A kind of elastic composite abrasive and emery cloth and preparation method thereof

By introducing elastic units into composite abrasives and adopting specific formulas and processes, the problems of poor fitting and insufficient processing accuracy of composite abrasives in the field of mirror polishing are solved, and abrasives with high fitting and precision are achieved, avoiding surface scratches Injury, prolongs the grinding life.

CN116083051BActive Publication Date: 2024-11-19BAIGE ABRASIVES CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202211679801.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-11-19
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

The existing abrasive cloth prepared with ceramics or thermosetting resins as bonding agents in the field of mirror polishing has problems such as poor fit, insufficient processing accuracy, and easy scratch on the surface, and the abrasive itself has poor elasticity.

Method used

Using elastic composite abrasives, elastic units such as rubber particles or cork particles are added, and through specific formulas and process preparation methods, the elasticity of the abrasives are improved, the island-like distribution is formed, the elastic deformation ability of the abrasives are enhanced, and the fitting properties with the workpiece are improved. Processing accuracy.

Benefits of technology

The prepared sand cloth has good fit and high processing accuracy, which is not easy to scratch the workpiece, extends the grinding life and improves processing consistency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116083051B_ABST
    Figure CN116083051B_ABST
Patent Text Reader

Abstract

The present invention discloses an elastic composite abrasive and emery cloth and a preparation method thereof. The elastic composite abrasive is composed of the following components by mass percentage: abrasive: 40-55%, elastic unit: 15-30%, phenolic resin: 5-20%, active heat dissipation filler: 1-20%, inert grinding aid filler: 1-30%, lubricating material: 1-8%, plasticizer: 1-3%, coupling agent: 1-2%, pigment: 1-2%; the abrasive types are corundum abrasive and silicon carbide abrasive; the elastic unit includes but is not limited to rubber particles or wood chip particles; the phenolic resin is a stage A water-soluble phenolic resin. The elastic unit is distributed in the composite abrasive in an island shape. When the composite abrasive is squeezed during the grinding process of the emery cloth, the elastic action of the elastic unit can cause the composite abrasive to undergo elastic deformation, thereby improving the conformity of the abrasive to the workpiece and improving the processing accuracy.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of grinding, and in particular relates to an elastic composite abrasive and emery cloth and a preparation method thereof. Background Art

[0002] Composite abrasive: also called stacked abrasive, refers to a large particle group formed by bonding countless small particles of abrasive with a binder. Compared with ordinary abrasives, the grinding tools made of composite abrasives have the advantages of long service life and good processing consistency during grinding.

[0003] Emery cloth: refers to the abrasive tool prepared by bonding the abrasive to a flexible substrate using a binder, also known as flexible abrasive tool.

[0004] Composite abrasives are large particles formed by countless small abrasive particles bonded by a binder. Compared with ordinary abrasives, the emery cloth made of composite abrasives has the advantages of long grinding life and good processing consistency, and is widely used in the grinding and polishing of metal and non-metallic materials. In the prior art, composite abrasives are mainly prepared with ceramics or thermosetting resins as binders. The abrasives themselves have poor elasticity. The emery cloth made of composite abrasives has problems such as poor adherence to the workpiece, insufficient processing accuracy, and easy surface scratches in the field of mirror polishing.

[0005] Patent name: A method for manufacturing emery cloth using an organic binder deposited abrasive; Patent number: CN102729158B.

[0006] This patent discloses a method for preparing an organic binder stacked abrasive, in which a thermosetting phenolic resin is used as a binder to prepare the stacked abrasive, and the abrasive itself has poor elasticity.

[0007] Patent name: A method for manufacturing emery cloth using an inorganic binder deposited abrasive; Patent number: CN102732215B.

[0008] This patent discloses a method for preparing an inorganic binder stacked abrasive, in which ceramic is used as a binder to prepare the stacked abrasive, and the abrasive itself has poor elasticity.

[0009] Patent name: A multi-layer abrasive for coated abrasives, a preparation method thereof, and a coated abrasive; Patent number: CN108972382B.

[0010] This patent discloses a method for preparing multi-layer abrasives for coated abrasive tools, in which ceramic is used as a binder to prepare the stacked abrasives, and the abrasives themselves have poor elasticity.

[0011] In the prior art, composite abrasives are mainly prepared with ceramics or thermosetting resins as binders. The abrasives themselves have poor elasticity, and the emery cloths made therefrom have problems such as poor adherence to the workpiece, insufficient machining accuracy, and easy surface scratches in the field of mirror polishing. Summary of the invention

[0012] The purpose of the present invention is to provide an elastic composite abrasive and emery cloth and a preparation method thereof. The composite abrasive and emery cloth are mainly used in the fields of automobile, biology, medical treatment, energy, etc., including grinding and polishing of metal materials, mirror polishing of decorative materials, surface drawing of stainless steel materials, etc.

