, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0055] Preferably, the mass ratio of the high carbon slag to the solute in the primary impregnation solution is 1:(1-3), for example, it can be 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8, 1:2, 1:2.2, 1:2.4, 1:2.6, 1:2.8, 1:3, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0056] Preferably, the immersion time is 1-3h, for example, it can be 1h, 1.2h, 1.4h, .6h, 1.8h, 2h, 2.3h, 2.5h, 2.8h, 3h, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0057] Preferably, the temperature of the primary immersion is 20-30°C, for example, it can be 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0058] Preferably, the temperature of the primary drying is 100-200°C, for example, it can be 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 90°C, 200°C, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0059] Preferably, the drying time is 1-3h, for example, it can be 1h, 1.2h, 1.4h, .6h, 1.8h, 2h, 2.3h, 2.5h, 2.8h, 3h, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0060] As a preferred technical solution of the present invention, the activation temperature in step (3) is 600-900°C, for example, it can be 600°C, 620°C, 650°C, 680°C, 700°C, 730°C, 750°C, 780°C, 800°C, 820°C, 850°C, 880°C, 900°C, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0061] Preferably, the activation time in step (3) is 0.5-3 h, for example, 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, 3 h, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0062] Preferably, the activation in step (3) is carried out under a nitrogen atmosphere.
[0063] Preferably, the flow rate of the nitrogen is 300-350 mL / min, for example, it can be 300 mL / min, 305 mL / min, 310 mL / min, 315 mL / min, 320 mL / min, 325 mL / min, 330 mL / min, 335 mL / min, 340 mL / min, 345 mL / min, 350 mL / min, etc., but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0064] As a preferred technical solution of the present invention, the carbon adsorption material in step (3) is subjected to secondary impregnation, washing, solid-liquid separation and secondary drying in sequence.
[0065] Preferably, the secondary impregnation liquid used in the secondary impregnation comprises a hydrochloric acid solution.
[0066] Preferably, the solute content in the secondary impregnation solution is 5-20%, for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0067] Preferably, the mass ratio of the carbon adsorption material to the secondary impregnation liquid is 1:(2-5), for example, it can be 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0068] Preferably, the secondary impregnation time is 5-24h, for example, it can be 5h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0069] Preferably, the temperature of the secondary impregnation is 20-30°C, for example, it can be 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0070] Preferably, the cleaning agent used for the cleaning comprises pure water.
[0071] Preferably, the solid-liquid separation method is suction filtration.
[0072] Preferably, the temperature of the secondary drying is 80-120°C, for example, it can be 80°C, 90°C, 100°C, 110°C, 120°C, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0073] Preferably, the secondary drying time is 4-6h, for example, it can be 4h, 4.2h, 4.5h, 4.8h, 5h, 5.3h, 5.5h, 5.8h, 6h, etc., but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0074] As a preferred technical solution of the present invention, the comprehensive utilization method comprises the following steps:
[0075] (1) First, the coal gasification slag is classified in a vibrating screen, a cyclone or a spiral classifier; second, it is re-selected in a sorting cyclone or a spiral chute; third, 0.5-2 kg / t of a regulator, 1-20 kg / t of a collector and 1-20 kg / t of a frother are added in sequence in a flotation machine or a flotation column for flotation to obtain a first high carbon slag, a medium carbon slag and a low carbon slag;
[0076] The adjusting agent comprises sodium hexametaphosphate and / or water glass; the collecting agent comprises a compound solution of 5-50wt% oleic acid and linoleic acid and 50-95wt% kerosene; the frother comprises methyl isobutyl carbinol; the flotation comprises 1-2 roughing selections, 1-3 cleaning selections and 1-3 scavenging selections in sequence; the medium carbon slag is used as a raw material for porous materials and / or ceramic materials;
[0077] (2) firstly subjecting the low carbon slag obtained in step (1) to acid leaching in a 3-10 mol / L acid leaching solution at 20-100° C. for 30-200 min, controlling the mass ratio of the acid leaching solution to the low carbon slag to (2-8):1, to obtain an acid leaching solution and an acid leaching slag; using potassium hydroxide, sodium hydroxide, calcium aluminate or carbide slag to control the pH of the acid leaching solution to a pH of 3-5, to obtain a ferroalloy and a water purifier; then, subjecting the acid leaching slag to alkaline leaching in a 0.5-5 mol / L alkaline leaching solution at a temperature of 60-180° C. and a stirring speed of 200-500 rpm for 60-240 min, to obtain a second high carbon slag and an alkaline leaching solution; and using the alkaline leaching solution as a raw material for water glass;
[0078] (3) The first high carbon slag and the second high carbon slag are mixed to obtain high carbon slag. First, the high carbon slag is immersed in a 3-5 mol / L potassium hydroxide solution at 20-30°C for 1-3 hours, and the mass ratio of the high carbon slag to the potassium hydroxide in the potassium hydroxide solution is controlled to be 1:(1-3); secondly, it is dried at 100-200°C for 1-3 hours; thirdly, it is activated at 600-900°C for 0.5-3 hours under a nitrogen atmosphere of 300-350 mL / min to obtain a carbon adsorption material; then, the carbon adsorption material is immersed in a 5-20% hydrochloric acid solution at 20-30°C for a second time for 5-24 hours, and the mass ratio of the carbon adsorption material to the hydrochloric acid solution is controlled to be 1:(2-5); then, it is washed with pure water, filtered, and then dried at 80-120°C for 4-6 hours;
[0079] The first high carbon slag and the second high carbon slag are carbon slags with a loss on ignition greater than 80%, the medium carbon slag is carbon slag with a loss on ignition of 20-50%, and the low carbon slag is carbon slag with a loss on ignition less than 5%.
