In / H-Beta@CeO2 catalyst and its preparation method and application
Prepared through the self-assembly method of In/H-Beta@CeO2 catalyst, the CeO2 protective layer is used to encapsulate In/H-Beta to form a porous structure, which solves the problem of deactivation of the active sites of the catalyst in H2O and SO2 environments, and significantly improves the efficiency of the catalyst. NOx conversion rate and denitrification efficiency.
Patent Information
- Application Number
- CN202310143044.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-21
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-21
AI Technical Summary
The active sites of existing In/H-Beta catalysts are deactivated in the presence of H2O and SO2, resulting in a decrease in NOx conversion rate, making it difficult to effectively remove NOx pollutants under harsh conditions.
In/H-Beta@CeO2 catalyst is used to prepare a core-shell catalyst through self-assembly method. CeO2 is used as a protective layer to encapsulate In/H-Beta to form a porous structure, which weakens the poisoning effect of H2O and SO2 and maintains the catalyst activity.
Under the conditions of 5vol% H2O and 100ppm SO2, the NOx conversion rate of In/H-Beta@CeO2 increased by 23% and reached 57.7% at 625°C, which significantly improved the denitrification efficiency and stability of the catalyst.
Smart Images

Figure CN116078423B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to an In / H-Beta@CeO2 catalyst and a preparation method and application thereof. Background Art
[0002] Nitrogen oxides (NO x ) is one of the most serious air pollutants affecting the environment and human health. x (CH4-SCR) has the advantages of easy use, simple operation, low maintenance cost, and abundant CH4 reserves. It is a promising method for removing NO x pollutants. However, due to the presence of H2O and SO2 in most purification systems, catalysts face the problem of active site deactivation during use. Therefore, for the practical application of CH4-SCR, it is urgent to develop catalysts with protected active sites. Various zeolite, alumina and transition metal-based catalysts have been reported for use in CH4-SCR denitrification systems, among which metal-exchanged zeolite catalysts have received increasing attention due to their high catalytic activity over a wide temperature range.
[0003] Research results show that in a water-free and sulfur-free environment, In / H-Beta catalysts exhibit excellent NO x However, in the presence of H2O and SO2, its performance dropped from over 90% to around 31%. This suggests that on In / H-Beta, the presence of SO2 competes with NO on the (InO)+ adsorption sites to form sulfate species, while H2O inhibits NO 3- The formation of In / H-beta hinders the further reaction of the catalyst. Therefore, in order to increase the active sites of In / H-Beta, existing researchers have adopted a variety of strategies. For example, Zhao et al. used amino acids to regulate the acid sites and surface oxygen species of In / H-beta; Zhao et al. introduced Co3O4 and Ga2O3 into In / H-beta to regulate The number of (Brønsted) acid sites. However, the protection of In / H-Beta active sites remains a serious problem. Therefore, constructing sacrificial sites or catalyst protection layers is an effective way to protect the catalyst from H2O and SO2 poisoning, and is one of the directions to improve the catalyst's ability to perform CH4-SCR catalytic denitrification in H2O and SO2 environments. Summary of the invention
[0004] In view of the above technical problems, the present invention discloses an In / H-Beta@CeO2 catalyst and its preparation method and application, which improves the performance of the catalyst in removing NO with CH4 as a reducing agent under harsh conditions. xThe ability of pollutants.
[0005] To this end, the technical solution adopted by the present invention is:
[0006] The preparation method of In / H-Beta@CeO2 catalyst comprises the following steps:
[0007] Step S1, ultrasonically dispersing H-Beta powder in a solvent, adding a surface stabilizer, a Ce source, a structure directing agent, and a pore-forming agent in sequence during stirring, and then refluxing and stirring at 55-65° C. for 1.5-2.5 hours, and then centrifuging and washing, drying, and calcining at 450-550° C. for 2-5 hours to obtain H-Beta@CeO2;
[0008] Step S2, adding the obtained H-Beta@CeO2 to the In source solution, stirring at a constant temperature of 75-85°C for 6-12h, filtering, washing, drying, and calcining at 450-550°C for 2-5h to obtain the product In / H-Beta@CeO2.
[0009] Using this technical solution, the core-shell catalyst In / H-Beta@CeO2 obtained by self-assembly has a unique mesoporous structure with high pore volume and pore size, which allows reactants to enter and exit the shell. Performance studies have shown that In / H-Beta@CeO2 has a NO x The conversion rate is as high as 57.7%, which is 23% higher than that of In / H-Beta. In-situ DRIFTS experiments confirmed that In / H-Beta@CeO2 has good active sites, and its amorphous porous core-shell structure protects the active sites and limits the formation of sulfate species on its surface. Different characterization techniques also confirmed that In / H-Beta@CeO2 contains a high content of Ce. 3+ / Ce total , surface oxygen species (O β / O total ), maintaining an appropriate balance between acidity and redox performance. Therefore, the In / H-Beta@CeO2 core-shell catalyst has potential application value in CH4-SCR mobile source and fixed source combustion devices. As a further improvement of the present invention, in step S1, the solvent is an ethanol aqueous solution.
