A low-temperature synergistic co-extruded white packaging film and its preparation process
By using a low-temperature synergistic co-extruded white encapsulating film with a white high-reflective layer and an infrared unidirectional reflective layer in photovoltaic modules, the problem of reduced power generation efficiency caused by rising temperature of photovoltaic modules is solved, achieving higher power generation efficiency and power. output.
Patent Information
- Application Number
- CN202310092167.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-12
AI Technical Summary
The increase in the operating temperature of photovoltaic modules leads to a decrease in power generation efficiency. It is difficult to effectively reduce the module temperature to improve power generation efficiency with existing technology.
A low-temperature synergistic co-extruded white encapsulating film composed of a white high-reflective layer, a transparent layer and an infrared unidirectional reflective layer is used to reduce the operating temperature of the cell by reflecting and transmitting sunlight, and through the infrared unidirectional reflective layer The fluorescent light conversion effect increases the utilization rate of sunlight.
Effectively reduce the operating temperature of photovoltaic modules, improve power generation efficiency and power generation, while keeping the gain of the modules unchanged.
Smart Images

Figure CN116082969B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a packaging adhesive film, in particular to a low-temperature synergistic co-extruded white packaging adhesive film and a preparation process thereof. Background Art
[0002] With the development of the times and the continuous consumption of resources, human beings have realized the urgency and importance of energy. As a renewable energy source, solar energy has been valued by all countries, and the photovoltaic industry has flourished.
[0003] With the development of batteries, auxiliary materials, installation methods, etc., the efficiency of photovoltaic power generation has made breakthroughs again and again. However, from the beginning to the end, there has always been one factor that restricts the power generation efficiency of photovoltaic modules - operating temperature.
[0004] According to relevant test statistics, for every 1°C increase in the operating temperature of the module, the power generation efficiency of N-type single crystal (single glass) decreases by 0.38%, and that of P-type cells decreases by 0.42%. When photovoltaic modules are exposed to strong sunlight for power generation, due to solar radiation and power generation heat conversion, the operating temperature of the modules can often increase by 70°C or even above 100°C, which is a very large loss of power generation. Summary of the invention
[0005] In view of the deficiencies of the prior art, the present invention provides a low-temperature efficiency-enhancing co-extruded white encapsulation film, which comprises a white high-reflection layer, a transparent layer, and an infrared one-way reflection layer from the outside to the inside. The white high-reflection layer has a very high full-band sunlight reflection, which plays a role in reflecting sunlight and improving the utilization rate of sunlight; the infrared one-way reflection layer has a strong one-way infrared transmittance and visible light transmittance. When the film is used to make a photovoltaic module, the sunlight irradiated on the gap of the module and the infrared band sunlight that passes through the battery cell to reach the film layer will reflect the infrared band sunlight again after being reflected by the white high-reflection layer and reaching the infrared one-way reflection layer, and the infrared one-way reflection layer will reflect the infrared band sunlight again, and repeat until all the energy is consumed as heat energy in the film layer, thereby reducing the actual working temperature of the battery cell and increasing the power generation efficiency in disguise. The high visible light transmittance of the infrared one-way transmission layer can keep the gain of the white film for the module unchanged. At the same time, the infrared one-way reflection layer has a certain fluorescence conversion effect, which increases the utilization rate of sunlight in disguise and increases the actual power generation power of the module.
[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0007] A low-temperature efficiency-enhanced co-extruded white packaging film, consisting of three layers, which are, from the outside to the inside, a white high-reflection layer, a transparent layer, and an infrared one-way reflection layer.
[0008] Generally speaking, the sunlight that shines on the gaps in the components and the infrared sunlight that passes through the cells and reaches the film layer will act on the surface of the cells again after being reflected by the white film. Since the infrared response of the cells is very weak, most of the infrared solar energy that acts on the cells will be converted into heat energy, causing the temperature of the cells to rise. The increase in power generation temperature will lead to a decrease in the power generation efficiency of the cells and an increase in the heat conversion efficiency, causing the operating temperature of the cells to rise over a large area and a decrease in power generation efficiency.