[0080] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0081] Compared with the prior art, the present invention has the following beneficial effects:
[0082] (1) The comprehensive utilization method of coal gasification slag of the present invention adopts a carbon ash separation process to obtain low carbon slag with a loss on ignition of less than 5%, medium carbon slag with a loss on ignition of 20-50%, and high carbon slag with a loss on ignition of more than 80%. The high carbon slag is used to prepare carbon adsorption materials, and the medium carbon slag is used as a raw material for porous materials, geopolymers, molecular sieves, microcrystalline glass or ceramsite, thereby realizing the separation of gasification slag carbon and other components, with less reagent usage, low operating cost, and high carbon ash separation efficiency;
[0083] (2) The comprehensive utilization method of coal gasification slag of the present invention first separates carbon ash, and prepares aluminum-based water purifier, silicon-based water glass and carbon-based adsorption material for low-carbon slag. The process is simple, the reaction is mild, no secondary solid waste is generated, and the prepared carbon-based adsorption material has a large specific surface area and a high adsorption capacity;
[0084] (3) The comprehensive utilization method of coal gasification slag described in the present invention can prepare a variety of products, which are not easily restricted by product market fluctuations. The high-, medium- and low-end utilization technologies are matched. On the one hand, medium- and low-end building materials and materials can solve the problem of large-scale disposal and utilization of gasification slag. On the other hand, high-end products can achieve economic benefits and supplement the cost investment in the preparation of medium- and low-end materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0085] Figure 1 This is a process flow chart of the method for comprehensive utilization of coal gasification slag according to the present invention. DETAILED DESCRIPTION
[0086] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0087] like Figure 1 As shown, the comprehensive utilization method of the present invention comprises the following steps:
[0088] (1) First, the coal gasification slag is classified in a vibrating screen, a cyclone or a spiral classifier; second, it is re-selected in a sorting cyclone or a spiral chute; third, a regulator, a collector and a frother are sequentially added in a flotation machine or a flotation column for flotation to obtain a first high carbon slag, a medium carbon slag and a low carbon slag;
[0089] Wherein, the adjusting agent comprises sodium hexametaphosphate and / or water glass; the collecting agent comprises a compound solution of oleic acid and / or linoleic acid and kerosene; the frother comprises methyl isobutyl carbinol; the flotation comprises roughing, cleaning and scavenging in sequence; the medium carbon slag is used as a raw material for porous material and / or ceramic material;
[0090] (2) The low carbon slag obtained in step (1) is first acid-leached in an acid leaching solution to obtain an acid leaching solution and an acid leaching residue; the pH of the acid leaching solution is adjusted using potassium hydroxide, sodium hydroxide, calcium aluminate or carbide slag to obtain a ferroalloy and a water purifier; the acid leaching solution can also be mixed with the medium carbon slag in step (1) to be used as a raw material for porous materials and / or ceramic materials. Then, the acid leaching residue is alkaline-leached in an alkaline leaching solution to obtain a second high carbon slag and an alkaline leaching solution; the alkaline leaching solution is used as a raw material for water glass;
[0091] (3) The first high carbon slag is mixed with the second high carbon slag to obtain high carbon slag, first, the high carbon slag is immersed in a potassium hydroxide solution once; secondly, it is dried; thirdly, it is activated in a nitrogen atmosphere to obtain a carbon adsorption material; then, the carbon adsorption material is immersed in a hydrochloric acid solution for a second time, and then, it is washed with pure water, filtered and dried; the high carbon slag can also be used as thermal coal;
[0092] The first high carbon slag and the second high carbon slag are carbon slags with a loss on ignition greater than 80%, the medium carbon slag is carbon slag with a loss on ignition of 20-50%, and the low carbon slag is carbon slag with a loss on ignition less than 5%.