[0010] As a further improvement of the present invention, in step S1 and step S2, calcination is performed under a nitrogen atmosphere. With this technical solution, the obtained catalyst has a higher catalytic activity.
[0011] As a further improvement of the present invention, in step S1, the surface stabilizer is polyvinyl pyrrolidone (PVP), and the mass ratio of the PVP to H-Beta is 2.5-10. Further, the mass ratio of the PVP to H-Beta is 2.5-7.5. Further, the mass ratio of the PVP to H-Beta is 2.5-5. Further, the mass ratio of the PVP to H-Beta is 5.
[0012] As a further improvement of the present invention, in step S1, the structure directing agent is HMTA. Further, the mass ratio of HMTA to H-Beta is 0.15-0.45. Further, the mass ratio of HMTA to H-Beta is 0.15-0.3.
[0013] As a further improvement of the present invention, the pore-forming agent is CTAB.
[0014] As a further improvement of the present invention, the Ce source is Ce(NO3)3; further, the mass ratio of Ce(NO3)3 to H-Beta is 0.2-0.4. Further, the mass ratio of Ce(NO3)3 to H-Beta is 0.4.
[0015] As a further improvement of the present invention, the method further comprises step S3, mixing ZrO2-Co3O4 with In / H-Beta@CeO2. Furthermore, the mass ratio of ZrO2-Co3O4 to In / H-Beta@CeO2 is 1-4:1.
[0016] The present invention also discloses an In / H-Beta@CeO2 catalyst, which is prepared by the preparation method of the In / H-Beta@CeO2 catalyst as described above.
[0017] As a further improvement of the present invention, the In / H-Beta@CeO2 catalyst is used in CH4-SCR for denitrification treatment.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] First, the catalyst of the technical solution of the present invention adopts a core-shell structure, with In / H-Beta as the core and CeO2 as the protective layer. The catalyst active substance is encapsulated in a porous shell, an appropriate amount of CeO2 is introduced and the integrity of the In / H-Beta structure is maintained, thereby weakening the poisoning effect of H2O and SO2, allowing reactants to enter and exit, and maintaining the stability of the active sites in harsh environments, thereby improving the denitrification efficiency.
[0020] Second, by adopting the technical solution of the present invention, CeO2 has good redox performance and oxygen storage capacity. 3+The ionic radius is 94 pm, Ce 3+ The higher ionic radius (115 pm) can reduce the oxygen migration barrier. In addition, CeO2 has a strong interaction with SO2, which can slow down the catalyst deactivation.
[0021] Third, the technical solution of the present invention overcomes the core-shell interfacial tension by a self-assembly method of covering CeO2 on In / H-Beta through chemical bonds, obtains a relatively uniform shell layer, and compared with liquid phase deposition and in situ growth methods, it basically does not damage H-Beta during the preparation process, so that the catalyst has better denitrification activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a schematic diagram of the preparation route of the In / H-Beta@CeO2 catalyst of the present invention.
[0023] Figure 2 1 and 2 are XRD spectra of the catalysts of the embodiments of the present invention and the comparative examples and the adsorption-desorption isothermal pore size distribution curves of nitrogen at 77K, wherein (a) is the XRD spectra and (b) is the adsorption-desorption isothermal pore size distribution curve.
[0024] Figure 3 2 are microstructure analysis diagrams of the catalysts of the embodiments of the present invention and the comparative examples, wherein (a) is a SEM image and (b) is an EDX mapping analysis diagram showing the distribution of Ce and In in different samples.
[0025] Figure 4 These are high-angle annular dark field scanning transmission electron microscopy images and elemental mapping images of the catalysts of the embodiments of the present invention and the comparative examples; wherein (a) and (b) are STEM-HAADF images of IB (In / H-Beta) at different magnification ratios, (c) is an elemental mapping image of In / H-Beta@CeO2-0.04 (IB@Ce-2), (d) and (e) are high-angle annular dark field scanning transmission electron microscopy images of In / H-Beta / CeO2 (IBCe) at different magnification ratios, and (f) is an elemental mapping image of IBCe.
[0026] Figure 5 are HRTEM images of the catalysts of the embodiments of the present invention and the comparative examples; wherein, (a) is In / H-Beta (IB), (b) is IB@Ce-2, (c) is In / H-Beta@CeO2-0.08 (IB@Ce-3), and (d) is IBCe.
[0027] Figure 6Spectra of the catalysts of the embodiments and comparative examples of the present invention; wherein, (a) to (c) are XPS spectra, (d) is an NH3-TPD spectrum, (e) is a Py-IR spectrum, and (f) is a H2-TPR spectrum.
[0028] Figure 7 The catalysts of the present invention and the comparative example are different in 400ppm NO, 400ppm CH4, 10vol% O2, 100vol% SO2, 5vol% H2O at GHSV 23,600h -1 The catalytic activity results under the conditions of (a) NO x Conversion rate (%), (b) is CH4 conversion rate, and (c) is CH4 selectivity.
[0029] Figure 8 3 are the in situ infrared spectra of IB and IB@Ce-2 in the embodiments of the present invention and the comparative examples in the presence of O2 and H2O; wherein, (a) to (c) are the in situ infrared spectra of IB, and (d) to (f) are the in situ infrared spectra of IB@Ce-2.