[0009] Compared with the traditional white film, the sunlight irradiated on the gap of the module and the infrared band sunlight that passes through the cell to reach the film layer will be reflected by the white high reflection layer and reach the infrared one-way reflection layer. The infrared band sunlight will be reflected again, and the energy will be consumed as heat energy in the film layer, thereby reducing the actual working temperature of the cell and increasing the power generation efficiency in disguise. The high visible light transmittance of the infrared one-way transmission layer can keep the gain of the white film for the module unchanged. At the same time, the infrared one-way reflection layer has a certain fluorescence conversion effect, which increases the utilization rate of sunlight in disguise and increases the actual power generation of the module.
[0010] As the only efficiency-enhancing film, white encapsulation film occupies a stable market share in the photovoltaic market. If it can ensure its efficient reflection while reducing the operating temperature of the packaging components, it will be a major improvement in the power generation efficiency of the photovoltaic industry.
[0011] Preferably, the white high reflective layer comprises, by weight:
[0012] 100 parts of base resin; 10-30 parts of white masterbatch; 0.2-2 parts of peroxide initiator; 0.2-1.5 parts of auxiliary crosslinking agent; 0.1-2 parts of silane coupling agent; 0.1-1 parts of light stabilizer; 0.1-3 parts of UV initiator;
[0013] The matrix resin material is POE or EVA resin.
[0014] Preferably, the transparent layer comprises, by weight: 100 parts of base resin; 0.2-2 parts of peroxide initiator; 0.2-1.5 parts of auxiliary cross-linking agent; 0.1-2 parts of silane coupling agent; 0.1-1 parts of light stabilizer;
[0015] The base resin is EVA or POE resin.
[0016] Preferably, the infrared one-way reflection layer comprises, by weight: 100 parts of base resin; 1-50 parts of infrared reflection masterbatch; 0.2-2 parts of peroxide initiator; 0.2-1.5 parts of auxiliary cross-linking agent; 0.1-2 parts of silane coupling agent; 0.1-1 parts of light stabilizer; 0.1-5 parts of structural stabilizer;
[0017] The base resin is EVA or POE resin.
[0018] Preferably, the infrared reflective masterbatch comprises:
[0019] 100 parts of POE / EVA resin, 20-60 parts of infrared reflective filler, 0.2-2 parts of structural stabilizer, and 0.1-2 parts of silane coupling agent;
[0020] The infrared reflective masterbatch is prepared by the following method: putting the resin into a twin-screw extruder granulator, pumping in the structural stabilizer and the structural stabilizer in the first stage, and setting the temperature of the first stage to 120°C-150°C; adding the infrared reflective filler in the second stage, and gradually reducing the temperature of the second stage from 120°C-150°C to 80°C-90°C, and maintaining the temperature of the third stage at 80°C-90°C, and then cutting into granules, and controlling the length of the second stage to 1.5m-2m.
