A high permeability mulberry silk membrane cloth and preparation method thereof

By combining facial mask base paper, mulberry silk, polyacrylonitrile nanofiber membrane and composite materials in the mask, a composite layer structure is formed, which solves the problem of insufficient penetration and moisturizing effect of existing facial masks, and achieves the effect of significantly increasing the skin's moisture content. .

CN116080177BActive Publication Date: 2024-10-11CHANGSHU LIANGHENG NON WOVEN PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310102048.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-13
Publication Date
2024-10-11
Estimated Expiration
2043-02-13

AI Technical Summary

Technical Problem

Existing facial masks have insufficient penetrating and moisturizing effects and cannot effectively increase the moisture content of the skin.

Method used

Using a preparation method of high-permeability mulberry silk membrane cloth, the facial mask base paper, mulberry silk, polyacrylonitrile nanofiber membrane, composite polyethyleneimine modified graphene oxide composite material, activated carbon, hydrophilic gel and frozen fermentation modification Plant fibers are combined in specific proportions and formed into a composite layer structure through the mask lamination process to enhance the mask's permeability.

Benefits of technology

The penetration effect of the facial mask is significantly improved. The moisture content of the facial skin can reach 42.5% 2 hours after use, which greatly improves the moisturizing effect of the facial mask liquid.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention discloses a high permeability mulberry silk membrane cloth and a preparation method thereof, belonging to the technical field of facial mask cloth, comprising the following raw materials in parts by weight: 55.1-78.2 parts of facial mask base paper, 12.8-21.5 parts of mulberry silk, 7.2-13.6 parts of polyacrylonitrile nanofiber membrane, 0.7-1.7 parts of composite polyethyleneimine modified graphene oxide composite material, 1.2-1.4 parts of activated carbon, 5.3-9.2 parts of hydrophilic gel, and 7.8-12.3 parts of frozen fermentation modified plant fiber. Through the above method, the present invention forms a composite layer of facial mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk by compounding, which can effectively improve the permeability effect of facial mask cloth and enhance the moisturizing effect of facial mask liquid.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of facial mask cloths, and in particular to a high-permeability mulberry silk membrane cloth and a preparation method thereof. Background Art

[0002] As a facial care product, facial masks are popular among consumers due to their advantages such as light weight, small size, easy to carry and convenient to use.

[0003] However, existing facial masks generally have a single-layer or double-layer mask base paper structure, and the penetration and moisturizing effect of the facial mask on the skin still needs to be further improved.

[0004] Based on this, the present invention designs a high-permeability mulberry silk membrane cloth and a preparation method thereof to solve the above problems. Summary of the invention

[0005] In view of the above-mentioned shortcomings of the prior art, the present invention provides a high-permeability mulberry silk membrane cloth and a preparation method thereof.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0007] A high-permeability mulberry silk membrane cloth comprises the following raw materials in parts by weight: 55.1-78.2 parts of mask base paper, 12.8-21.5 parts of mulberry silk, 7.2-13.6 parts of polyacrylonitrile nanofiber membrane, 0.7-1.7 parts of composite polyethyleneimine modified graphene oxide composite material, 1.2-1.4 parts of activated carbon, 5.3-9.2 parts of hydrophilic gel, and 7.8-12.3 parts of frozen fermentation modified plant fiber.

[0008] Furthermore, the mass ratio of the polyacrylonitrile nanofiber membrane to the composite polyethyleneimine modified graphene oxide composite material is 8 to 11:1.

[0009] Furthermore, the frozen fermented modified plant fiber is prepared in the following steps:

[0010] A. centrifugally dispersing the plant fiber, microfibrillated cellulose pulp and sodium hyaluronate by a centrifuge;

[0011] B. then freezing the mixture;

[0012] C. After freezing, the obtained material is ground into particles;

[0013] D. mixing the obtained particles with yeast powder, fermenting them, and mixing them evenly after fermentation to obtain frozen fermented modified plant fiber;

[0014] Furthermore, in step B, the mixture is then frozen and stored at -78 to -80°C for 2 to 8 hours.

[0015] Furthermore, in step C, after freezing treatment, the obtained material is ground into particles with a particle size less than 0.25 mm.

[0016] Furthermore, in step D, the obtained particles are mixed with yeast powder in a weight ratio of 1:0.03-0.05, fermented at 30-33° C. for 10-12 hours, and mixed evenly after fermentation to obtain frozen fermented modified plant fiber.