[0030] Fig. 9 These are the CH4-SCR denitration activity results of different catalysts in Example 1 of the present invention and Comparative Example 3.
[0031] Fig.10 These are the CH4-SCR denitration activity results of the catalysts obtained with different PVP contents in Example 1 of the present invention and Comparative Example 4.
[0032] Fig.11 These are the CH4-SCR denitration activity results of the catalysts obtained with different HMTA contents in Example 1 of the present invention and Comparative Example 5.
[0033] Fig.12 The NO of the catalysts mixed in different proportions in Example 3 and Comparative Example 6 of the present invention is x Conversion rate.
[0034] Fig.13 It is the CH4 conversion rate of the catalysts mixed in different proportions in Example 3 of the present invention and Comparative Example 6. DETAILED DESCRIPTION
[0035] The preferred embodiments of the present invention are described in further detail below.
[0036] Preparation method of In / H-Beta@CeO2 catalyst, such as Figure 1 As shown, it mainly includes two steps, as follows:
[0037] Step S1, adding H-Beta (SiO2 / Al2O3=25) powder into a water / ethanol (volume ratio 1:1) solvent for ultrasonic dispersion, then adding a surface stabilizer PVP, Ce(NO3)3, a structure directing agent HMTA, and a pore-forming agent CTAB in sequence, stirring, refluxing and stirring at 60°C for 2h, then centrifuging, washing, drying, and calcining at 500°C in a nitrogen atmosphere for 3h to obtain H-Beta@CeO2;
[0038] Step S2, adding the obtained H-Beta@CeO2 to the In(NO3)3 solution, stirring at a constant temperature of 80°C for 8 hours, filtering, washing, drying, and calcining at 500°C in a nitrogen atmosphere for 3 hours to obtain the product In / H-Beta@CeO2.
[0039] The core-shell catalyst uses polyvinyl pyrrolidone (PVP) as a surface stabilizer and nanoparticle dispersant to prevent CeO2 particle agglomeration, hexamethylenetetramine (HMTA) as a structure-directing agent, and cetyltrimethylammonium bromide (CTAB) as a pore-forming agent to form a porous structure and allow NO x The above steps adopt a self-assembly method to first encapsulate H-Beta into the CeO2 shell layer, and then introduce indium metal oxide into the pore structure of the intermediate material through ion exchange.
[0040] The following describes it in conjunction with specific embodiments.
[0041] Example 1
[0042] 0.1 g H-Beta powder was ultrasonically dispersed in 100 ml water / ethanol (v / v=1) mixed solvent, and 0.5 g PVP, 0.04 g Ce(NO3)2·6H2O, 0.03 g HMTA and 0.1 g CTAB were added successively under stirring. The mixture was refluxed and stirred at 60°C for 2 h. After the mixture was centrifuged and washed with deionized water, dried in air at 80°C overnight, and calcined in nitrogen environment at 500°C for 3 h. The sample was collected as H-Beta@CeO2.
[0043] The H-Beta@CeO2 sample was added to a 0.033 M In(NO3)3 solution and stirred at 80°C for 8 h. The product was obtained by filtration, washing, drying, and calcination at 500°C for 3 h. The catalyst In / H-Beta@CeO2 was obtained and named IB@Ce-2.
[0044] Example 2
[0045] Based on Example 1, the difference of this comparative example is that the added amount of Ce(NO3)2·6H2O is 0.02 g, and the rest is the same as Example 1. The obtained product is named IB@Ce-1.
[0046] Comparative Example 1
[0047] Based on Example 1, the difference of this comparative example is that the added amount of Ce(NO3)2·6H2O is 0.08 g, and the rest is the same as Example 1. The obtained product is named IB@Ce-3.
[0048] Comparative Example 2
[0049] As a comparative example, 0.04 g Ce(NO3)2·6H2O was dissolved in 0.1 g In / H-beta by wet impregnation method, which is a common method for introducing metal sites into zeolite. After drying at 80°C, it was calcined in a nitrogen environment at 500°C. The obtained sample was named IBCe.
[0050] The morphology and microstructure of the catalysts were examined by high-angle annular dark field scanning transmission electron microscopy (STEM-HAADF) and scanning electron microscopy (SEM, HITACHI S-4800), both equipped with energy dispersive X-ray spectroscopy (EDX) mapping analysis. A Rigaku D / MAX 2500PC X-ray diffractometer equipped with Cu Kα radiation was used at 40 kV, 200 mA, and a scan rate of 4 ° min -1 Under the conditions of , x-ray diffraction (XRD) patterns reflecting the phase composition and crystal structure were obtained. Its structural properties were analyzed by N2 adsorption and desorption measurements (Micromeritics 2020HD88 instrument). X-ray photoelectron spectroscopy (XPS) tests were carried out on an ESCALAB MK-II spectrometer from VG Scientific, USA, using Al Kα (hν=1486.6eV, 15kV, 20mA) as the radiation source. The element content was analyzed by inductively coupled plasma atomic emission spectrometry (ICP-OES) (Agilent, Technologies, model 5100). Ammonia temperature-programmed desorption experiments (NH3-TPD) and hydrogen temperature-programmed reduction experiments (H2-TPR) were carried out on Micromeritics (AutoChem1 II2920) to study the acidity and redox properties of the catalyst. NH3-TPD was exposed to 5vol% NH3 / N2, and H2-TPR was exposed to 10vol% H2 / Ar with a flow rate of 30ml min -1 , the temperature ranged from 50°C to 650°C. Before each experiment, 0.05 g of catalyst was heated at 500°C (10°C min -1 ) with He or N2 gas (30 mL min -1) was degassed for 2 h and then cooled to 50 °C. In addition, pyridine-infrared (Py-IR) spectroscopy (Thermo fisher Nicolet iS50) was used to quantify and Lewis acid sites.