[0093] Example 1
[0094] This embodiment provides a method for comprehensive utilization of coal gasification slag, which comprises the following steps:
[0095] (1) First, the coal gasification slag is classified in a vibrating screen; second, it is re-selected in a spiral chute; third, 0.5 kg / t sodium hexametaphosphate, 10 kg / t collector and 5 kg / t methyl isobutyl carbinol are added in sequence in a flotation machine for flotation to obtain a first high carbon slag, a medium carbon slag and a low carbon slag;
[0096] The collector comprises a compound solution of 20 wt% oleic acid and 80 wt% kerosene; the flotation comprises one roughing selection, two cleaning selections and one scavenging selection in sequence; the medium carbon slag is used as a raw material for ceramic materials;
[0097] (2) the low carbon slag obtained in step (1) is first acid-leached in a 4 mol / L hydrochloric acid solution at 80°C for 120 min, and the mass ratio of the hydrochloric acid solution to the low carbon slag is controlled to be 3:1, to obtain an acid leaching solution and an acid leaching slag; the pH of the acid leaching solution is adjusted to 5 using potassium hydroxide to obtain a ferroalloy and a water purifier; then, the acid leaching slag is alkaline-leached in a 0.5 mol / L sodium hydroxide solution at a temperature of 90°C and a stirring speed of 500 rpm for 200 min to obtain a second high carbon slag and an alkaline leaching solution; and the alkaline leaching solution is used as water glass;
[0098] (3) The first high carbon slag and the second high carbon slag are mixed to obtain high carbon slag. First, the high carbon slag is immersed in a 3 mol / L potassium hydroxide solution at 25°C for 2 hours, and the mass ratio of the high carbon slag to the potassium hydroxide in the potassium hydroxide solution is controlled to be 1:1.5; secondly, it is dried at 160°C for 2 hours; thirdly, it is activated at 700°C for 2 hours under a nitrogen atmosphere of 300 mL / min to obtain a carbon adsorption material; then, the carbon adsorption material is immersed in a 10% hydrochloric acid solution at 25°C for a second time for 10 hours, and the mass ratio of the carbon adsorption material to the hydrochloric acid solution is controlled to be 1:3; then, it is washed with pure water, filtered, and then dried at 100°C for 5 hours;
[0099] Among them, the ignition loss of the first high carbon slag is 80.97%, the ignition loss of the second high carbon slag is 81.33%, the ignition loss of the medium carbon slag is 31.07% of the carbon slag, and the ignition loss of the low carbon slag is 4.51%.
[0100] Example 2
[0101] This embodiment provides a method for comprehensive utilization of coal gasification slag, which comprises the following steps:
[0102] (1) First, the coal gasification slag is classified in a vibrating screen; second, it is re-selected in a spiral chute; third, 1 kg / t of sodium hexametaphosphate, 12 kg / t of collector and 7 kg / t of methyl isobutyl carbinol are added in a flotation machine for flotation to obtain a first high carbon slag, a medium carbon slag and a low carbon slag;
[0103] The collector comprises a compound solution of 5wt% oleic acid and 95wt% kerosene; the flotation comprises two roughing selections, one fine selection and three scavenging selections in sequence; the medium carbon slag is used as a raw material for ceramic materials;
[0104] (2) the low carbon slag obtained in step (1) is first acid-leached in a 3 mol / L hydrochloric acid solution at 100°C for 30 min, and the mass ratio of the hydrochloric acid solution to the low carbon slag is controlled to be 2:1, to obtain an acid leaching solution and an acid leaching slag; the pH of the acid leaching solution is adjusted to pH 4 using sodium hydroxide to obtain a ferroalloy and a water purifier; then, the acid leaching slag is alkaline-leached in a 5 mol / L sodium hydroxide solution at a temperature of 60°C and a stirring speed of 200 rpm for 240 min to obtain a second high carbon slag and an alkaline leaching solution; and the alkaline leaching solution is used as water glass;
[0105] (3) The first high carbon slag and the second high carbon slag are mixed to obtain high carbon slag. First, the high carbon slag is immersed in a 4 mol / L potassium hydroxide solution at 30°C for 1 hour, and the mass ratio of the high carbon slag to the potassium hydroxide in the potassium hydroxide solution is controlled to be 1:3; secondly, it is dried at 100°C for 3 hours; thirdly, it is activated at 600°C for 3 hours under a nitrogen atmosphere of 325 mL / min to obtain a carbon adsorption material; then, the carbon adsorption material is immersed in a 20% hydrochloric acid solution at 30°C for a second time for 5 hours, and the mass ratio of the carbon adsorption material to the hydrochloric acid solution is controlled to be 1:2; then, it is washed with pure water, filtered, and then dried at 120°C for 4 hours;
[0106] Among them, the ignition loss of the first high carbon slag is 81.29%, the ignition loss of the second high carbon slag is 80.86%, the ignition loss of the medium carbon slag is 31.64% of the carbon slag, and the ignition loss of the low carbon slag is 3.25%.