[0017] The present invention also provides a method for preparing the high-permeability silk membrane cloth, comprising the following steps:

[0018] Step 1: dissolving the hydrophilic gel in water, and placing the mask base paper in the hydrophilic gel solution for soaking; then drying the mask base paper, and the remaining hydrophilic gel solution is used for later use;

[0019] Step 2: mixing the remaining hydrophilic gel solution, activated carbon and frozen fermented modified plant fiber, and then grinding them into a granular solution with a particle size of less than 0.3 mm;

[0020] Step 3: coating the particle solution between the composite polyethyleneimine modified graphene oxide composite material layer and the polyacrylonitrile nanofiber membrane layer, and forming a composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer through a mask lamination process;

[0021] Step 4: attaching a mask base paper and a mulberry silk layer to both sides of the composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer, respectively, and forming a mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer through a mask lamination process;

[0022] Step 5: Dry the mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer at 80-88° C. for 1-2 hours to obtain a high-permeability mulberry silk membrane cloth.

[0023] Furthermore, in step one, the hydrophilic gel and water are mixed in a weight ratio of 1:0.5 to 1, and the mask base paper is placed in the hydrophilic gel solution and immersed for 10 to 20 minutes.

[0024] The present invention also provides a high-permeability mulberry silk membrane cloth prepared by the preparation method of the high-permeability mulberry silk membrane cloth.

[0025] Beneficial Effects

[0026] The present invention forms a composite layer of mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk by compounding, which can effectively improve the penetration effect of the mask cloth and enhance the moisturizing effect of the mask liquid.

[0027] The high permeability silk membrane cloth of this embodiment was loaded with a commercially available common facial mask liquid, and applied in the usual way for 15 minutes, then the mask was removed and the face was washed. The moisture content of the facial skin 2 hours after applying the mask was measured using a skin moisture tester (Corneometer CM825) and found to be 42.5%. (Test standard QB / T4256-2011). DETAILED DESCRIPTION

[0028] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The present invention will be further described below in conjunction with the embodiments.

[0030] Example 1

[0031] This embodiment provides a method for preparing a high-permeability silk membrane cloth, comprising the following steps:

[0032] Step 1: Prepare the following raw materials: 55.1kg of facial mask base paper, 21.5kg of mulberry silk, 7.2kg of polyacrylonitrile nanofiber membrane, 1.7kg of composite polyethyleneimine modified graphene oxide composite material, 1.2kg of activated carbon, 9.2kg of hydrophilic gel, and 7.8kg of frozen fermented modified plant fiber;

[0033] Wherein, the frozen fermented modified plant fiber is prepared in the following steps:

[0034] A. 40 kg of plant fiber, 20 kg of microfibrillated cellulose pulp and 5 kg of sodium hyaluronate are centrifugally dispersed by a centrifuge;

[0035] B. Then, the mixture was frozen at -78°C for 8 hours;

[0036] C. After freezing, the obtained material is ground into particles with a particle size of less than 0.25 mm;

[0037] D. Mixing the obtained particles with yeast powder in a weight ratio of 1:0.03, fermenting at 33° C. for 10 h, and mixing evenly after fermentation to obtain frozen fermented modified plant fiber;

[0038] Preferably, the composite polyethyleneimine modified graphene oxide composite material is prepared using the Chinese invention patent publication number CN107057351B;

[0039] Step 2: Mix the hydrophilic gel and water in a weight ratio of 1:0.5, and soak the mask base paper in the hydrophilic gel solution for 20 minutes; then dry the mask base paper, and keep the remaining hydrophilic gel solution for later use;

[0040] Step 3: mixing the remaining hydrophilic gel solution, activated carbon and frozen fermented modified plant fiber, and then grinding them into a granular solution with a particle size of less than 0.3 mm;

[0041] Step 4: coating the particle solution between the composite polyethyleneimine modified graphene oxide composite material layer and the polyacrylonitrile nanofiber membrane layer, and forming a composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer through a mask lamination process;

[0042] Step 5, attaching a mask base paper and a mulberry silk layer to both sides of the composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer, respectively, and forming a mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer through a mask lamination process;

[0043] Step six: Dry the mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer at 80° C. for 2 h to obtain a high-permeability mulberry silk membrane cloth.