[0051] Catalytic activity evaluation: CH4-SCR test was carried out in a fixed bed continuous flow reactor using the temperature programmed surface reaction (TPSR) technique. The reaction gas contained 400ppm NO, 400ppm CH4, 10vol% O2, 100ppm SO2 and 5vol% H2O, with Ar as the balance gas and a flow rate of 100ml min -1 , airspeed is 23600h -1 , using 0.1g of sample, the particle size ranged from 40 to 60 mesh. First, it was balanced at 100℃, and then the temperature was increased from 100℃ to 650℃, with a rise rate of 5℃ / min. The post-reaction gas was measured using a nitrogen oxide analyzer (Thermo Scientific, 42i) and an online gas chromatograph (GC-2014C, Shimadzu, Japan) equipped with a Porapak-Q column and a flame ionization detector (FID) for NO and CH4, respectively. Finally, the intermediate products of the CH4-SCR reaction were studied by in situ DRIFTS. The catalyst performance evaluation index is NO x And CH4 conversion (%) and CH4 selectivity (%).
[0052] The ICP-OES analysis results of Example 1 and Comparative Examples 1 to 3 are shown in Table 1. It can be seen that after the Ce source is introduced by adding a Ce precursor, the Ce contents of IB@Ce-1, IB@Ce-2 and IB@Ce-3 increase by 0.251, 0.264 and 7.48 wt.%, respectively. Meanwhile, the sample IBCe prepared by the wet impregnation method shows a Ce content similar to that of IB@Ce-3 (7.70 wt.%), which indicates that the Ce content of IB@Ce-3 may be excessive. In addition, the In content of IBCe is the highest at 14.51 wt.%, followed by IB@Ce-2 at 11.8 wt.%.
[0053] Table 1 Elemental analysis of the synthesized catalyst (wt.%)
[0054]
[0055] XRD spectrum Figure 2As shown in a), it can be seen that the diffraction peak intensity of the modified catalysts IB@Ce-1, IB@Ce-2, and IB@Ce-3 at 7.8° and 22.5° decreases with the increase of CeO2 content. In addition, new peaks appear at 28.9, 47.7, 56.6, and 77.9° for IB@Ce-3 and IBCe, which are related to the 111, 220, 311, and 311 CeO2 crystal planes, indicating that crystalline CeO2 exists on the outer surface of these catalysts. In contrast, in IB@Ce-1 and IB@Ce-2 samples, this peak is weaker, indicating that the dispersion of CeO2 in the samples is high, or the amorphous CeO2 on the core surface is more uniformly distributed. Comparison with the In / H-Beta diffraction peak shows that CeO2 changes the strength of H-Beta zeolite but does not affect its crystal form.
[0056] The porosity and specific surface area of the catalyst are shown in Figure 2 b) and Table 2. It can be seen that all catalysts show type-II isotherms, indicating that they are mesoporous materials. In addition, the CeO2 protective layer reduces the specific surface area of In / H-Beta, and the specific surface areas of IB@Ce-1, IB@Ce-2, and IB@Ce-3 increase from 528 m2 of IB to 1.5 m2 of IB, respectively. 2 / g dropped to 463m 2 / g, 440m 2 / g and 388m 2 / g, indicating that coating In / H-Beta with CeO2 may cover part of the pores and prevent nitrogen from entering all adsorption sites of IB. It is worth noting that IB@Ce-2 has the highest pore volume and pore size, which are 0.342 cm 3 / g and 3.30nm.
[0057] like Figure 2 As shown in Figure b), IB@Ce-1 and IB@Ce-2 prepared by the self-assembly method in the example and the sample IBCe prepared by the wet impregnation method in the comparative example 3 have similar pore distributions, indicating that the introduction of CeO2 does not interfere with the structure of In / H-Beta. However, IB@Ce-3 with a high CeO2 coating shows a different pattern, and ICP-OES and XRD analysis confirm the high CeO2 loading of IB@Ce-3, which affects its structural properties.
[0058] Table 2 Adsorption-desorption results of nitrogen on various catalysts
[0059] IB IB@Ce-1 IB@Ce-2 IB@Ce-3 IBC <![CDATA[SA(m 2 / g)]]> 528 463 440 388 447 <![CDATA[PV(cm 3 / g)]]> 0.333 0.287 0.342 0.256 0.307 PS(nm) 3.10 3.06 3.30 3.02 3.07
[0060] Note: SA is the BET surface area, PV is the pore volume after BJH desorption, and PS is the average pore size of desorption.