[0107] Example 3
[0108] This embodiment provides a method for comprehensive utilization of coal gasification slag, which comprises the following steps:
[0109] (1) First, the coal gasification slag is classified in a vibrating screen; second, it is re-selected in a sorting cyclone; third, 2 kg / t of water glass, 1 kg / t of collector and 20 kg / t of methyl isobutyl carbinol are added in a flotation machine in sequence for flotation to obtain a first high carbon slag, a medium carbon slag and a low carbon slag;
[0110] The collector comprises a compound solution of 30 wt% linoleic acid and 70 wt% kerosene; the frother comprises; the flotation comprises 1 roughing, 3 cleaning and 2 scavenging in sequence; the medium carbon slag is used as a raw material for the porous material;
[0111] (2) the low carbon slag obtained in step (1) is first acid-leached in a 10 mol / L sulfuric acid solution at 20°C for 200 min, and the mass ratio of the sulfuric acid solution to the low carbon slag is controlled to be 6:1, to obtain an acid leaching solution and an acid leaching slag; the pH of the acid leaching solution is adjusted to 5 using calcium aluminate to obtain a ferroalloy and a water purifier; then, the acid leaching slag is alkaline-leached in a 3 mol / L potassium hydroxide solution at a temperature of 180°C and a stirring speed of 200 rpm for 60 min to obtain a second high carbon slag and an alkaline leaching solution; and the alkaline leaching solution is used as water glass;
[0112] (3) The first high carbon slag and the second high carbon slag are mixed to obtain high carbon slag. First, the high carbon slag is immersed in a 5 mol / L potassium hydroxide solution at 20°C for 3 hours, and the mass ratio of the high carbon slag to the potassium hydroxide in the potassium hydroxide solution is controlled to be 1:1; secondly, it is dried at 200°C for 1 hour; thirdly, it is activated at 900°C for 0.5 hour under a nitrogen atmosphere of 350 mL / min to obtain a carbon adsorption material; then, the carbon adsorption material is immersed in a 5% hydrochloric acid solution at 20°C for a second time for 24 hours, and the mass ratio of the carbon adsorption material to the hydrochloric acid solution is controlled to be 1:5; then, it is washed with pure water, filtered, and then dried at 80°C for 6 hours;
[0113] Among them, the ignition loss of the first high carbon slag is 80.88%, the ignition loss of the second high carbon slag is 80.54%, the ignition loss of the medium carbon slag is 25.66% of the carbon slag, and the ignition loss of the low carbon slag is 3.03%.
[0114] Example 4
[0115] This embodiment provides a method for comprehensive utilization of coal gasification slag, which comprises the following steps:
[0116] (1) First, the coal gasification slag is classified in a vibrating screen; second, it is re-selected in a spiral chute; third, 0.5 kg / t of water glass, 20 kg / t of collector and 1 kg / t of methyl isobutyl carbinol are added in sequence in a flotation machine for flotation to obtain a first high carbon slag, a medium carbon slag and a low carbon slag;
[0117] The collector comprises a mixed solution of 50 wt% oleic acid and linoleic acid and 50 wt% kerosene; the flotation comprises one roughing selection, one fine selection and one scavenging selection in sequence; the medium carbon slag is used as a raw material for ceramic materials;
[0118] (2) the low carbon slag obtained in step (1) is first acid-leached in a 7 mol / L sulfuric acid solution at 50°C for 100 min, and the mass ratio of the sulfuric acid solution to the low carbon slag is controlled to be 8:1, to obtain an acid leaching solution and an acid leaching slag; the pH of the acid leaching solution is adjusted to 5 using potassium hydroxide to obtain a ferroalloy and a water purifier; then, the acid leaching slag is alkaline-leached in a 2 mol / L alkaline leaching solution at a temperature of 140°C and a stirring speed of 300 rpm for 120 min to obtain a second high carbon slag and an alkaline leaching solution; and the alkaline leaching solution is used as water glass;
[0119] (3) The first high carbon slag and the second high carbon slag are mixed to obtain high carbon slag. First, the high carbon slag is immersed in a 4 mol / L potassium hydroxide solution at 20°C for 3 hours, and the mass ratio of the high carbon slag to the potassium hydroxide in the potassium hydroxide solution is controlled to be 1:1; secondly, it is dried at 200°C for 1 hour; thirdly, it is activated at 900°C for 0.75 hours under a nitrogen atmosphere of 350 mL / min to obtain a carbon adsorption material; then, the carbon adsorption material is immersed in a 15% hydrochloric acid solution at 20°C for 20 hours, and the mass ratio of the carbon adsorption material to the hydrochloric acid solution is controlled to be 1:4; then, it is washed with pure water, filtered, and then dried at 100°C for 5 hours;
[0120] Among them, the ignition loss of the first high carbon slag is 82.30%, the ignition loss of the second high carbon slag is 80.27%, the ignition loss of the medium carbon slag is 41.90%, and the ignition loss of the low carbon slag is 3.25%.
[0121] Example 5
[0122] This embodiment provides a method for comprehensive utilization of coal gasification slag, which refers to the method for comprehensive utilization of coal gasification slag described in Example 1, with the only difference being that the activation temperature in step (3) is replaced from 700°C to 400°C.
[0123] Example 6
[0124] This embodiment provides a method for comprehensive utilization of coal gasification slag, which refers to the method for comprehensive utilization of coal gasification slag described in Example 1, with the only difference being that the activation temperature in step (3) is replaced from 700°C to 1000°C.