[0021] Preferably, the peroxide initiator is one or more of tert-amyl peroxy-2-ethylhexyl carbonate, di-tert-butyl peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, 5-dimethylethane, cumene oxide, tert-butyl peroxy isopropyl carbonate, 3,3-di(tert-butylperoxy)butyrate, and n-butyl 4,4-di(tert-amylperoxy)valerate;
[0022] The auxiliary cross-linking agent is one or a combination of triallyl isocyanate, ethylenediaminetetramethylenephosphonic acid, triethylene glycol dimethacrylate, 1,3,5-tri-2-propenyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, triallyl isocyanate, ethylene glycol dimethacrylate, dibenzoylbenzoquinone dioxime, xylene ketone, and 2-hydroxy-2-methyl-1-(4-(2-hydroxyethoxy)phenyl)-1-propanone;
[0023] The silane coupling agent is one or more of γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrichlorosilane, trimethoxysilane, 2-(3,4-epoxycyclohexyl)hexyltrimethoxysilane, bistriethoxysilylpropylamine, tetraethyl orthosilicate Si-40, γ-methacryloxypropyltrimethoxysilane, and 3-methacryloxypropyltri(trimethylsiloxy)silane;
[0024] The UV initiator is one or more of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, m-phenoxybenzyl acrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylol triacrylate, ethoxylated phenoxy acrylate, and isobornyl methacrylate;
[0025] The light stabilizer is one or more of N,N,-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, sebacate bis-2,2,6,6-tetramethylpiperidinol ester, and bis(2,2,6,6-tetramethylpiperidinyl) sebacate;
[0026] The structural stabilizer is one or more of 1,4-naphthoquinone, 1,4-p-benzoquinone, 4-methoxyphenol and hydroquinone.
[0027] Preferably, the infrared reflective filler is a ferroferric oxide-bridged nanocomposite of one or more of cadmium selenide, cadmium sulfide, zinc sulfide, titanium dioxide, and zirconium oxide.
[0028] Preferably, the thickness of the white high-reflection layer is 0.2-2 mm; the thickness of the transparent layer is 0.2-2 mm, and the thickness of the infrared one-way reflection layer is 0.05-0.3 mm.
[0029] A preparation process of a low-temperature synergistic co-extruded white packaging film, wherein the low-temperature synergistic co-extruded white packaging film is produced by a three-layer in-mold co-extrusion method, and the co-extrusion die head used is equipped with a high-temperature magnetic field, which can apply a strong magnetic field during the film extrusion process, so that the infrared reflective filler is oriented during the extrusion process to achieve a unidirectional infrared reflection effect.
[0030] Preferably, the magnetic field ranges from 0.5T to 4T.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. Infrared reflective fillers include cadmium selenide, cadmium sulfide, zinc sulfide, titanium dioxide, zirconium oxide and one or more ferroferric oxide bridged nanocomposites. During the multi-layer co-extrusion process, they can be oriented under the action of a strong magnetic field, thereby achieving the function of allowing the normal passage of sunlight in the normal band and unidirectional reflection of sunlight in the infrared band.
[0033] 2. The application of infrared one-way reflection layer allows the visible light band with strong cell response band to maintain normal passage, and intercepts infrared sunlight in a directional manner, so that the infrared sunlight that shines on the gap of the component and passes through the cell sheet and is reflected by the white high reflection layer to reach the infrared one-way reflection layer is reflected again, and the energy is reciprocated until all the energy is consumed as heat energy in the film layer. Due to the high specific heat capacity of the film, the temperature rise is lower. At the same time, because the heat is concentrated in the film, the heat dissipation distance is shorter and the heat dissipation is faster. The functions of the two achieve the purpose of reducing the working temperature of the component and increasing the actual power generation.
[0034] 3. The infrared one-way reflection layer has a certain fluorescence conversion effect, which can further convert ultraviolet sunlight into visible light, increase the utilization rate of sunlight, and increase the actual power generation of the components in disguise. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 It is a structural diagram of the packaging film of the present invention.
[0036] Reference numerals: 1. battery cell; 2. infrared one-way reflection layer; 3. transparent layer; 4. white high reflection layer. DETAILED DESCRIPTION
[0037] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.
[0038] Embodiment 1:
[0039] A low-temperature synergistic co-extruded white packaging film, consisting of three layers, which are, from the outside to the inside, a white high-reflection layer, a transparent layer, and an infrared one-way reflection layer.
[0040] The white high-reflective layer uses POE as the base resin, and its ingredients are 100 parts of POE, 20 parts of white masterbatch, 0.7 parts of 2-ethylhexyl peroxide tert-pentanoic acid, 0.9 parts of triallyl isocyanate, 1.0 parts of vinyl trichlorosilane, 0.2 parts of bis(2,2,6,6-tetramethylpiperidinyl) sebacate, and 1.0 parts of trimethylolpropane triacrylate.