[0044] The high permeability silk membrane cloth of this embodiment was loaded with a commercially available common facial mask liquid, and applied for 15 minutes using the usual facial mask application method, then the mask was removed and the face was washed. The moisture content of the facial skin before applying the mask was measured using a skin moisture tester (Corneometer CM825) and was 30.7%, and the moisture content of the facial skin 2 hours after applying the mask was 41.3%. (Test standard QB / T4256-2011).

[0045] Example 2

[0046] This embodiment provides a method for preparing a high-permeability silk membrane cloth, comprising the following steps:

[0047] Step 1: Prepare the following raw materials: 78.2kg of facial mask base paper, 12.8kg of mulberry silk, 13.6kg of polyacrylonitrile nanofiber membrane, 0.7kg of composite polyethyleneimine modified graphene oxide composite material, 1.4kg of activated carbon, 5.3kg of hydrophilic gel, and 12.3kg of frozen fermented modified plant fiber;

[0048] Wherein, the frozen fermented modified plant fiber is prepared in the following steps:

[0049] A. 60 kg of plant fiber, 10 kg of microfibrillated cellulose pulp and 11 kg of sodium hyaluronate are centrifugally dispersed using a centrifuge;

[0050] B. Then, the mixture was frozen at -80°C for 2 hours;

[0051] C. After freezing, the obtained material is ground into particles with a particle size less than 0.25 mm;

[0052] D. Mixing the obtained particles with yeast powder in a weight ratio of 1:0.05, fermenting at 30° C. for 12 h, and mixing evenly after fermentation to obtain frozen fermented modified plant fiber;

[0053] Preferably, the composite polyethyleneimine modified graphene oxide composite material is prepared using the Chinese invention patent publication number CN107057351B;

[0054] Step 2: Mix the hydrophilic gel and water in a weight ratio of 1:1, and soak the mask base paper in the hydrophilic gel solution for 10 minutes; then dry the mask base paper, and keep the remaining hydrophilic gel solution for later use;

[0055] Step 3: mixing the remaining hydrophilic gel solution, activated carbon and frozen fermented modified plant fiber, and then grinding them into a granular solution with a particle size of less than 0.3 mm;

[0056] Step 4: coating the particle solution between the composite polyethyleneimine modified graphene oxide composite material layer and the polyacrylonitrile nanofiber membrane layer, and forming a composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer through a mask lamination process;

[0057] Step 5, attaching a mask base paper and a mulberry silk layer to both sides of the composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer, respectively, and forming a mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer through a mask lamination process;

[0058] Step six: Dry the mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer at 88° C. for 1 hour to obtain a high-permeability mulberry silk membrane cloth.

[0059] The high permeability silk membrane cloth of this embodiment was loaded with a commercially available common facial mask liquid, and the mask was applied for 15 minutes using the usual mask application method, then the mask was removed and the face was washed. The moisture content of the facial skin before applying the mask was measured using a skin moisture tester (Corneometer CM825) and was 32.3%, and the moisture content of the facial skin 2 hours after applying the mask was 43.6%. (Test standard QB / T4256-2011).

[0060] Example 3

[0061] This embodiment provides a method for preparing a high-permeability silk membrane cloth, comprising the following steps:

[0062] Step 1: Prepare the following raw materials: 62.3kg of facial mask base paper, 18.2kg of mulberry silk, 8kg of polyacrylonitrile nanofiber membrane, 1kg of composite polyethyleneimine modified graphene oxide composite material, 1.3kg of activated carbon, 6.3kg of hydrophilic gel, and 10.7kg of frozen fermented modified plant fiber;

[0063] Wherein, the frozen fermented modified plant fiber is prepared in the following steps:

[0064] A. 48 kg of plant fiber, 19 kg of microfibrillated cellulose pulp and 10.3 kg of sodium hyaluronate are centrifugally dispersed using a centrifuge;

[0065] B. Then, the mixture was frozen at -79°C for 5 hours;

[0066] C. After freezing, the obtained material is ground into particles with a particle size less than 0.25 mm;

[0067] D. Mixing the obtained particles with yeast powder in a weight ratio of 1:0.04, fermenting at 31° C. for 11 h, and mixing evenly after fermentation to obtain frozen fermented modified plant fiber;

[0068] Preferably, the composite polyethyleneimine modified graphene oxide composite material is prepared using the Chinese invention patent publication number CN107057351B;