[0125] Example 7
[0126] This embodiment provides a method for comprehensive utilization of coal gasification slag, which refers to the method for comprehensive utilization of coal gasification slag described in Example 1, except that after the activation in step (3), secondary impregnation, washing, solid-liquid separation and secondary drying are not performed in sequence; that is, the specific steps of step (3) are as follows:
[0127] (3) The first high carbon slag is mixed with the second high carbon slag to obtain high carbon slag. First, the high carbon slag is immersed in a 3 mol / L potassium hydroxide solution at 25°C for 2 h, and the mass ratio of the high carbon slag to the potassium hydroxide in the potassium hydroxide solution is controlled to be 1:1.5; secondly, it is dried at 160°C for 2 h; and thirdly, it is activated at 700°C for 2 h under a nitrogen atmosphere of 300 mL / min to obtain a carbon adsorption material.
[0128] Comparative Example 1
[0129] This comparative example provides a method for comprehensive utilization of coal gasification slag, referring to the method for comprehensive utilization of coal gasification slag described in Example 1, except that no carbon ash separation is performed; that is, the comprehensive utilization method comprises the following steps:
[0130] (1) firstly subjecting the coal gasification slag to acid leaching in a 4 mol / L hydrochloric acid solution at 80°C for 120 min, controlling the mass ratio of the hydrochloric acid solution to the coal gasification slag to be 3:1, to obtain an acid leaching solution and an acid leaching slag; using potassium hydroxide to control the pH of the acid leaching solution to a pH of 5, to obtain a ferroalloy and a water purifier; then, subjecting the acid leaching slag to alkaline leaching in a 0.5 mol / L sodium hydroxide solution at a temperature of 90°C and a stirring speed of 500 rpm for 200 min, to obtain an alkaline leaching slag and an alkaline leaching solution; and using the alkaline leaching solution as water glass;
[0131] (2) First, the alkali leaching residue was immersed in a 3 mol / L potassium hydroxide solution at 25°C for 2 h, and the mass ratio of the alkali leaching residue to the potassium hydroxide in the potassium hydroxide solution was controlled to be 1:1.5; secondly, it was dried at 160°C for 2 h; thirdly, it was activated at 700°C for 2 h under a nitrogen atmosphere of 300 mL / min to obtain a carbon adsorption material; then, the carbon adsorption material was immersed in a 10% hydrochloric acid solution at 25°C for a second time for 10 h, and the mass ratio of the carbon adsorption material to the hydrochloric acid solution was controlled to be 1:3; then, it was washed with pure water, filtered, and then dried at 100°C for 5 h.
[0132] Comparative Example 2
[0133] This comparative example provides a method for comprehensive utilization of coal gasification slag, which refers to the method for comprehensive utilization of coal gasification slag described in Example 1, except that acid leaching and alkali leaching are not performed; that is, the comprehensive utilization method comprises the following steps:
[0134] The comprehensive utilization method comprises the following steps:
[0135] (1) First, the coal gasification slag is classified in a vibrating screen; second, it is re-selected in a spiral chute; third, 0.5 kg / t sodium hexametaphosphate, 10 kg / t collector and 5 kg / t methyl isobutyl carbinol are added in a flotation machine for flotation to obtain high carbon slag, medium carbon slag and low carbon slag;
[0136] The collector comprises a mixed solution of 20 wt% oleic acid and 80 wt% kerosene; the flotation comprises one roughing selection, two cleaning selections and one scavenging selection in sequence; the medium carbon slag is used as a raw material for porous materials and / or ceramic materials; the low carbon slag is directly used as a building material;
[0137] (2) First, the high carbon slag obtained in step (1) is immersed in a 3 mol / L potassium hydroxide solution at 25°C for 2 hours, and the mass ratio of the high carbon slag to the potassium hydroxide in the potassium hydroxide solution is controlled to be 1:1.5; secondly, it is dried at 160°C for 2 hours; thirdly, it is activated at 700°C for 2 hours under a nitrogen atmosphere of 300 mL / min to obtain a carbon adsorption material; then, the carbon adsorption material is immersed in a 10% hydrochloric acid solution at 25°C for a second time for 10 hours, and the mass ratio of the carbon adsorption material to the hydrochloric acid solution is controlled to be 1:3; then, it is washed with pure water, filtered, and then dried at 100°C for 5 hours;
[0138] Among them, the loss on ignition of high carbon slag is 80.97%, the loss on ignition of medium carbon slag is 31.07%, and the loss on ignition of low carbon slag is 4.51%.
[0139] (I) The specific surface area of the carbon adsorption materials obtained in the above examples and comparative examples was tested by the following method: the test was performed by the BET specific surface area test method.
[0140] The test results of the specific surface areas of the above embodiments and comparative examples are listed in Table 1.