[0041] The transparent layer uses POE as the base resin, and its ingredients are 100 parts of POE resin, 0.7 parts of 2-ethylhexyl peroxide tert-pentanoic acid, 0.9 parts of triallyl isocyanurate, 1.0 parts of vinyl trichlorosilane, 0.2 parts of bis(2,2,6,6-tetramethylpiperidinyl) sebacate, and 1.0 parts of trimethylolpropane triacrylate.
[0042] The infrared one-way reflection layer uses POE as the base resin, and its ingredients are 100 parts of POE resin, 15 parts of infrared reflection masterbatch, 0.7 parts of 2-ethylhexyl peroxide tert-pentanoic acid, 0.9 parts of triallyl isocyanurate, 1.0 parts of vinyl trichlorosilane, 0.2 parts of bis(2,2,6,6-tetramethylpiperidinyl) sebacate, 1.0 parts of trimethylolpropane triacrylate, and 0.4 parts of 1,4-naphthoquinone.
[0043] The infrared reflective masterbatch uses POE as the base resin, and its composition is 100 parts of POE base resin, 40 parts of cadmium selenide, titanium dioxide ferroferric oxide bridged nanocomposite in equal proportions, 0.2 parts of 1,4-naphthoquinone, and 0.7 parts of vinyltrichlorosilane. The first stage temperature is set at 135°C, the second stage temperature settings are 135°C, 120°C, 105°C, and 85°C respectively, and the third stage temperature is maintained at 85°C.
[0044] Magnetic field strength: 0.5T.
[0045] Embodiment 2:
[0046] A low-temperature synergistic co-extruded white packaging film, consisting of three layers, which are, from the outside to the inside, a white high-reflection layer, a transparent layer, and an infrared one-way reflection layer.
[0047] The white high-reflective layer uses POE as the base resin, and its ingredients are 100 parts of POE, 30 parts of white masterbatch, 0.9 parts of 3,3-di(tert-butylperoxy)butyric acid ethyl ester, 0.9 parts of 1,3,5-tri-2-propenyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1.2 parts of trimethoxysilane, 0.4 parts of bis(2,2,6,6-tetramethylpiperidinyl)sebacate, and 1.0 parts of isobornyl methacrylate.
[0048] The transparent layer uses POE as the base resin, and its ingredients are 100 parts of POE resin, 0.9 parts of 3,3-di(tert-butylperoxy)ethyl butyrate, 0.9 parts of 1,3,5-tri-2-propenyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1.2 parts of trimethoxysilane, 0.4 parts of bis(2,2,6,6-tetramethylpiperidinyl)sebacate, and 1.0 parts of isobornyl methacrylate.
[0049] The infrared one-way reflection layer uses POE as the base resin, and its ingredients are 100 parts of POE resin, 25 parts of infrared reflection masterbatch, 0.9 parts of 3,3-di(tert-butylperoxy)butyric acid ethyl ester, 0.9 parts of 1,3,5-tri-2-propenyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, 1.2 parts of trimethoxysilane, 0.4 parts of bis(2,2,6,6-tetramethylpiperidinyl)sebacate, 1.0 parts of isobornyl methacrylate, and 0.4 parts of 1,4-naphthoquinone.
[0050] The infrared reflective masterbatch uses POE as the base resin, and its composition is 100 parts of POE base resin, 40 parts of cadmium selenide, titanium dioxide ferroferric oxide bridged nanocomposite in equal proportions, 0.5 parts of 1,4-naphthoquinone, and 1 part of vinyltrichlorosilane. The first stage temperature is set at 135°C, the second stage temperature settings are 135°C, 120°C, 105°C, and 85°C respectively, and the third stage temperature is maintained at 85°C.