[0061] Scanning electron microscope images Figure 3 As shown in the figure, the shapes of the samples are slightly different, and the average particle size is between 125 and 420 nm. In addition, EDX mapping shows that the In and Ce elements are evenly distributed and slightly aggregated on the surface of IB@Ce-1, IB@Ce-2, IB@Ce-3 and IBCe. Further careful observation using high-angle annular dark field scanning transmission electron microscopy (STEM-HAADF) revealed that the core-shell structure of IB@Ce-2 has an average diameter of 33.2 nm, as shown in the figure. Figure 4 a)-4c). At the same time, Figure 4 d)-4f), the samples prepared by wet impregnation method do not show core-shell structure. In addition, IB@Ce-1 and IB@Ce-2 are amorphous surface phases with very poor crystallinity, while IB@Ce-3 and IBCe are crystalline with lattice spacings of 0.36 and 0.32 nm, respectively. Figure 5 As shown, it is consistent with the XRD results.
[0062] The surface elemental composition and elemental state of the catalysts were tested by X-ray photoelectron spectroscopy (XPS). For the series of samples, 5 (IB@Ce-2) to 8 (IB@Ce-3) Ce 3d peaks were observed, such as Figure 6 a). The peaks of 886.5eV and 905.3eV of IB@Ce-1, 886.5eV and 904.9eV of IB@Ce-2, 885.5eV and 903.8eV of IB@Ce-3, and 886.5eV and 904.8eV of IBCe are attributed to Ce. 3+ The remaining 9005eV~917.2eV and 882.4eV~898.6eV belong to Ce respectively. 4+ 3d 3 / 2 and 3D 5 / 2 , indicating that Ce 3+ and Ce 4+ In addition, as shown in Table 3, the surface Ce content of the samples prepared by the self-assembly method increases with the increase of Ce precursor. In addition, although the Ce content of IBCe is as high as 7.7% (as shown in Table 2), its surface content (0.23%) is lower than that of the sample IB@Ce-2 (0.475%) synthesized using the same Ce precursor, which also verifies the core-shell nature of the samples prepared by the self-assembly method, as confirmed by the STEM-HAADF images. Among them, the Ce content of IB@Ce-2 is 3+ The highest content is 56%; high Ce 3+ The content is beneficial to improve the mobility of oxygen in cerium oxide. 3+ and Ce 4+ Coexistence can enhance the adsorption of active reactants or intermediates, thereby improving the catalytic activity.
[0063] In 3d 5 / 2 The deconvolution of the signal is Figure 6 b), and the data are shown in Table 3. IB, IB@Ce-1 and IB@Ce-2 show three peaks at 444.7 eV, 445.4 eV and 446.1 eV, corresponding to In2O3, InO + and In(OH) 3-z z+ In contrast, the IB@Ce-3 and IBCe samples only have two peaks at 444.8 eV and 445.5 eV, belonging to In2O3 and InO + As shown in Table 3, InO + is the main form of In, with relative contents of 39.6%, 40.8% and 37.9% respectively, while the main form in IB@Ce-3 (76.9%) and IBCe (78.6%) samples is In2O3, with relative contents of 76.9% and 78.6% respectively. Since the concentration of In solution used in the synthesis of each sample is the same, the main form of In in IB@Ce-3 and IBCe is In2O3, which may be due to the high Ce content, which means that the shell thickness may affect the In species form. It should be pointed out that InO + The presence of species is beneficial to CH4-SCR, InO + It is beneficial to the activation of CH4 and the conversion of NO into nitrate.
[0064] also, Figure 6 c) shows the three oxygen species of all samples, corresponding to the lattice oxygen (O α ), 532.1eV-532.6eV surface oxygen (O β ) and 532.8eV-533.1eV hydroxyl oxygen (O γ ). Sample IB@Ce-3 has an additional peak at 529.6 eV, which is caused by lattice oxygen. In addition, as shown in Table 3, adding different amounts of Ce to the In / H-Beta catalyst increases the lattice (O α ) and surface oxygen (O β ) content, while reducing the oxygen (O γ In addition to the high lattice oxygen content of IB@Ce-3, the surface oxygen (O 2- ,O2 - ,O -) content is high. It is worth mentioning that IB@Ce-2 has the highest surface oxygen content (43.1%), which is 6.3% higher than IB. Studies have shown that lattice oxygen participates in selective oxidation reactions, while surface oxygen preferentially participates in complete oxidation reactions. Therefore, a higher surface oxygen ion density is beneficial to the oxidation of CH4 due to its higher reaction mobility and promotes NO by changing the reaction energy. x of restoration.
[0065] Table 3 Surface composition (%) of different samples.
