Epoxy composite intercalation anticorrosive coating and preparation method thereof

By introducing kaolin intercalation composite into the epoxy resin network to form a multi-layer structure, it solves the problem of insufficient antibacterial and bactericidal properties of existing coatings in the oil and gas industry environment, and achieves high barrier and good anti-corrosion effects.

CN116082923BActive Publication Date: 2024-10-11CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111313767.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-08
Publication Date
2024-10-11
Estimated Expiration
2041-11-08

AI Technical Summary

Technical Problem

It is difficult for existing coatings to maintain stable antibacterial and bactericidal properties in the acidic, high-sulfur, and high-salt environments of the oil and gas industry, and it is difficult to adapt to the high barrier and low oxygen permeability requirements of the oil and gas development industry.

Method used

Diamine-modified low-molecular epoxy resin is used to form a high cross-linking density polymer network, and a kaolin intercalation compound is introduced into the network to improve the permeability resistance and adhesion of the coating through urea intercalation to form a multi-layer Structural kaolin intercalation structure.

Benefits of technology

It achieves good anti-corrosion properties of the coating, improves permeability resistance and adhesion, achieves high barrier properties, and is suitable for harsh environments in the oil and gas industry.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses an epoxy composite intercalation anticorrosive coating and a preparation method thereof, comprising component A and component B, wherein component A comprises kaolin intercalation-modified epoxy resin network polymer, organic solvent, film former, filler, additive; component B comprises organic solvent and curing agent; the kaolin intercalation-modified epoxy resin network polymer is obtained by intercalation reaction of kaolin intercalation compound and modified epoxy resin. The present invention also discloses a preparation method of the above coating. The present invention adopts a high cross-linking density polymer network formed by a low molecular weight epoxy resin modified by diamine, introduces a kaolin intercalation compound into the polymer network, and adopts urea intercalation kaolin to obtain the kaolin intercalation compound.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to an epoxy composite intercalation anti-corrosion coating and a preparation method thereof. Background Art

[0002] The strata in the Northwest Oilfield are highly mineralized, and the chloride ion content in the produced water can often reach more than 10,000 ppm, and the mineral content can reach 100,000 ppm, or even as high as 240,000 ppm, which puts great pressure on the anti-corrosion of oil and gas pipelines. Conventional anti-corrosion materials for oil and gas pipelines are difficult to achieve good anti-corrosion effects. At the same time, produced water containing a large amount of minerals is very easy to scale and penetrate in pipelines or processing equipment, further aggravating the corrosion of pipelines and equipment in oil and gas fields.

[0003] Patent CN102181219A discloses a water-based anti-corrosion coating of a nano-montmorillonite and polypyrrole composite and a preparation method thereof, and relates to a coating. The raw material composition is montmorillonite 1-50, solvent 20-300, protonic acid 0.8-55, organic activator 0.07-18.5, ferric chloride hexahydrate or ferric sulfate 8.5-50.6, pyrrole 0.8-56, surfactant 4.5-50, base resin 10-55, modified resin 0-10, neutralizer 0.34-5.6, pigment 0.6-10, deionized water 20-100, defoamer 0.05-1.2, anti-settling agent 0.22-1.34, dispersant 0.13-1.15, leveling agent 0.02-1.08, and film-forming aid 0.05-1.04. The nano-montmorillonite and polypyrrole composite is prepared first, including the pretreatment of montmorillonite and the synthesis of the nano-montmorillonite and polypyrrole composite, and then the coating is prepared.

[0004] Patent CN102634276A discloses a polyaniline heavy anticorrosion coating and a preparation method thereof. The prepared anticorrosion coating not only has strong anticorrosion performance, but also has antifouling and antistatic capabilities. The raw material composition of the polyaniline heavy anticorrosion coating is as follows: 8-15 of polyaniline and montmorillonite composite material, 10-15 of mica powder, 10-15 of talc powder, 15-20 of quartz powder, 30-40 of base resin, 0-5 of modified resin, 0-3 of pigment, 0.5-1.0 of defoamer, 0.5-1.0 of dispersant, 0.5-1.0 of leveling agent, 0.5-1.0 of film-forming aid, and 30-40 of solvent. First, prepare the polyaniline and montmorillonite composite material, including the pretreatment of montmorillonite, the in-situ intercalation reaction of aniline, and the synthesis of the polyaniline and montmorillonite intercalation composite material. It is best to prepare the polyaniline heavy anticorrosion coating.