[0051] Magnetic field strength 1T.
[0052] Embodiment 3:
[0053] A low-temperature synergistic co-extruded white packaging film, consisting of three layers, which are, from the outside to the inside, a white high-reflection layer, a transparent layer, and an infrared one-way reflection layer.
[0054] The white high-reflective layer uses POE as the base resin, and its ingredients are 100 parts of POE, 20 parts of white masterbatch, 1.3 parts of di-tert-butyl peroxide, 0.8 parts of dibenzoylbenzoquinone dioxime, 0.9 parts of bistriethoxysilylpropylamine, 0.6 parts of N,N,-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, and 1.2 parts of propoxylated trihydroxymethyl triacrylate.
[0055] The transparent layer uses POE as the base resin, and its ingredients are 100 parts of POE resin, 1.3 parts of di-tert-butyl peroxide, 0.8 parts of dibenzoylbenzoquinone dioxime, 0.9 parts of bistriethoxysilylpropylamine, 0.6 parts of N,N,-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, and 1.2 parts of propoxylated trimethylol triacrylate.
[0056] The infrared one-way reflection layer uses POE as the base resin, and its ingredients are 100 parts of POE resin, 10 parts of infrared reflection masterbatch, 1.3 parts of di-tert-butyl peroxide, 0.8 parts of dibenzoylbenzoquinone dioxime, 0.9 parts of triethoxysilylpropylamine, 0.6 parts of N,N,-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, 1.2 parts of propoxylated trihydroxymethyl triacrylate, and 0.3 parts of 4-methoxyphenol.
[0057] The infrared reflective masterbatch uses POE as the base resin, and its composition is 100 parts of POE base resin, 60 parts of ferroferric oxide bridged nanocomposite of cadmium sulfide and zirconium oxide in equal proportions, 0.5 parts of 4-methoxyphenol, and 1 part of propoxylated trimethylol triacrylate. The first stage temperature is set at 135°C, the second stage temperature settings are 135°C, 115°C, 100°C, and 80°C respectively, and the third stage temperature is maintained at 80°C.
[0058] Magnetic field strength: 1.5T.
[0059] Embodiment 4:
[0060] A low-temperature synergistic co-extruded white packaging film, consisting of three layers, which are, from the outside to the inside, a white high-reflection layer, a transparent layer, and an infrared one-way reflection layer.
[0061] The white high-reflective layer uses EVA as the base resin, and its ingredients are 100 parts of EVA, 20 parts of white masterbatch, 1.5 parts of tert-butyl peroxyisopropyl carbonate, 1 part of 2-hydroxy-2-methyl-1-(4-(2-hydroxyethoxy)phenyl)-1-propanone, 0.8 parts of bistriethoxysilylpropylamine, 0.9 parts of bis-2,2,6,6-tetramethylpiperidinol sebacate, and 1.2 parts of trimethylolpropane trimethacrylate.
[0062] The transparent layer uses EVA as the base resin, and its ingredients are 100 parts of EVA resin, 1.5 parts of tert-butyl peroxy isopropyl carbonate, 1 part of 2-hydroxy-2-methyl-1-(4-(2-hydroxyethoxy)phenyl)-1-propanone, 0.8 parts of bistriethoxysilylpropylamine, 0.9 parts of bis-2,2,6,6-tetramethylpiperidinol sebacate, and 1.2 parts of trimethylolpropane trimethacrylate.
[0063] The infrared one-way reflection layer uses EVA as the base resin, and its ingredients are 100 parts of EVA resin, 10 parts of infrared reflection masterbatch, 1.5 parts of tert-butyl peroxy isopropyl carbonate, 1 part of 2-hydroxy-2-methyl-1-(4-(2-hydroxyethoxy)phenyl)-1-propanone, 0.8 parts of bistriethoxysilylpropylamine, 0.9 parts of bis-2,2,6,6-tetramethylpiperidinol sebacate, 1.5 parts of trimethylolpropane trimethacrylate, and 0.4 parts of 4-methoxyphenol.