[0066]
[0067] In addition, the acidity of the catalyst was determined by NH3-TPD. Figure 6 d). It can be seen that the peak around 101°C is physically adsorbed NH3, and the peaks around 158°C and 300°C are NH3 chemically adsorbed on weak acid and strong acid sites, respectively. The total acidity of IB, IBCe, IB@Ce-2, IB@Ce-1, and IB@Ce-3 were calculated in sequence through the NH3 desorption peak, which were 2.14mmol / g, 1.80mmol / g, 1.7mmol / g, 1.63mmol / g, and 1.51mmol / g, respectively. Pyridine infrared (Py-IR) was used to quantitatively analyze the Bronsted acid and Lewis acid to further understand the type and strength of the acid site. The results of IB, IB@Ce-2, and IBCe are shown in Figure 2. Figure 6 e) as shown. 1545cm -1 and 1450cm -1 The peaks near 1490 cm-1 belong to the Brønsted and Lewis acid sites, respectively. -1 The peaks nearby are the vibrations generated by the interaction between pyridine and the Brønsted or Lewis acid sites. After Ce is loaded on IB, the peak at 1598 cm -1 A new peak appeared at 350 °C, which may be due to the interaction between Ce and the Brønsted acid sites. As shown in Table 4, at 350 °C, the ratio of Brønsted and Lewis acid sites of IB@Ce-2 and IBCe decreased from 0.56 to 0.25 and 0.51, respectively, compared with IB. Reducing the surface acidity helps to balance the acidity and redox properties and improve the catalytic activity. Compared with the XPS results in Table 3, IBCe has high acid sites, which further confirms that Ce 4+ It is the main Ce species.
[0068] Table 4 Peak position (℃) and surface acid content (mol / g)
[0069]
[0070] Note: BS, Brønsted acid site; LS, Lewis acid site.
[0071] The redox properties of the synthesized catalysts were investigated by H2-TPR experiments. Figure 6 f). InO + It is easier to reduce than In2O3, which is usually reduced to In(0) at about 600°C. Therefore, for IB, the peak centered at 330°C is similar to that of InO + The reduction of InO + is adsorbed on the proton zeolite sites, while the peak at 487 °C belongs to InO + The CeO2-loaded samples IB@Ce-1, IB@Ce-2, IB@Ce-3 and IBCe showed new broad peaks at 510℃, 600℃, 563℃ and 590℃, respectively, which may be related to the reduction of oxygen species on the CeO2 surface. It is worth noting that after adding CeO2, InO + The peaks of CeO2 shift to lower temperatures, namely IB@Ce-2 (324°C), IB@Ce-3 (262°C) and IBCe (244°C), indicating that the presence of CeO2 affects the + The reduction of IB is beneficial to the catalytic activity. In addition, the H2 consumption of IB catalyst (0.94mmol / g) is also much higher than that of CeO2-loaded catalysts. The H2 consumption of IB@Ce-1, IB@Ce-2, IB@Ce-3 and IBCe catalysts are 0.56mmol / g, 0.37mmol / g, 0.36mmol / g and 0.74mmol / g, respectively, indicating that the protective effect of CeO2 inhibits the redox characteristics of IB.
[0072] The following experiments were conducted on the catalytic performance of the embodiments and comparative examples.
[0073] In the presence of water vapor and SO2, the performance of the synthesized catalyst for the selective catalytic reduction of NO with CH4 was evaluated using a temperature-programmed surface reaction (TPSR). Figure 7 a) As shown in Figure 2, as the temperature increases, NO x The conversion rate increases significantly, reaching a maximum before starting to decrease. x The decrease in conversion rate may be due to the oxidation reaction of CH4 with O2 at high temperature, which inhibits the reduction of NO by CH4. Figure 7 As shown in b), the conversion rate of CH4 increases exponentially from 550℃ to 650℃. In addition, the selectivity of CH4 for SCR reaction is shown in Figure 7 As shown in Figure 3c), it can be seen that at 550°C, the maximum CH4 is effectively used as a reducing agent for NO instead of being directly oxidized to CO2 by O2.
[0074] Figure 7 The results show that IB has poor catalytic activity under sulfur-containing and water-containing conditions, and the highest NOx conversion rate is only 35% at 625°C. After coating with CeO2, the NO conversion rate is significantly improved. In the entire temperature range, the NOx conversion rate of the IB@Ce-2 core-shell catalyst is the highest, reaching 57.7% at 625°C, which is 23% higher than that of the IB catalyst. IB@Ce-2 is better than IBCe prepared by the traditional method (Comparative Example 3). The NOx conversion rate of IBCe at 625°C is 48.7%, and IB@Ce-1 is also better than IBCe. . It is worth noting that with the increase of CeO2 loading, the catalyst performance first increases and then decreases. IB@Ce-2 of Example 1, IB@Ce-1 of Example 1, and IB@Ce-3 of Comparative Example 1 embody catalysts with shells of different thicknesses. It can be seen that IB@Ce-1 and IB@Ce-2 obtained with Ce(NO3)3 / H-Beta of 0.2 and 0.4 have better catalytic denitrification activity. However, further increase will lead to a sharp decline in catalyst performance, such as IB@Ce-3, which has the worst catalytic activity for NO among all catalysts including IBCe. Combined with the analysis in Table 2, it can be seen that this may be caused by pore blockage and structural shrinkage.