[0141] (II) The adsorption capacity of the carbon adsorption materials obtained in the above examples and comparative examples was tested, and the test method was as follows:
[0142] A carbon adsorbent material with a mass of M is placed in a methylene blue solution with a volume of V and an initial concentration of C0. After oscillating on an oscillator for 1 hour, a sample is taken to test the concentration of the remaining methylene blue in the solution, which is recorded as C i , the adsorption amount of methylene blue can be obtained by calculation, that is, the adsorption amount of methylene blue = (C0-C i )×V / M, where C0=2.5g / L, V=0.05L and M=0.1g.
[0143] The test results of the adsorption capacity of the above examples and comparative examples are listed in Table 1.
[0144] (III) The alkaline leaching solution obtained in the above embodiments and comparative examples was used as water glass, and the modulus of the water glass was tested. The test method is as follows:
[0145] The silicon ion content and sodium ion content in water glass are determined by inductively coupled plasma spectrometer (ICP), and converted into silicon dioxide molar content and sodium oxide molar content. The ratio of silicon dioxide molar content to sodium oxide molar content is the modulus of water glass.
[0146] The modulus test results of the waterglass obtained in the above examples and comparative examples are listed in Table 1.
[0147] Table 1
[0148] project <![CDATA[Specific surface area / m 2 ·g -1 > <![CDATA[Adsorption capacity / mg·g -1 > Water glass modulus Example 1 1842 619 3.55 Example 2 1585 611 3.51 Example 3 1434 608 3.48 Example 4 1717 615 3.52 Example 5 429 303 3.55 Example 6 433 308 3.55 Example 7 468 316 3.55 Comparative Example 1 221 209 1.94 Comparative Example 2 1578 610 /
[0149] From Table 1, we can draw the following conclusions:
[0150] (1) As can be seen from Examples 1-4, the comprehensive utilization method of coal gasification slag of the present invention adopts a carbon ash separation process to prepare a carbon adsorption material and a silicon-based water glass. The obtained carbon adsorption material has a large specific surface area and a high adsorption capacity, and the obtained water glass has a high modulus;
[0151] (2) By comparing Example 1 with Examples 5 and 6, it can be found that since the activation temperature in step (3) of Example 5 is 400°C, which is lower than the preferred 600-900°C of the present invention, the activation reaction is incomplete, the pores are small, and the specific surface area is greatly reduced; since the activation temperature in step (3) of Example 6 is 1000°C, which exceeds the preferred 600-900°C of the present invention, the temperature is too high, resulting in micropore collapse and a decrease in the specific surface area;
[0152] (3) By comparing Example 1 with Example 7, it can be found that after the activation in step (3), Example 7 did not perform secondary impregnation, washing, solid-liquid separation and secondary drying in sequence; the secondary impregnation was performed using hydrochloric acid to remove impurities and form pores. Since Example 7 did not perform secondary impregnation after activation, the carbon adsorption material had fewer pores and a reduced specific surface area, which in turn led to a decrease in adsorption capacity;
[0153] (4) By comparing Example 1 with Comparative Example 1, it can be found that since Comparative Example 1 did not perform carbon ash separation, the ignition loss of the residue produced after acid leaching and alkali leaching was only 50.53%, the resource utilization efficiency was low, the modulus of the obtained silicon-based water glass was low, and the specific surface area of the obtained carbon adsorption material decreased to 221m 2 ·g -1 , the adsorption amount decreased to 209 mg·g -1 ;
[0154] (5) By comparing Example 1 with Comparative Example 2, it can be found that since Comparative Example 2 did not undergo acid leaching and alkali leaching, resource utilization could not be achieved, and thus ferroalloy, aluminum-based water purifiers and silicon-based water glass could not be obtained.
[0155] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for comprehensive utilization of coal gasification slag, characterized in that: The comprehensive utilization method comprises the following steps: (1) separating the coal gasification slag into carbon ash to obtain a first high-carbon slag, a medium-carbon slag and a low-carbon slag; (2) subjecting the low carbon slag obtained in step (1) to acid leaching to obtain an acid leaching solution and an acid leaching slag; and subjecting the acid leaching slag to alkali leaching to obtain a second high carbon slag and an alkali leaching solution; (3) activating the first high carbon slag in step (1) and the second high carbon slag in step (2) to obtain a carbon adsorption material; The first high carbon slag and the second high carbon slag are both carbon slags with a loss on ignition greater than 80%, the medium carbon slag is carbon slag with a loss on ignition of 20-50%, and the low carbon slag is carbon slag with a loss on ignition less than 5%.
2. The comprehensive utilization method according to claim 1, characterized in that: The carbon ash separation in step (1) includes classification, gravity separation and flotation performed in sequence.
3. The comprehensive utilization method according to claim 2, characterized in that: The classification equipment includes any one of a vibrating screen, a cyclone or a spiral classifier, or a combination of at least two of them.
4. The comprehensive utilization method according to claim 2, characterized in that: The re-selection equipment includes a sorting cyclone and / or a spiral chute.
5. The comprehensive utilization method according to claim 2, characterized in that: The flotation equipment includes a flotation machine and / or a flotation column.
6. The comprehensive utilization method according to claim 2, characterized in that: During the flotation process, a regulator, a collector and a frother are added in sequence.