[0005] Patent CN110079808A discloses a Ti 3+-LDH intercalated sodium dodecyl sulfate and 8-hydroxyquinoline composite and its application. ZnTi double-layer hydroxide intercalated with sodium dodecyl sulfate and 8-hydroxyquinoline is synthesized by back-mixing coprecipitation; wherein the molar ratio of zinc ions, titanium ions, sodium dodecyl sulfate and 8-hydroxyquinoline in the composite is 4:2:1-3:1-3. The composite of the present invention has both anticorrosion and bactericidal effects, can be anticorrosive and antifouling at the same time, and has high efficiency and long action time, can effectively inhibit the damage of fouling bacteria and environmental corrosion, and has broad application prospects.

[0006] The paper (Yin Hui. Preparation and performance study of organic intercalation modified kaolin / poly (2,3-dimethylaniline) nanocomposites [D]. Chongqing University.) used an in-situ polymerization method to prepare intercalation-exfoliation type P(2,3-DMA) / organic kaolin (POK) nanocomposites. By optimizing the conditions, the effects of oxidant dosage, phosphoric acid concentration, reaction time and reaction temperature on the anti-corrosion performance of POK were explored. The structure and stability of POK were characterized by Fourier transform infrared spectroscopy (FTIR), X-ray diffraction (XRD), scanning electron microscopy (SEM), and thermogravimetric-differential thermal analysis (TGA-DTA), respectively. The corrosion protection effect of epoxy resin coating containing POK on metals was studied in 3.5% NaCl. At the same time, P(2,3-DMA) / layered silicate (PLS) nanocomposites were prepared by emulsion system, and the corrosion protection performance of coating containing PLS on cold-rolled steel was studied.

[0007] In summary, although a variety of coatings with high barrier and low oxygen permeability have been proposed in the prior art, there has not yet been a high barrier and low oxygen permeability coating specifically for the oil and gas development industry. The disclosed high barrier and low oxygen permeability coatings are also difficult to adapt to the harsh acidic, high sulfur and high salt environment of the oil and gas industry, and it is difficult to ensure stable antibacterial and bactericidal properties. Summary of the invention

[0008] Based on this, the present invention provides an epoxy composite intercalation anti-corrosion coating and a preparation method thereof, which improves the permeability resistance and adhesion of the coating by using a diamine-modified low-molecular epoxy resin to form a high cross-linking density polymer network and introducing a kaolin intercalation composite into the polymer network, thereby achieving good anti-corrosion performance.

[0009] To achieve the above object, the present invention provides the following technical solutions:

[0010] On the one hand, the present invention provides an epoxy composite intercalation anti-corrosion coating, comprising component A and component B, wherein component A comprises kaolin intercalation-modified epoxy resin network polymer, organic solvent, film former, filler, and additive; and component B comprises organic solvent and curing agent;

[0011] The kaolin intercalation-modified epoxy resin network polymer is obtained by the intercalation reaction of kaolin intercalation compound and modified epoxy resin.

[0012] Furthermore, the modified epoxy resin is obtained by modifying a low molecular weight epoxy resin with a diamine;

[0013] The molecular weight of the low molecular weight epoxy resin is 1000-5000;

[0014] Preferably, the molecular weight of the low molecular weight epoxy resin is 2000-4000;

[0015] Furthermore, the kaolin intercalation composite is intercalated with urea.

[0016] Furthermore, the raw materials of component A include, by weight: 20-30 parts of kaolin intercalation-modified epoxy resin network polymer, 30-40 parts of organic solvent, 10-15 parts of film former, 7-10 parts of filler, and 1-5 parts of additive; the raw materials of component B include, by weight: 40-50 parts of organic solvent and 25-40 parts of curing agent.

[0017] Preferably, the raw materials of component A include, by weight: 22-28 parts of kaolin intercalation-modified epoxy resin network polymer, 32-38 parts of organic solvent, 11-14 parts of film former, 8-9 parts of filler, and 2-4 parts of additives; the raw materials of component B include, by weight: 42-48 parts of organic solvent and 28-38 parts of curing agent.