[0075] pass Figure 2 a) XRD and Figure 5 b) HRTEM results confirm that the excellent performance of IB@Ce-2 in H2O and SO2 environments may be attributed to the amorphous nature of the CeO2 shell. A lower amorphous CeO2 content in the catalyst can enhance its tolerance to SO2 and H2O poisons. In addition, Figure 6 f) H2-TPR spectrum shows that after CeO2 is doped, InO + The reduction temperature decreases, indicating that the presence of amorphous CeO2 can stabilize InO + At the same time, the loading of CeO2 leads to the decrease of surface acidity and redox performance, which indicates that there may be an appropriate balance between acidity and redox performance, which helps to enhance the catalytic activity of IB@Ce-2 for NO reduction. In addition, combined with Table 3, the Ce on the surface of IB@Ce-2 3+ / Ce total The exposure was the highest, promoting the increase of surface oxygen species. Figure 8 The in-situ drift spectra of IB and IB@Ce-2 in the presence of SO2 and H2O. Figure 8 a) and Figure 8 d) as shown, 3016cm -1 and 1329cm -1The peaks near the surface are related to the carbon-hydrogen bond stretching vibration signals of CH4. The surface oxygen reacts with CH4 and NO to form formate (HCOO-) and nitrate (NO 3- ). Figure 8 c) and Figure 8 f) as shown in 1554cm -1 The peak at 1661 cm -1 、1602cm -1 and 1209cm -1 The peak at 2353 cm-1 can be assigned to nitrate. The nitrate peak intensity of IB@Ce-2 is lower than that of IB, which may be due to the reduction of In active sites by the CeO2 shell. -1 The peak near (temperature above 400°C) may be the signal of the reaction product CO2. Figure 8 c) shown, 1382cm -1 、1354cm -1 and 1189cm -1 The peak at 0.040 Å confirms that the adsorption of SO2 on IB leads to the generation of sulfate species on the surface, which means that IB is susceptible to SO2 poisoning. Figure 8 f), no sulfate species peak was detected in IB@Ce-2. Therefore, it can be shown that the CeO2 shell plays an important role in limiting the formation of sulfate species on the surface of IB@Ce-2, thus promoting the high catalytic performance of the catalyst in H2O and SO2. Based on the above analysis, it can be concluded that the amorphous nature of the CeO2 shell, the high Ce 3+ / Ce total content, surface oxygen species ratio (O β / O total ), suitable acidity and redox properties are the key factors for the core-shell structure IB@Ce-2 catalyst to have high CH4-SCR reaction performance in H2O and SO2 environments.
[0076] Comparative Example 3
[0077] On the basis of Example 1, in this comparative example, the same idea was adopted to obtain In / H-Beta@La2O3, In / H-Beta@Co3O4, and In / H-Beta@MnO2 by self-assembly method.
[0078] Specifically, 0.1 g H-Beta powder was ultrasonically dispersed in 100 ml water / ethanol (1:1) mixed solution, and 0.75 g PVP, 0.06 g La(NO3)3, 0.03 g HMTA, and 0.1 g CTAB were added successively under stirring conditions. The mixture was refluxed and stirred at 60°C for 2 h. After completion, it was centrifuged and washed with deionized water. After drying at 100°C, it was calcined at 500°C for 3 h. The collected sample was named H-Beta@La2O3. The sample was added to 0.033 M In(NO3)3 solution and stirred at 80°C for 8 h. The product was obtained by filtration, washing, drying, and calcination at 500°C for 3 h, and was recorded as In / H-Beta@La2O3.
[0079] Similarly, Ce(NO3)3 in Example 1 is replaced by Co(NO3)2, and the rest is the same as Example 1, to obtain In / H-Beta@Co3O4. Ce(NO3)3 in Example 1 is replaced by Mn(NO3)2, and the rest is the same as Example 1, to obtain In / H-Beta@MnO2.
[0080] The catalyst of Example 1 and the catalyst of Comparative Example 3 were evaluated for CH4-SCR activity. The reaction conditions were: initial concentrations of NO and CH4 were both 400 ppm, O2 content was 10%, SO2 concentration was 100 ppm, water vapor content was 5 vol%, and the space velocity was 23600 h -1 , 100℃ ventilation balance for 40min, then heated to 650℃ at a heating rate of 5℃ / min, the catalyst NO x Conversion rate Fig. 9 As shown, it can be seen that the activity is better when CeO2 and MnO2 are used for coating, among which In / H-Beta@CeO2 has the best activity, with a denitrification activity of up to 57.7% at 625°C, and the active temperature window is the widest.
[0081] Comparative Example 4
[0082] Based on Example 1, in this comparative example, under the condition of keeping other variables the same, In / H-Beta@CeO2 was synthesized with 5 different PVP / H-Beta mass ratios, and the denitrification activity results of the obtained catalysts are as follows: Fig.10 It can be seen that the PVP content in the synthesis process has a great influence on the denitrification activity of the material. Insufficient or excessive PVP content will reduce the denitrification activity. When the PVP / H-Beta mass ratio is 5, the denitrification activity of the synthesized catalyst is significantly better than that of other catalysts.