[0069] Step 2: Mix the hydrophilic gel and water in a weight ratio of 1:0.7, and soak the mask base paper in the hydrophilic gel solution for 16 minutes; then dry the mask base paper, and keep the remaining hydrophilic gel solution for later use;

[0070] Step 3: mixing the remaining hydrophilic gel solution, activated carbon and frozen fermented modified plant fiber, and then grinding them into a granular solution with a particle size of less than 0.3 mm;

[0071] Step 4: coating the particle solution between the composite polyethyleneimine modified graphene oxide composite material layer and the polyacrylonitrile nanofiber membrane layer, and forming a composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer through a mask lamination process;

[0072] Step 5, attaching a mask base paper and a mulberry silk layer to both sides of the composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer, respectively, and forming a mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer through a mask lamination process;

[0073] Step six: Dry the mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer at 85° C. for 1.6 h to obtain a high-permeability mulberry silk membrane cloth.

[0074] The high permeability silk membrane cloth of this embodiment was loaded with a commercially available common facial mask liquid, and the mask was applied for 15 minutes using the usual mask application method, then the mask was removed and the face was washed. The moisture content of the facial skin before applying the mask was measured using a skin moisture tester (Corneometer CM825), which was 31.8%, and the moisture content of the facial skin 2 hours after applying the mask was 40.7%. (Test standard QB / T4256-2011).

[0075] Example 4

[0076] Different from Example 1, step one of this example is: prepare the following raw materials: 55.1 kg of mask base paper, 21.5 kg of mulberry silk, 11 kg of polyacrylonitrile nanofiber membrane, 1 kg of composite polyethyleneimine modified graphene oxide composite material, 1.2 kg of activated carbon, 9.2 kg of hydrophilic gel, and 7.8 kg of frozen fermented modified plant fiber.

[0077] The high permeability silk membrane cloth of this embodiment was loaded with a commercially available common facial mask liquid, and the mask was applied for 15 minutes using the usual method, then the mask was removed and the face was washed. The moisture content of the facial skin before applying the mask was measured using a skin moisture tester (Corneometer CM825), which was 31.3%, and the moisture content of the facial skin 2 hours after applying the mask was 42.5%. (Test standard QB / T4256-2011).

[0078] Comparative Example 1

[0079] This embodiment provides a method for preparing a high-permeability silk membrane cloth, comprising the following steps:

[0080] Step 1: Prepare the following raw materials: 55.1kg of facial mask base paper, 21.5kg of mulberry silk, 7.2kg of polyacrylonitrile nanofiber membrane, 1.2kg of activated carbon, 9.2kg of hydrophilic gel, and 7.8kg of frozen fermented modified plant fiber;

[0081] Wherein, the frozen fermented modified plant fiber is prepared in the following steps:

[0082] A. 40 kg of plant fiber, 20 kg of microfibrillated cellulose pulp and 5 kg of sodium hyaluronate are centrifugally dispersed by a centrifuge;

[0083] B. Then, the mixture was frozen at -78°C for 8 hours;

[0084] C. After freezing, the obtained material is ground into particles with a particle size of less than 0.25 mm;

[0085] D. Mixing the obtained particles with yeast powder in a weight ratio of 1:0.03, fermenting at 33° C. for 10 h, and mixing evenly after fermentation to obtain frozen fermented modified plant fiber;

[0086] Step 2: Mix the hydrophilic gel and water in a weight ratio of 1:0.5, and soak the mask base paper in the hydrophilic gel solution for 20 minutes; then dry the mask base paper, and keep the remaining hydrophilic gel solution for later use;

[0087] Step 3: mixing the remaining hydrophilic gel solution, activated carbon and frozen fermented modified plant fiber, and then grinding them into a granular solution with a particle size of less than 0.3 mm;

[0088] Step 4: coating the particle solution on the polyacrylonitrile nanofiber membrane layer;

[0089] Step 5: attaching a mask base paper and a mulberry silk layer to both sides of the polyacrylonitrile nanofiber membrane layer, respectively, and forming a mask base paper / polyacrylonitrile nanofiber membrane / mulberry silk composite layer through a mask lamination process;

[0090] Step six: Dry the mask base paper / polyacrylonitrile nanofiber membrane / mulberry silk composite layer at 80° C. for 2 hours to obtain the membrane cloth.