[0064] The infrared reflective masterbatch uses EVA as the matrix resin, and its composition is 100 parts of EVA matrix resin, 60 parts of ferroferric oxide bridged nanocomposite of equal proportions of cadmium sulfide and zirconium oxide, 0.5 parts of 4-methoxyphenol, and 1 part of trimethylolpropane trimethacrylate. The first stage temperature is set at 135°C, the second stage temperature settings are 135°C, 115°C, 100°C, and 80°C respectively, and the third stage temperature is maintained at 80°C.
[0065] Magnetic field strength: 1.5T.
[0066] Embodiment 5:
[0067] A low-temperature synergistic co-extruded white packaging film, consisting of three layers, which are, from the outside to the inside, a white high-reflection layer, a transparent layer, and an infrared one-way reflection layer.
[0068] The white high-reflective layer uses EVA as the base resin, and its ingredients are 100 parts of EVA, 30 parts of white masterbatch, 1.0 parts of tert-butyl peroxide 2-ethylhexyl carbonate, 0.8 parts of triethylene glycol dimethacrylate, 1.2 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, 1.2 parts of bis-2,2,6,6-tetramethylpiperidinol sebacate, and 1.2 parts of m-phenoxybenzyl acrylate.
[0069] The transparent layer uses EVA as the base resin, and its ingredients are 100 parts of EVA resin, 1.0 parts of tert-butyl peroxide 2-ethylhexyl carbonate, 0.8 parts of triethylene glycol dimethacrylate, 1.2 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, 1.2 parts of bis-2,2,6,6-tetramethylpiperidinol sebacate, and 1.2 parts of m-phenoxybenzyl acrylate.
[0070] The infrared one-way reflection layer uses EVA as the base resin, and its ingredients are 100 parts of EVA resin, 40 parts of infrared reflection masterbatch, 1.0 part of tert-butyl peroxide 2-ethylhexyl carbonate, 0.8 part of triethylene glycol dimethacrylate, 1.2 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, 1.2 parts of bis-2,2,6,6-tetramethylpiperidinol sebacate, 1.2 parts of meta-phenoxybenzyl acrylate, 0.2 parts of hydroquinone, and 0.2 parts of 4-methoxyphenol.
[0071] The infrared reflective masterbatch uses EVA as the matrix resin, and its composition is 100 parts of EVA matrix resin, 60 parts of ferroferric oxide bridged nanocomposite of equal proportions of zinc sulfide and zirconium oxide, 0.4 parts of 4-methoxyphenol, and 1.2 parts of m-phenoxybenzyl methacrylate. The first stage temperature is set at 135°C, the second stage temperature settings are 135°C, 115°C, 100°C, and 90°C respectively, and the third stage temperature is maintained at 90°C.
[0072] Magnetic field strength: 2.5T.
[0073] Embodiment 6:
[0074] A low-temperature synergistic co-extruded white packaging film, consisting of three layers, which are, from the outside to the inside, a white high-reflection layer, a transparent layer, and an infrared one-way reflection layer.
[0075] The white high-reflective layer uses EVA as the base resin, and its ingredients are 100 parts of EVA, 10 parts of white masterbatch, 1.9 parts of 4,4-di(tert-amylperoxy)valeric acid n-butyl ester, 1 part of triallyl isocyanate, 1.5 parts of vinyl trichlorosilane, 1.2 parts of bis-2,2,6,6-tetramethylpiperidinol sebacate, and 1.5 parts of m-phenoxybenzyl acrylate.
[0076] The transparent layer uses EVA as the base resin, and its ingredients are 100 parts of EVA resin, 1.9 parts of 4,4-di(tert-amylperoxy) valeric acid n-butyl ester, 1 part of triallyl isocyanate, 1.5 parts of vinyl trichlorosilane, 1.2 parts of bis-2,2,6,6-tetramethylpiperidinol sebacate, and 1.5 parts of m-phenoxybenzyl acrylate.