[0083] Comparative Example 5
[0084] Based on Example 1, in this comparative example, under the condition of keeping other variables the same, In / H-Beta@CeO2 was synthesized with 5 different HMTA / H-Beta mass ratios, and the denitrification activity results of the obtained catalysts are as follows: Fig.11 As shown in the figure, it can be seen that the HMTA content in the synthesis process has a great influence on the denitrification activity of the material. When the HMTA / H-Beta mass ratio is 0.15-0.45, the denitrification activity is better. At 650℃, NO x The conversion rate can reach more than 50%. According to this result, it can be seen that excessive HMTA will affect the denitrification activity of the material. The reason may be that excessive HMTA causes the change of CeO2 growth direction, and no CeO2 coating layer is formed on the periphery of H-Beta.
[0085] Example 3
[0086] Based on Example 1, this example also includes: mixing the obtained In / H-Beta@CeO2 and ZrO2-Co3O4 by mechanical mixing, wherein the mass ratio of In / H-Beta@CeO2 to ZrO2-Co3O4 is 4:1, to obtain a mixed catalyst.
[0087] Comparative Example 6
[0088] On the basis of Example 3, in this comparative example, the mass ratio of In / H-Beta@CeO2 to ZrO2-Co3O4 is 1:1, and a mixed catalyst is obtained.
[0089] Under the premise of keeping the catalyst loading amount of a single experiment at 0.1 g, the denitrification activity and methane activation performance of the mixed catalysts of In / H-Beta@CeO2, ZrO2-Co3O4 of Example 1, Example 3 and Comparative Example 6 were evaluated. The results are as follows Fig.12 and Fig.13 It can be seen that when In / H-Beta@CeO2:ZrO2-Co3O4 is mechanically mixed in a mass ratio of 4:1, its active temperature window is significantly widened, and its NO x The conversion rate increased from 22.1% to 41.4%, but the amount of In / H-Beta@CeO2 decreased due to the doping of ZrO2-Co3O4, which made the NO xThe conversion rate decreased. When In / H-Beta@CeO2:ZrO2-Co3O4 were mechanically mixed in a mass ratio of 1:1, the temperature window was also widened. In summary, the doping of an appropriate amount of ZrO2-Co3O4 can promote the activation of CH4 in the process of In / H-Beta@CeO2 catalytic denitrification, broaden the active temperature window of the reaction and move it toward the low temperature direction. The greater the amount of ZrO2-Co3O4 doping, the more obvious the improvement in CH4 conversion rate. However, the doping of ZrO2-Co3O4 will lead to a decrease in the amount of In / H-Beta@CeO2, which will cause the highest NO x The conversion rate decreases, and the greater the doping amount, the more significant the decrease.
[0090] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the scope of protection of the present invention.
Claims
1. A method for preparing an In / H-Beta@CeO2 catalyst for CH4-SCR denitration, characterized in that: The steps include: Step S1, ultrasonically dispersing H-Beta powder in a solvent, adding a surface stabilizer, a Ce source, a structure directing agent hexamethylenetetramine HMTA, and a pore-forming agent cetyltrimethylammonium bromide CTAB in sequence during stirring, and then refluxing and stirring at 55-65° C. for 1.5-2.5 h, and then centrifuging and washing, drying, and calcining at 450-550° C. for 2-5 h to obtain H-Beta@CeO2; Step S2, adding the obtained H-Beta@CeO2 to the In source solution, stirring at a constant temperature of 75-85°C for 6-12 h, filtering, washing, drying, and calcining at 450-550°C for 2-5 h to obtain the product In / H-Beta@CeO2; In step S1, the surface stabilizer is polyvinyl pyrrolidone, and the mass ratio of PVP to H-Beta is 2.5-7.5; the mass ratio of HMTA to H-Beta is 0.15-0.45; the Ce source is Ce(NO3)3, and the mass ratio of Ce(NO3)3 to H-Beta is 0.2-0.
4.
2. The method for preparing the In / H-Beta@CeO2 catalyst for CH4-SCR denitration according to claim 1, characterized in that: In step S1, the solvent is an ethanol aqueous solution; in step S1 and step S2, calcination is performed under a nitrogen atmosphere.
3. The method for preparing the In / H-Beta@CeO2 catalyst for CH4-SCR denitration according to claim 1, characterized in that: The mass ratio of the polyvinyl pyrrolidone to H-Beta is 2.5-5.
4. The method for preparing the In / H-Beta@CeO2 catalyst for CH4-SCR denitration according to claim 1, characterized in that: The method further includes step S3 of mixing ZrO2-Co3O4 with In / H-Beta@CeO2.
5. The method for preparing the In / H-Beta@CeO2 catalyst for CH4-SCR denitration according to claim 4, characterized in that: The mass ratio of ZrO2-Co3O4 to In / H-Beta@CeO2 is 1-4:
1.
6. A catalyst, characterized in that: The method is prepared according to any one of claims 1 to 5.
7. Use of the catalyst as claimed in claim 6, characterized in that: The catalyst is used in CH4-SCR for denitration treatment.
Citation Information
Patent Citations
CeO2@MnOx low-temperature SCR flue gas denitrification catalyst as well as preparation method thereof and application thereof
CN106732536A
Core-shell catalyst for denitration of FCC regeneration flue gas and preparation method of core-shell catalyst
CN107029782A
Cited By
In-coated H-Beta / Fe3O4 catalyst, preparation method thereof and application of In-coated H-Beta / Fe3O4 catalyst in methane selective catalytic reduction of nitric oxide
CN121775902A