[0018] More preferably, the raw materials of component A include, by weight: 24-26 parts of kaolin intercalation-modified epoxy resin network polymer, 34-36 parts of organic solvent, 12-13 parts of film former, 8-9 parts of filler, and 3-4 parts of additives; the raw materials of component B include, by weight: 44-46 parts of organic solvent and 30-35 parts of curing agent.

[0019] Wherein, the organic solvent is selected from one or more of acetone, ethanol, isobutanol, and ethyl acetate;

[0020] The film-forming agent is selected from one or more of amino resin, organic silicon resin, organic fluorine resin, ethyl silicate, sodium silicate and acrylic resin;

[0021] The filler is a mixture of nano titanium dioxide, nano zirconium dioxide and pigment; the nano titanium dioxide is 1-5 parts, the nano zirconium dioxide is 2-7 parts, and the pigment is 1-5 parts.

[0022] On the other hand, the present invention also discloses a method for preparing an epoxy composite intercalation anti-corrosion coating, which specifically comprises the following steps:

[0023] S1, preparing modified epoxy resin;

[0024] S2, preparing kaolin intercalation composite;

[0025] S3, prepare component A and component B respectively;

[0026] S4. Add component B to component A, and stir and disperse them evenly to obtain the coating for use.

[0027] Furthermore, the preparation of the modified epoxy resin comprises the following steps:

[0028] S11, preparing a low molecular weight epoxy resin: adding bisphenol A and epichlorohydrin into an organic solvent, stirring and dissolving, and then heating to 50-75° C., and then adding a 10% by mass sodium hydroxide solution to react to obtain a low molecular weight epoxy resin;

[0029] S12, preparing modified epoxy resin: adding diamine to the low molecular weight epoxy resin prepared in step S11, stirring and heating to 80-90° C., and continuing stirring and reacting for 2-8 hours to obtain modified epoxy resin;

[0030] The preparation method of the kaolin intercalation composite is as follows: adding dry kaolin into an aqueous solution of urea, stirring and reacting at room temperature for 10-24 hours, and then washing with 50-60° C. ethanol to obtain the kaolin intercalation composite.

[0031] The molar ratio of bisphenol A to epichlorohydrin is 1:3-9; the molar ratio of sodium hydroxide solution to bisphenol A is 0.5-1:1; the molar ratio of epoxy resin to diamine is 1:0.8-2; and the molar ratio of kaolin to urea is 0.1-0.3:1.

[0032] Compared with the prior art, the present invention has the following beneficial effects:

[0033] (1) The present invention discloses an epoxy composite intercalation anti-corrosion coating, which uses a diamine-modified low-molecular epoxy resin to form a high cross-linking density polymer network, and introduces a kaolin intercalation composite into the polymer network to improve the coating's permeability resistance and adhesion, thereby achieving good anti-corrosion performance;

[0034] (2) The present invention discloses an epoxy composite intercalation anti-corrosion coating, which uses urea intercalated kaolin, which has a small molecular weight and a high intercalation degree, and can obtain a multi-layer kaolin intercalation structure, which is beneficial to improving the barrier properties of the coating;

[0035] (3) The preparation method of the epoxy composite intercalation anti-corrosion coating disclosed in the present invention is simple, and the prepared anti-corrosion coating has good corrosion resistance, low oxygen permeability, and good barrier properties. DETAILED DESCRIPTION

[0036] Basic Example An epoxy composite intercalation anticorrosive coating

[0037] The invention comprises component A and component B. The raw materials of component A comprise, by weight, 20-30 parts of kaolin intercalation-modified epoxy resin network polymer, 30-40 parts of organic solvent, 10-15 parts of film former, 7-10 parts of filler and 1-5 parts of additive; the raw materials of component B comprise, by weight, 40-50 parts of organic solvent and 25-40 parts of curing agent.

[0038] The kaolin intercalation-modified epoxy resin network polymer is obtained by the intercalation reaction of kaolin intercalation compound and modified epoxy resin.

[0039] The modified epoxy resin is obtained by modifying a low molecular weight epoxy resin with a diamine;

[0040] The molecular weight of the low molecular weight epoxy resin is 1000-5000;

[0041] Preferably, the molecular weight of the low molecular weight epoxy resin is 2000-4000;

[0042] The kaolin intercalation composite is intercalated by urea.