[0077] The infrared one-way reflection layer uses EVA as the base resin, and its ingredients are 100 parts of EVA resin, 40 parts of infrared reflection masterbatch, 1.9 parts of 4,4-di(tert-amylperoxy)valeric acid n-butyl ester, 1 part of triallyl isocyanate, 1.5 parts of vinyl trichlorosilane, 1.2 parts of bis-2,2,6,6-tetramethylpiperidinol sebacate, 1.5 parts of m-phenoxybenzyl acrylate, and 0.4 parts of 1,4-benzoquinone.
[0078] The infrared reflective masterbatch uses EVA as the matrix resin, and its composition is 100 parts of EVA matrix resin, 60 parts of ferroferric oxide bridging nanocomposite of zinc sulfide and zirconium oxide in equal proportions, 0.4 parts of 1,4-benzoquinone, and 1.2 parts of m-phenoxybenzyl acrylate. The first stage temperature is set at 135°C, the second stage temperature settings are 135°C, 115°C, 100°C, and 90°C respectively, and the third stage temperature is maintained at 90°C.
[0079] Magnetic field strength: 3T.
[0080] Comparative Example 1:
[0081] One of the most popular white co-extruded encapsulation films for photovoltaic modules on the market.
[0082] Comparative Example 2:
[0083] One of the most efficient white encapsulation films for photovoltaic modules on the market.
[0084] Test example:
[0085] The packaging films of Examples 1-6 and Comparative Example 1 were used for component packaging. The front layer of the film used a unified high-transmittance EVA packaging film. N-type single crystal and P-type single crystal cells were used for packaging, respectively. Each group of tests used 500 components from the same batch of battery components. All components were installed in the same power station environment, and the power generation and temperature were monitored. The power generation statistics period was 90 days.
[0086] The test results are shown in Table 1. The temperature monitoring was tested using an infrared thermal imager, and the ambient temperature during the monitoring test was 38.17°C;
[0087] Table 1 Encapsulation film component test table
[0088]
[0089]
[0090] It can be seen from the comparative data in Table 1 that the temperature of the components prepared using the product of the present invention is well reduced during outdoor use, and the power generation efficiency is significantly improved.
[0091] The above-mentioned implementation modes are only preferred implementation modes of the present invention and cannot be used to limit the scope of protection of the present invention. Any non-substantial changes and substitutions made by technicians in this field on the basis of the present invention shall fall within the scope of protection required by the present invention.
Claims
1. A low temperature synergistic co-extruded white packaging film, Features: It consists of three layers, from outside to inside, namely white high-reflection layer, transparent layer, and infrared one-way reflection layer; The infrared one-way reflection layer comprises, by weight: 100 parts of base resin; 1-50 parts of infrared reflection masterbatch; 0.2-2 parts of peroxide initiator; 0.2-1.5 parts of auxiliary cross-linking agent; 0.1-2 parts of silane coupling agent; 0.1-1 parts of light stabilizer; 0.1-5 parts of structural stabilizer; the base resin is EVA or POE resin; The infrared reflective masterbatch comprises: 100 parts of POE or EVA resin, 20-60 parts of infrared reflective filler, 0.2-2 parts of structural stabilizer, and 0.1-2 parts of silane coupling agent; The infrared reflective filler is a ferroferric oxide bridged nanocomposite of one or more of cadmium selenide, cadmium sulfide, zinc sulfide, titanium dioxide, and zirconium oxide; The low-temperature enhanced co-extruded white packaging film is produced by a three-layer in-mold co-extrusion method. The co-extrusion die head used is equipped with a high-temperature magnetic field, which can apply a strong magnetic field during the film extrusion process, so that the infrared reflective filler is oriented during the extrusion process to achieve a unidirectional infrared reflection effect.