[0013] Based on the above purpose, the present invention adopts the following technical solutions:

[0014] An elastic composite abrasive comprises, by mass percentage, 40-55% abrasive, 15-30% elastic unit, 5-20% phenolic resin, 1-20% active heat dissipation filler, 1-30% inert grinding aid filler, 1-8% lubricating material, 1-3% plasticizer, 1-2% coupling agent and 1-2% pigment.

[0015] The abrasives are of the corundum type and silicon carbide type; and the abrasive particle size is 80-1200 meshes.

[0016] The elastic unit is a granular material with elasticity, including but not limited to rubber particles or cork particles; the particle size of the rubber particles or cork particles is 80-240 mesh; the rubber particles are one or a mixture of any proportion of styrene-butadiene rubber, nitrile rubber, and silicone rubber; the cork particles are oak particles.

[0017] The phenolic resin is a stage A water-soluble phenolic resin; the active heat dissipation filler is one of cryolite, potassium fluoroborate, and sodium fluoroborate, or a mixture of two or more thereof in any proportion; the inert grinding aid filler is one of calcium carbonate and wollastonite, or a mixture of two or more thereof in any proportion; the lubricating material is one of talcum powder, graphite, zinc stearate, and calcium stearate, or a mixture of two or more thereof in any proportion; the plasticizer is lignin sulfonate or naphthalene sulfonate; the coupling agent is one of silane coupling agents KH550 and KH570, or a mixture of two or more thereof in any proportion; and the pigment is black iron oxide, red iron oxide, or carbon black.

[0018] The preparation method of elastic composite abrasive includes two steps: mixing and granulation.

[0019] Mixing: Add abrasive, elastic unit, active heat dissipation filler, inert grinding aid filler, lubricating material, plasticizer, coupling agent and pigment into the mixer in sequence and stir. After the powder is evenly stirred, add phenolic resin to the powder while stirring. After the phenolic resin is evenly mixed, add 1-20% of the total mass of the raw materials. Water, stir evenly to improve the fluidity and plasticity of the mixture.

[0020] Granulation: Granulate the mixed material using a granulator to obtain a composite abrasive, dry the composite abrasive in an oven at 70-110°C for 5-8 hours, crush and sieve the dried composite abrasive to obtain an elastic composite abrasive.

[0021] Preparation method of elastic composite abrasive cloth:

[0022] The process includes 9 steps: applying primer on the substrate, planting sand, pre-drying, leveling the sand surface, applying glue, main drying, winding, curing and kneading.

[0023] The substrate is one of treated polyester cloth, pure cotton cloth, and polyester-cotton blended cloth; the unit weight of the substrate is 200-800 g / m 2 ;

[0024] In the primer coating process, the primer viscosity is 1000-3500 mpa·s and the coating amount is 200-500 g / m 2 ;

[0025] In the sand planting process, the composite abrasive particle size is 8-20 mesh, the small particle size of the composite abrasive is 80-1200 mesh, and the amount of sand planting is 400-1000 g / m 2 ;

[0026] The pre-drying process has a drying temperature curve of: temperature 80-105°C, time 45-100 min;

[0027] The sand surface leveling process uses a pair of squeezing rollers to squeeze and level the excess abrasive on the sand surface to ensure the flatness of the sand surface;

[0028] In the above-mentioned adhesive coating process, the adhesive viscosity is 1000-3500 mpa·s and the coating amount is 200-500 g / m 2 ;

[0029] The main drying process has a drying temperature curve of: temperature 65-115°C, time 60-120 min;

[0030] The winding process is hot winding, and the winding temperature is 105-115°C;

[0031] The curing process has a curing temperature curve of: temperature 110-115°C, time 2-6 h;

[0032] The solidified product can be formed into a large roll of abrasive cloth after a kneading process.

[0033] The base glue and the top glue in this application can adopt the existing known formulas. Specifically,

[0034] The base glue composition is:

[0035] Calculated by mass percentage: phenolic resin: 35~50%, polyurethane: 10~15%, filler: 32~52%, penetrant: 1~2%, silane coupling agent: 1~2%.

[0036] The phenolic resin is a stage A water-soluble phenolic resin; the polyurethane is a water-soluble polyurethane; the filler is calcium carbonate, wollastonite or a mixture of two of them in any proportion; the penetrant is fatty alcohol polyoxyethylene ether; and the silane coupling agent is KH550 or KH570 or a mixture of two of them in any proportion.