[0043] Preferably, the raw materials of component A include, by weight: 22-28 parts of kaolin intercalation-modified epoxy resin network polymer, 32-38 parts of organic solvent, 11-14 parts of film former, 8-9 parts of filler, and 2-4 parts of additives; the raw materials of component B include, by weight: 42-48 parts of organic solvent and 28-38 parts of curing agent.

[0044] More preferably, the raw materials of component A include, by weight: 24-26 parts of kaolin intercalation-modified epoxy resin network polymer, 34-36 parts of organic solvent, 12-13 parts of film former, 8-9 parts of filler, and 3-4 parts of additives; the raw materials of component B include, by weight: 44-46 parts of organic solvent and 30-35 parts of curing agent.

[0045] Wherein, the organic solvent is selected from one or more of acetone, ethanol, isobutanol, and ethyl acetate;

[0046] The film-forming agent is selected from one or more of amino resin, organic silicon resin, organic fluorine resin, ethyl silicate, sodium silicate and acrylic resin;

[0047] The filler is a mixture of nano titanium dioxide, nano zirconium dioxide and pigment; the nano titanium dioxide is 1-5 parts, the nano zirconium dioxide is 2-7 parts, and the pigment is 1-5 parts.

[0048] On the other hand, the present invention also discloses a method for preparing an epoxy composite intercalation anti-corrosion coating, which specifically comprises the following steps:

[0049] S1, preparing modified epoxy resin;

[0050] S2, preparing kaolin intercalation composite;

[0051] S3, prepare component A and component B respectively;

[0052] S4. Add component B to component A, and stir and disperse them evenly to obtain the coating for use.

[0053] Furthermore, the preparation of the modified epoxy resin comprises the following steps:

[0054] S11, preparing a low molecular weight epoxy resin: adding bisphenol A and epichlorohydrin into an organic solvent, stirring and dissolving, and then heating to 50-75° C., and then adding a 10% by mass sodium hydroxide solution to react to obtain a low molecular weight epoxy resin;

[0055] S12, preparing modified epoxy resin: adding diamine to the low molecular weight epoxy resin prepared in step S11, stirring and heating to 80-90° C., and continuing stirring and reacting for 2-8 hours to obtain modified epoxy resin;

[0056] The preparation method of the kaolin intercalation composite is as follows: adding dry kaolin into an aqueous solution of urea, stirring and reacting at room temperature for 10-24 hours, and then washing with 50-60° C. ethanol to obtain the kaolin intercalation composite.

[0057] The molar ratio of bisphenol A to epichlorohydrin is 1:3-9; the molar ratio of sodium hydroxide solution to bisphenol A is 0.5-1:1; the molar ratio of epoxy resin to diamine is 1:0.8-2; and the molar ratio of kaolin to urea is 0.1-0.3:1.

[0058] Example 1 An epoxy composite intercalation anticorrosive coating

[0059] The invention comprises component A and component B. The raw materials of component A comprise, by weight, 20 parts of kaolin intercalation-modified epoxy resin network polymer, 30 parts of organic solvent, 10 parts of film former, 7 parts of filler and 1 part of additive; the raw materials of component B comprise, by weight, 40 parts of organic solvent and 25 parts of curing agent.

[0060] In component A, the filler is: 2 parts of nano titanium dioxide, 4 parts of nano zirconium dioxide, 1 part of carbon black; the solvent is acetone; the film-forming agent is ethyl silicate; the additives are: substrate wetting agent: Digo 450, 0.3 parts; defoaming agent, Merck MOK4021, 0.2 parts; thickener: sodium methylcellulose, 0.2 parts; dispersant: Digo 610s, 0.3 parts;

[0061] In component B: the solvent is acetone; the curing agent is dicyandiamide

[0062] The kaolin intercalation-modified epoxy resin network polymer is obtained by the intercalation reaction of kaolin intercalation compound and modified epoxy resin.

[0063] The modified epoxy resin is obtained by modifying a low molecular weight epoxy resin with a diamine;

[0064] The molecular weight of the low molecular weight epoxy resin is 1000-5000;

[0065] The kaolin intercalation composite is intercalated by urea.