2. A low temperature synergistic co-extruded white packaging film according to claim 1, Features: The white high-reflection layer comprises, by weight: 100 parts of base resin; 10-30 parts of white masterbatch; 0.2-2 parts of peroxide initiator; 0.2-1.5 parts of auxiliary crosslinking agent; 0.1-2 parts of silane coupling agent; 0.1-1 parts of light stabilizer; 0.1-3 parts of UV initiator; The matrix resin material is POE or EVA resin; The UV initiator is one or more of trimethylolpropane triacrylate, trimethylolpropane trimethacrylate, m-phenoxybenzyl acrylate, ethoxylated trimethylolpropane triacrylate, propoxylated trimethylol triacrylate, ethoxylated phenoxy acrylate, and isobornyl methacrylate.
3. The low temperature synergistic co-extruded white packaging film according to claim 1, Features: The transparent layer comprises, by weight: 100 parts of base resin; 0.2-2 parts of peroxide initiator; 0.2-1.5 parts of auxiliary cross-linking agent; 0.1-2 parts of silane coupling agent; 0.1-1 parts of light stabilizer; The base resin is EVA or POE resin.
4. The low temperature synergistic co-extruded white packaging film according to claim 1, Features: The infrared reflective masterbatch is prepared by the following method: putting the resin into a twin-screw extruder granulator, pumping in a structural stabilizer and a silane coupling agent in a first stage, and setting the temperature of the first stage to 120°C-150°C; adding the infrared reflective filler in a second stage, and gradually reducing the temperature of the second stage from 120°C-150°C to 80°C-90°C, and maintaining the temperature of the third stage at 80°C-90°C, and then cutting into granules, and controlling the length of the second stage to be 1.5m-2m.
5. A low temperature synergistic co-extruded white packaging film according to claim 2, 3 or 4, Features: The peroxide initiator is one or more of tert-amyl peroxy-2-ethylhexyl carbonate, di-tert-butyl peroxide, tert-butyl peroxy-2-ethylhexyl carbonate, tert-butyl peroxy isopropyl carbonate, 3,3-di(tert-butyl peroxy)butyrate, and n-butyl 4,4-di(tert-amyl peroxy)valerate; The auxiliary cross-linking agent is one or a combination of triallyl isocyanurate, triethylene glycol dimethacrylate, 1,3,5-tri-2-propenyl-1,3,5-triazine-2,4,6(1H,3H,5H)-trione, and ethylene glycol dimethacrylate; The silane coupling agent is one or more of γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, vinyltrichlorosilane, trimethoxysilane, 2-(3,4-epoxycyclohexyl)hexyltrimethoxysilane, bistriethoxysilylpropylamine, tetraethyl orthosilicate Si-40, γ-methacryloxypropyltrimethoxysilane, and 3-methacryloxypropyltris(trimethylsiloxy)silane; The light stabilizer is one or more of N,N'-bis(2,2,6,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine, sebacate bis-2,2,6,6-tetramethylpiperidinol ester, and bis(2,2,6,6-tetramethylpiperidinyl) sebacate; The structural stabilizer is one or more of 1,4-naphthoquinone, 1,4-p-benzoquinone, 4-methoxyphenol and hydroquinone.
6. The low temperature synergistic co-extruded white packaging film according to claim 1, Features: The thickness of the white high-reflection layer is 0.2-2 mm; the thickness of the transparent layer is 0.2-2 mm, and the thickness of the infrared one-way reflection layer is 0.05-0.3 mm.
7. The low temperature enhanced co-extruded white packaging film according to claim 1, Features: The magnetic field ranges from 0.5T to 4T.
Citation Information
Patent Citations
Preparation method of superparamagnetic ferroferric oxide composite magnetic mesoporous material
CN104445438A
Solar cell packaging glue
CN106560932A
Packaging film for solar cell as well as preparation method and application of packaging film
CN108148517A