[0091] The membrane cloth of this comparative example was loaded with a commercially available common facial mask liquid, and applied in the usual way for 15 minutes, then the mask was removed and the face was washed. The moisture content of the facial skin before applying the mask was measured by a skin moisture tester (Corneometer CM825), which was 32.2%, and the moisture content of the facial skin 2 hours after applying the mask was 33.9%. (Test standard QB / T 4256-2011).

[0092] It can be seen that, compared with the comparative example, the present invention can effectively improve the penetration effect of the mask cloth and enhance the moisturizing effect of the mask liquid by compositely forming a mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer.

[0093] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A high permeability mulberry silk membrane cloth, characterized in that: The invention comprises the following raw materials in parts by weight: 55.1-78.2 parts of mask base paper, 12.8-21.5 parts of mulberry silk, 7.2-13.6 parts of polyacrylonitrile nanofiber membrane, 0.7-1.7 parts of composite polyethyleneimine modified graphene oxide composite material, 1.2-1.4 parts of activated carbon, 5.3-9.2 parts of hydrophilic gel, 7.8-12.3 parts of frozen fermentation modified plant fiber; The frozen fermented modified plant fiber is prepared in the following steps: A. centrifugally dispersing the plant fiber, microfibrillated cellulose pulp and sodium hyaluronate by a centrifuge to obtain a mixed material; B. Then, the mixture is frozen at -78~-80℃ for 2~8h; C. After freezing, the obtained material is ground into particles; D. Mix the obtained particles with yeast powder in a weight ratio of 1:0.03-0.05, ferment at 30-33°C for 10-12h, and mix evenly after fermentation to obtain frozen fermented modified plant fiber; The method for preparing the high-permeability silk membrane cloth comprises the following steps: Step 1: dissolving the hydrophilic gel in water, and placing the mask base paper in the hydrophilic gel solution for soaking; then drying the mask base paper, and the remaining hydrophilic gel solution is used for later use; Step 2: mixing the remaining hydrophilic gel solution, activated carbon and frozen fermented modified plant fiber, and then grinding them into a granular solution with a particle size of less than 0.3 mm; Step 3: coating the particle solution between the composite polyethyleneimine modified graphene oxide composite material layer and the polyacrylonitrile nanofiber membrane layer, and forming a composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer through a mask lamination process; Step 4: attaching a mask base paper and a mulberry silk layer to both sides of the composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer, respectively, and forming a mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer through a mask lamination process; Step 5: Dry the mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer at 80-88° C. for 1-2 hours to obtain a high-permeability mulberry silk membrane cloth.

2. The high permeability mulberry silk membrane cloth according to claim 1, characterized in that: The mass ratio of the polyacrylonitrile nanofiber membrane to the composite polyethyleneimine modified graphene oxide composite material is 8-11:

1.

3. The high permeability mulberry silk membrane cloth according to claim 1, characterized in that: Step C: After freezing, the obtained material is ground into particles with a particle size of less than 0.25 mm.

4. A method for preparing the high permeability mulberry silk membrane cloth according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step 1: dissolving the hydrophilic gel in water, and placing the mask base paper in the hydrophilic gel solution for soaking; then drying the mask base paper, and the remaining hydrophilic gel solution is used for later use; Step 2: mixing the remaining hydrophilic gel solution, activated carbon and frozen fermented modified plant fiber, and then grinding them into a granular solution with a particle size of less than 0.3 mm; Step 3: coating the particle solution between the composite polyethyleneimine modified graphene oxide composite material layer and the polyacrylonitrile nanofiber membrane layer, and forming a composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer through a mask lamination process; Step 4: attaching a mask base paper and a mulberry silk layer to both sides of the composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane composite layer, respectively, and forming a mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer through a mask lamination process; Step 5: Dry the mask base paper / composite polyethyleneimine modified graphene oxide composite material / polyacrylonitrile nanofiber membrane / mulberry silk composite layer at 80-88° C. for 1-2 hours to obtain a high-permeability mulberry silk membrane cloth.

5. The method for preparing the high permeability mulberry silk membrane cloth according to claim 4, characterized in that: In step 1, the hydrophilic gel and water are mixed in a weight ratio of 1:0.5-1, and the mask base paper is placed in the hydrophilic gel solution and immersed for 10-20 minutes.