[0037] The preparation process of the primer is as follows:

[0038] Add phenolic resin and polyurethane into the mixing glue pot, turn on the agitator, the agitator speed is 600 r / min, the stirring time is 3~5 minutes, after mixing evenly, add penetrant and silane coupling agent, continue stirring for 3~5 minutes, then add filler, stir for 10-15 minutes, after the filler is completely mixed, add water, and adjust the viscosity of the base glue to the process value.

[0039] The composition of the compounding material is:

[0040] Calculated by mass percentage: phenolic resin: 35~50%, polyurethane: 5~10%, toughening agent: 1~5%, filler: 45~65%, leveling agent: 1~2%, silane coupling agent: 1~2%, pigment: 1~2%.

[0041] The phenolic resin is a stage A water-soluble phenolic resin; the polyurethane is a water-soluble polyurethane; the toughening agent is one or a mixture of any proportion of liquid nitrile rubber, polyvinyl butyral, polyether sulfone, and polyphenylene ether ketone; the filler is one or a mixture of any proportion of wollastonite, cryolite, potassium fluoroborate, and sodium fluoroborate; the leveling agent is one or a mixture of any proportion of polydimethylsiloxane, polymethylphenylsiloxane, and organic modified polysiloxane; the silane coupling agent is one or a mixture of any proportion of KH550 and KH570; and the pigment is black iron oxide or red iron oxide.

[0042] The process of compounding glue is as follows:

[0043] Add phenolic resin and polyurethane into the mixing pot, turn on the agitator, the agitator speed is 600 r / min, the stirring time is 3~5 minutes, after mixing evenly, add leveling agent, silane coupling agent, toughening agent in turn, continue stirring for 3~5 minutes, then add filler, stir for 10-15 minutes, after the filler is completely mixed, add pigment, stir for 25~35 minutes, finally add water, and adjust the viscosity of the compound to the process value.

[0044] Elastic composite abrasive: plays a grinding role in the abrasive tool;

[0045] Primer: Bond and fix abrasive;

[0046] Coating glue: Coated on the surface of the abrasive to further fix and hold the abrasive.

[0047] During the preparation process of the emery cloth, elastic composite abrasive is introduced. The prepared emery cloth has good conformity to the workpiece, high processing accuracy, and is not easy to scratch the workpiece.

[0048] Composite abrasives are large particles formed by countless small abrasive particles bonded by a binder. Compared with ordinary abrasives, the emery cloth made of composite abrasives has the advantages of long grinding life and good processing consistency, and is widely used in the grinding and polishing of metal and non-metallic materials. In the prior art, composite abrasives are mainly prepared with ceramics or thermosetting resins as binders. The abrasives themselves have poor elasticity. The emery cloth made of composite abrasives has problems such as poor adherence to the workpiece, insufficient processing accuracy, and easy surface scratches in the field of mirror polishing.

[0049] The present invention introduces an elastic unit into the abrasive during the preparation of the composite abrasive to solve the problem that the abrasive itself has poor elasticity. The abrasive cloth made of the elastic composite abrasive has good conformability to the workpiece, high processing accuracy, and is not easy to scratch the workpiece.

[0050] During the preparation of the composite abrasive, an elastic unit is introduced into the abrasive. The elastic unit is a granular elastic material, including but not limited to rubber particles and cork particles, to solve the problem of poor elasticity of the abrasive itself. The elastic unit is distributed in the composite abrasive in an island shape. When the composite abrasive is squeezed during the grinding process of the sandpaper, the elastic action of the elastic unit can cause the composite abrasive to undergo elastic deformation, thereby improving the conformity of the abrasive to the workpiece, improving the processing accuracy, and not easily scratching the workpiece. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] Figure 1 It is a schematic diagram of the elastic composite abrasive structure;

[0052] Figure 2 It is a schematic diagram of elastic composite abrasive cloth;

[0053] Figure 3 This is the surface morphology of the plate after grinding. DETAILED DESCRIPTION

[0054] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments.

[0055] Embodiment 1:

[0056] An elastic composite abrasive comprises, by mass percentage, 50% black silicon carbide with a particle size of 320 meshes, 15% styrene-butadiene rubber particles with a particle size of 120 meshes, 15% stage A water-soluble phenolic resin, 2.5% cryolite, 2.5% potassium fluoroborate, 5% wollastonite, 3% calcium stearate, 3% talc, 1.5% sodium lignin sulfonate, 1.5% silane coupling agent KH550 and 1% carbon black.