[0066] The preparation method of the epoxy composite intercalation anti-corrosion coating comprises the following steps:

[0067] S1, preparing modified epoxy resin;

[0068] S11, preparing a low molecular weight epoxy resin: adding bisphenol A and epichlorohydrin (molar ratio of 4:1) into an organic solvent, stirring and dissolving, and then heating to 50-75° C., and then adding a 10% by mass fraction sodium hydroxide solution (molar ratio of sodium hydroxide to bisphenol A is 0.8:1) to react to obtain a low molecular weight epoxy resin;

[0069] S12, preparing modified epoxy resin: adding diamine (the molar ratio of epoxy resin to diamine is 1:1) to the low molecular weight epoxy resin prepared in step S11, stirring and heating to 80-90° C., and continuing stirring and reacting for 2-8 hours to obtain modified epoxy resin;

[0070] S2, preparing kaolin intercalation composite;

[0071] The dried kaolin is added to a 15% urea aqueous solution (molar ratio of 0.2:1), and reacted at room temperature with stirring for 10-24 hours, and then washed with 50-60° C. ethanol to obtain a kaolin intercalation composite.

[0072] S3, prepare component A and component B respectively;

[0073] S4. Add component B into component A, and stir and disperse them evenly to obtain the coating.

[0074] Example 2 An epoxy composite intercalation anticorrosive coating

[0075] The invention comprises component A and component B. The raw materials of component A comprise, by weight, 30 parts of kaolin intercalation-modified epoxy resin network polymer, 40 parts of organic solvent, 15 parts of film former, 10 parts of filler and 5 parts of additive; the raw materials of component B comprise, by weight, 50 parts of organic solvent and 40 parts of curing agent.

[0076] In component A, the filler is: 1 part of nano titanium dioxide, 7 parts of nano zirconium dioxide, 2 parts of carbon black; the solvent is acetone; the film-forming agent is ethyl silicate; the additives are: substrate wetting agent: Digo 450, 0.3 parts; defoaming agent, Merck MOK4021, 0.2 parts; thickener: sodium methyl cellulose, 0.2 parts; dispersant: Digo 610s, 0.3 parts;

[0077] In component B: the solvent is acetone; the curing agent is dicyandiamide

[0078] The kaolin intercalation-modified epoxy resin network polymer is obtained by the intercalation reaction of kaolin intercalation compound and modified epoxy resin.

[0079] The modified epoxy resin is obtained by modifying a low molecular weight epoxy resin with a diamine;

[0080] The molecular weight of the low molecular weight epoxy resin is 1000-5000;

[0081] The kaolin intercalation composite is intercalated by urea.

[0082] The preparation method of the epoxy composite intercalation anti-corrosion coating comprises the following steps:

[0083] S1, preparing modified epoxy resin;

[0084] S11, preparing a low molecular weight epoxy resin: adding bisphenol A and epichlorohydrin (molar ratio of 4:1) into an organic solvent, stirring and dissolving, and then heating to 50-75° C., and then adding a 10% by mass fraction sodium hydroxide solution (molar ratio of sodium hydroxide to bisphenol A is 0.8:1) to react to obtain a low molecular weight epoxy resin;

[0085] S12, preparing modified epoxy resin: adding diamine (the molar ratio of epoxy resin to diamine is 1:1) to the low molecular weight epoxy resin prepared in step S11, stirring and heating to 80-90° C., and continuing stirring and reacting for 2-8 hours to obtain modified epoxy resin;

[0086] S2, preparing kaolin intercalation composite;

[0087] The dried kaolin is added into a 15% urea aqueous solution (molar ratio of 0.2:1), and reacted at room temperature with stirring for 10-24 hours, and then washed with 50-60° C. ethanol to obtain a kaolin intercalation composite.

[0088] S3, prepare component A and component B respectively;

[0089] S4. Add component B into component A, and stir and disperse them evenly to obtain the coating.

[0090] Example 3: An epoxy composite intercalation anticorrosive coating

[0091] The invention comprises component A and component B. The raw materials of component A comprise, by weight, 22 parts of kaolin intercalation-modified epoxy resin network polymer, 38 parts of organic solvent, 11 parts of film former, 9 parts of filler and 4 parts of additive; the raw materials of component B comprise, by weight, 48 parts of organic solvent and 28 parts of curing agent.