7. The comprehensive utilization method according to claim 6, characterized in that: The adjusting agent includes sodium hexametaphosphate and / or water glass.
8. The comprehensive utilization method according to claim 6, characterized in that: The dosage of the adjusting agent is 0.5-2kg / t.
9. The comprehensive utilization method according to claim 6, characterized in that: The collector comprises a composite solution of oleic acid, linoleic acid and kerosene.
10. The comprehensive utilization method according to claim 9, characterized in that: The sum of the contents of oleic acid and linoleic acid in the composite solution is 5-50 wt %.
11. The comprehensive utilization method according to claim 9, characterized in that: The content of kerosene in the composite solution is 50-95wt%.
12. The comprehensive utilization method according to claim 6, characterized in that: The dosage of the collector is 1-20 kg / t.
13. The comprehensive utilization method according to claim 6, characterized in that: The blowing agent includes methyl isobutyl carbinol.
14. The comprehensive utilization method according to claim 6, characterized in that: The dosage of the foaming agent is 1-20 kg / t.
15. The comprehensive utilization method according to claim 2, characterized in that: The flotation comprises roughing, cleaning and scavenging which are carried out in sequence.
16. The comprehensive utilization method according to claim 15, characterized in that: The number of times of rough selection is 1-2 times.
17. The comprehensive utilization method according to claim 15, characterized in that: The number of times of selection is 1-3 times.
18. The comprehensive utilization method according to claim 15, characterized in that: The scanning is performed 1 to 3 times.
19. The comprehensive utilization method according to claim 1, characterized in that: The concentration of the acid leaching solution used in the acid leaching in step (2) is 3-10 mol / L.
20. The comprehensive utilization method according to claim 19, characterized in that: The solute of the acid leaching solution includes any one of hydrochloric acid, nitric acid or sulfuric acid, or a combination of at least two of them.
21. The comprehensive utilization method according to claim 19, characterized in that: The mass ratio of the acid leaching solution to the low-carbon slag is (2-8):
1.
22. The comprehensive utilization method according to claim 1, characterized in that: The temperature of the acid leaching in step (2) is 20-100°C.
23. The comprehensive utilization method according to claim 1, characterized in that: The acid leaching time in step (2) is 30-200 minutes.
24. The comprehensive utilization method according to claim 1, characterized in that: The comprehensive utilization method further comprises: controlling the pH value of the acid leaching solution in step (2) to obtain ferroalloy and water purifier.
25. The comprehensive utilization method according to claim 24, characterized in that: The reagent used for pH control includes any one of potassium hydroxide, sodium hydroxide, calcium aluminate or carbide slag, or a combination of at least two of them.
26. The comprehensive utilization method according to claim 24, characterized in that: The end point pH of the pH regulation is 3-5.
27. The comprehensive utilization method according to claim 1, characterized in that: The concentration of the alkali leaching solution used in the alkali leaching in step (2) is 0.5-5 mol / L.
28. The comprehensive utilization method according to claim 27, characterized in that: The solute of the alkaline leaching solution includes sodium hydroxide and / or potassium hydroxide.
29. The comprehensive utilization method according to claim 1, characterized in that: The temperature of the alkali leaching in step (2) is 60-180°C.
30. The comprehensive utilization method according to claim 1, characterized in that: The alkali leaching time in step (2) is 60-240 minutes.
31. The comprehensive utilization method according to claim 1, characterized in that: The stirring speed of the alkali leaching in step (2) is 200-500 rpm.
32. The comprehensive utilization method according to claim 1, characterized in that: The comprehensive utilization method also includes: using the medium carbon slag in step (1) as a raw material for porous materials and / or ceramic materials; and using the alkaline leaching solution in step (2) as a raw material for water glass.
33. The comprehensive utilization method according to claim 1, characterized in that: Before the activation in step (3), the first high carbon slag and the second high carbon slag are sequentially mixed, impregnated once and dried once.
34. The comprehensive utilization method according to claim 33, characterized in that: The first high carbon slag and the second high carbon slag are mixed to obtain high carbon slag.
35. The comprehensive utilization method according to claim 33, characterized in that: The primary impregnation liquid used in the primary impregnation includes a potassium hydroxide solution.
36. The comprehensive utilization method according to claim 35, characterized in that: The concentration of the primary impregnation solution is 3-5 mol / L.
37. The comprehensive utilization method according to claim 35, characterized in that: The mass ratio of the high carbon slag to the solute in the primary impregnation solution is 1:(1-3).
38. The comprehensive utilization method according to claim 33, characterized in that: The time of the first immersion is 1-3 hours.
39. The comprehensive utilization method according to claim 33, characterized in that: The temperature of the primary immersion is 20-30°C.
40. The comprehensive utilization method according to claim 33, characterized in that: The primary drying temperature is 100-200°C.
41. The comprehensive utilization method according to claim 33, characterized in that: The time of the primary drying is 1-3h.
42. The comprehensive utilization method according to claim 1, characterized in that: The activation temperature in step (3) is 600-900°C.
43. The comprehensive utilization method according to claim 1, characterized in that: The activation time in step (3) is 0.5-3h.
44. The comprehensive utilization method according to claim 1, characterized in that: The activation in step (3) is carried out under a nitrogen atmosphere.
45. The comprehensive utilization method according to claim 44, characterized in that: The flow rate of the nitrogen is 300-350 mL / min.
46. The comprehensive utilization method according to claim 1, characterized in that: The carbon adsorption material in step (3) is sequentially subjected to secondary impregnation, washing, solid-liquid separation and secondary drying.
47. The comprehensive utilization method according to claim 46, characterized in that: The secondary impregnation liquid used in the secondary impregnation includes a hydrochloric acid solution.
48. The comprehensive utilization method according to claim 47, characterized in that: The content of solute in the secondary impregnation solution is 5-20%.
49. The comprehensive utilization method according to claim 47, characterized in that: The mass ratio of the carbon adsorption material to the secondary impregnation liquid is 1:(2-5).
50. The comprehensive utilization method according to claim 46, characterized in that: The secondary impregnation time is 5-24h.
51. The comprehensive utilization method according to claim 46, characterized in that: The temperature of the secondary impregnation is 20-30°C.
52. The comprehensive utilization method according to claim 46, characterized in that: The cleaning agent used in the cleaning includes pure water.
53. The comprehensive utilization method according to claim 46, characterized in that: The solid-liquid separation method is suction filtration.
54. The comprehensive utilization method according to claim 46, characterized in that: The temperature of the secondary drying is 80-120°C.
55. The comprehensive utilization method according to claim 46, characterized in that: The secondary drying time is 4-6 hours.
56. The comprehensive utilization method according to claim 1, characterized in that: The comprehensive utilization method comprises the following steps: (1) First, the coal gasification slag is classified in a vibrating screen, a cyclone or a spiral classifier; second, it is re-selected in a sorting cyclone or a spiral chute; third, 0.5-2 kg / t of a regulator, 1-20 kg / t of a collector and 1-20 kg / t of a frother are added in sequence in a flotation machine or a flotation column for flotation to obtain a first high carbon slag, a medium carbon slag and a low carbon slag; The adjusting agent comprises sodium hexametaphosphate and / or water glass; the collecting agent comprises a compound solution of 5-50wt% oleic acid and linoleic acid and 50-95wt% kerosene; the frother comprises methyl isobutyl carbinol; the flotation comprises 1-2 roughing selections, 1-3 cleaning selections and 1-3 scavenging selections in sequence; the medium carbon slag is used as a raw material for porous materials and / or ceramic materials; (2) firstly subjecting the low carbon slag obtained in step (1) to acid leaching in a 3-10 mol / L acid leaching solution at 20-100° C. for 30-200 min, controlling the mass ratio of the acid leaching solution to the low carbon slag to (2-8):1, to obtain an acid leaching solution and an acid leaching slag; using potassium hydroxide, sodium hydroxide, calcium aluminate or carbide slag to control the pH of the acid leaching solution to a pH of 3-5, to obtain a ferroalloy and a water purifier; then, subjecting the acid leaching slag to alkaline leaching in a 0.5-5 mol / L alkaline leaching solution at a temperature of 60-180° C. and a stirring speed of 200-500 rpm for 60-240 min, to obtain a second high carbon slag and an alkaline leaching solution; and using the alkaline leaching solution as a raw material for water glass; (3) The first high carbon slag and the second high carbon slag are mixed to obtain high carbon slag. First, the high carbon slag is immersed in a 3-5 mol / L potassium hydroxide solution at 20-30°C for 1-3 hours, and the mass ratio of the high carbon slag to the potassium hydroxide in the potassium hydroxide solution is controlled to be 1:(1-3); secondly, it is dried at 100-200°C for 1-3 hours; thirdly, it is activated at 600-900°C for 0.5-3 hours under a nitrogen atmosphere of 300-350 mL / min to obtain a carbon adsorption material; then, the carbon adsorption material is immersed in a 5-20% hydrochloric acid solution at 20-30°C for a second time for 5-24 hours, and the mass ratio of the carbon adsorption material to the hydrochloric acid solution is controlled to be 1:(2-5); then, it is washed with pure water, filtered, and then dried at 80-120°C for 4-6 hours; The first high carbon slag and the second high carbon slag are both carbon slags with a loss on ignition greater than 80%, the medium carbon slag is carbon slag with a loss on ignition of 20-50%, and the low carbon slag is carbon slag with a loss on ignition less than 5%.
Citation Information
Patent Citations
Method for treating coal chemical gasified slag
CN102980195A
Lightweight ceramisite prepared from coal ashes and gasification slag as well as preparation method and application thereof
CN104774023A
Composition for producing filter ceramic and the filter ceramic, and preparation method and application thereof
CN105130487A
Preparation method of insulating baking-free brick
CN106336164A
Burning-free brick preparation process method
CN106467376A