[0092] In component A, the filler is: 5 parts of nano titanium dioxide, 3 parts of nano zirconium dioxide, 1 part of carbon black; the solvent is acetone; the film-forming agent is ethyl silicate; the additives are: substrate wetting agent: Digo 450, 0.3 parts; defoaming agent, Merck MOK4021, 0.2 parts; thickener: sodium methyl cellulose, 0.2 parts; dispersant: Digo 610s, 0.3 parts;

[0093] The kaolin intercalation-modified epoxy resin network polymer is obtained by the intercalation reaction of kaolin intercalation compound and modified epoxy resin.

[0094] The modified epoxy resin is obtained by modifying a low molecular weight epoxy resin with a diamine;

[0095] The molecular weight of the low molecular weight epoxy resin is 2000-4000;

[0096] The kaolin intercalation composite is intercalated by urea.

[0097] The preparation method of the epoxy composite intercalation anti-corrosion coating comprises the following steps:

[0098] S1, preparing modified epoxy resin;

[0099] S11, preparing a low molecular weight epoxy resin: adding bisphenol A and epichlorohydrin (molar ratio of 4:1) into an organic solvent, stirring and dissolving, and then heating to 50-75° C., and then adding a 10% by mass fraction sodium hydroxide solution (molar ratio of sodium hydroxide to bisphenol A is 0.8:1) to react to obtain a low molecular weight epoxy resin;

[0100] S12, preparing modified epoxy resin: adding diamine (the molar ratio of epoxy resin to diamine is 1:1) to the low molecular weight epoxy resin prepared in step S11, stirring and heating to 80-90° C., and continuing stirring and reacting for 2-8 hours to obtain modified epoxy resin;

[0101] S2, preparing kaolin intercalation composite;

[0102] The dried kaolin is added into a 15% urea aqueous solution (molar ratio of 0.2:1), and reacted at room temperature with stirring for 10-24 hours, and then washed with 50-60° C. ethanol to obtain a kaolin intercalation composite.

[0103] S3, prepare component A and component B respectively;

[0104] S4. Add component B into component A, and stir and disperse them evenly to obtain the coating.

[0105] Example 4: An epoxy composite intercalation anticorrosive coating

[0106] The invention comprises component A and component B. The raw materials of component A comprise, by weight, 24 parts of kaolin intercalation-modified epoxy resin network polymer, 36 parts of organic solvent, 12 parts of film former, 8 parts of filler and 3 parts of additive; the raw materials of component B comprise, by weight, 46 parts of organic solvent and 35 parts of curing agent.

[0107] In component A, the filler is: 2 parts of nano titanium dioxide, 4 parts of nano zirconium dioxide, 1 part of carbon black; the solvent is acetone; the film-forming agent is ethyl silicate; the additives are: substrate wetting agent: Digo 450, 0.3 parts; defoaming agent, Merck MOK4021, 0.2 parts; thickener: sodium methylcellulose, 0.2 parts; dispersant: Digo 610s, 0.3 parts;

[0108] The kaolin intercalation-modified epoxy resin network polymer is obtained by the intercalation reaction of kaolin intercalation compound and modified epoxy resin.

[0109] The modified epoxy resin is obtained by modifying a low molecular weight epoxy resin with a diamine;

[0110] The molecular weight of the low molecular weight epoxy resin is 2000-4000;

[0111] The kaolin intercalation composite is intercalated by urea.

[0112] The preparation method of the epoxy composite intercalation anti-corrosion coating comprises the following steps:

[0113] S1, preparing modified epoxy resin;

[0114] S11, preparing a low molecular weight epoxy resin: adding bisphenol A and epichlorohydrin (molar ratio of 4:1) into an organic solvent, stirring and dissolving, and then heating to 50-75° C., and then adding a 10% by mass fraction sodium hydroxide solution (molar ratio of sodium hydroxide to bisphenol A is 0.8:1) to react to obtain a low molecular weight epoxy resin;

[0115] S12, preparing modified epoxy resin: adding diamine (the molar ratio of epoxy resin to diamine is 1:1) to the low molecular weight epoxy resin prepared in step S11, stirring and heating to 80-90° C., and continuing stirring and reacting for 2-8 hours to obtain modified epoxy resin;

[0116] S2, preparing kaolin intercalation composite;

[0117] The dried kaolin is added into a 15% urea aqueous solution (molar ratio of 0.2:1), and reacted at room temperature with stirring for 10-24 hours, and then washed with 50-60° C. ethanol to obtain a kaolin intercalation composite.

[0118] S3, prepare component A and component B respectively;

[0119] S4. Add component B into component A, and stir and disperse them evenly to obtain the coating.

[0120] Performance test

[0121] 1. Permeability test

[0122] Test method: Apply the paint on the surface of the steel plate, immerse it in water with red color developer after it dries and forms a film, wipe it clean after 24 hours and observe whether the paint cross section has the color of the color developer

[0123] 2. Adhesion test

[0124] Test method: cross-cut method

[0125] 3. Anti-corrosion performance test

[0126] Test method: Test according to the method specified in SYT0457-2000

[0127] The test results are shown in Table 1 below.

[0128] Table 1 Anticorrosion coating performance test results

[0129]

[0130] According to the test data in Table 1 above, it can be seen that the epoxy composite intercalation anti-corrosion coating prepared by the present invention adopts a high cross-linking density polymer network formed by a low molecular weight epoxy resin modified by diamine, and introduces a kaolin intercalation composite into the polymer network, and adopts urea intercalation kaolin, which has a small molecular weight and a high degree of intercalation, and can obtain a multi-layer kaolin intercalation structure, which not only improves the permeability resistance and adhesion of the coating, achieves good anti-corrosion performance, but also improves the barrier performance of the coating.

[0131] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. An epoxy composite intercalation anti-corrosion coating, characterized in that: The invention comprises component A and component B, wherein the raw materials of component A include, by weight: 20-30 parts of kaolin intercalation-modified epoxy resin network polymer, 30-40 parts of organic solvent, 10-15 parts of film former, 7-10 parts of filler and 1-5 parts of additive; The raw materials of component B include, by weight: 40-50 parts of organic solvent and 25-40 parts of curing agent; The kaolin intercalation-modified epoxy resin network polymer is obtained by the intercalation reaction of kaolin intercalation composite and modified epoxy resin; The modified epoxy resin is obtained by modifying a low molecular weight epoxy resin with a diamine; The molecular weight of the modified epoxy resin is 1000-5000; The kaolin intercalation composite is intercalated by urea; The organic solvent is selected from one or more of acetone, ethanol, isobutanol and ethyl acetate; The film-forming agent is selected from one or more of amino resin, organic silicon resin, organic fluorine resin, ethyl silicate, sodium silicate and acrylic resin; The filler is a mixture of nano titanium dioxide, nano zirconium dioxide and pigment; the nano titanium dioxide is 1-5 parts, the nano zirconium dioxide is 2-7 parts, and the pigment is 1-5 parts; The curing agent is dicyandiamide; The preparation method of the epoxy composite intercalation anti-corrosion coating comprises the following steps: S1, preparing modified epoxy resin; The preparation of the modified epoxy resin also includes the following steps: S11, preparing a low molecular weight epoxy resin: adding bisphenol A and epichlorohydrin into an organic solvent, stirring and dissolving, and then heating to 50-75° C., and then adding a 10% by mass sodium hydroxide solution to react to obtain a low molecular weight epoxy resin; S12, preparing modified epoxy resin: adding diamine to the low molecular weight epoxy resin prepared in step S11, stirring and heating to 80-90° C., and continuing stirring and reacting for 2-8 hours to obtain modified epoxy resin; S2, preparing kaolin intercalation composite; The preparation method of the kaolin intercalation composite is as follows: adding dry kaolin to an aqueous solution of urea, stirring and reacting at room temperature for 10-24 hours, and then washing with 50-60° C. ethanol to obtain the kaolin intercalation composite; S3, prepare component A and component B respectively; S4, adding component B to component A, and stirring and dispersing them evenly to obtain the coating; The molar ratio of bisphenol A to epichlorohydrin is 1:3-9; the molar ratio of the low molecular weight epoxy resin to the diamine is 1:0.8-2.