[0057] The A-stage water-soluble phenolic resin is a A-stage water-soluble phenolic resin with a viscosity of 1800-2500 mpa·s, a solid content of 76-82wt%, a gel time of 120°C of 12-15min, and a water dilution of ≥1:2.5 at 30°C.

[0058] The preparation method of elastic composite abrasive is as follows:

[0059] Mixing: Add black silicon carbide, styrene-butadiene rubber particles, cryolite, potassium fluoroborate, wollastonite, calcium stearate, talcum powder, sodium lignin sulfonate, silane coupling agent KH550, and carbon black into the mixer in sequence and stir. After the powder is evenly stirred, gradually add phenolic resin to the powder while stirring continuously. After the phenolic resin is evenly mixed, add 5% of the total weight of the raw materials into water and continue to stir evenly to improve the fluidity and plasticity of the mixture.

[0060] Granulation: Granulate the mixed material with a granulator to obtain composite abrasive. Dry the composite abrasive in an oven, and the drying temperature curve is: 70~110℃, 6h (the specific operation is, when the oven temperature is 70℃, put the composite abrasive in, set the heating temperature to 110℃, and the heating time is 6h). Crush and sieve the dried composite abrasive, and the sieve used for sieving is 16 mesh / 20 mesh. Take the basic particles in the middle layer of the sieve to obtain the elastic composite abrasive. The specific schematic diagram is as follows Figure 1 shown.

[0061] Preparation method of elastic composite abrasive cloth:

[0062] The process includes 9 steps: applying primer on the substrate, planting sand, pre-drying, leveling the sand surface, applying glue, main drying, winding, curing and kneading.

[0063] The substrate is a treated polyester cloth with a unit weight of 600 g / m 2 ;

[0064] In the primer coating step, the primer formula is specifically composed of the following by mass percentage: stage A water-soluble phenolic resin: 45%, water-soluble polyurethane: 10%, wollastonite: 42%, fatty alcohol polyoxyethylene ether (CAS No.: 111-09-3): 1.5%, KH550: 1.5%, and the preparation process is: add phenolic resin and polyurethane into the ingredient glue pot in proportion, turn on the agitator, the agitator speed is 600 r / min, the stirring time is 3 minutes, after mixing evenly, add fatty alcohol polyoxyethylene ether and KH550, continue stirring for 3 minutes, then add wollastonite, stir for 15 minutes, after the wollastonite is completely mixed, add water, and adjust the viscosity of the primer to the process value.

[0065] The viscosity of the A-stage water-soluble phenolic resin is 1800-2500 mpa·s, the solid content is 76-82wt%, the gel time at 120°C is 12-15min, and the water dilution at 30°C is ≥1:2.5; the solid content of the water-soluble polyurethane is 45±2wt%; and the pH of the fatty alcohol polyoxyethylene ether is 7.

[0066] The viscosity of the primer is 2500 mpa·s and the coating amount is 350 g / m 2 ;

[0067] In the sand planting process, the elastic composite abrasive particle size is 16-20 mesh, the small particle size of the elastic composite abrasive is 320 mesh, and the sand planting amount is 950 g / m 2 ;

[0068] The pre-drying process has a drying temperature curve of 85°C-30min, 95°C-30min, and 100°C-30min;

[0069] The sand surface leveling process uses a pair of squeezing rollers to squeeze and level the excess abrasive on the sand surface to ensure the flatness of the sand surface;

[0070] In the adhesive coating step, the adhesive coating formula is composed by mass percentage: water-soluble phenolic resin: 40%, water-soluble polyurethane: 5%, polyvinyl butyral (CAS No.: 63148-65-2): 5%, cryolite: 20%, potassium fluoroborate: 20%, wollastonite: 6%, polydimethylsiloxane: 1.5%, KH550: 1.5%, and black iron oxide: 1%.

[0071] The viscosity of the A-stage water-soluble phenolic resin is 1800-2500 mpa·s, the solid content is 76-82wt%, the gel time at 120°C is 12-15min, and the water dilution at 30°C is ≥1:2.5; the solid content of the water-soluble polyurethane is 45±2wt%.

[0072] The preparation process of the compound glue is as follows: add phenolic resin and polyurethane into the glue pot, turn on the agitator, the agitator speed is 600 r / min, the stirring time is 3 minutes, after mixing evenly, add polydimethylsiloxane, KH550, polyvinyl butyral in turn, continue stirring for 3 minutes, then add cryolite and potassium fluoroborate, stir for 15 minutes, after the filler is completely mixed, add black iron oxide, stir for 30 minutes, and finally add water to adjust the viscosity of the compound glue to the process value.

[0073] The viscosity of the composite glue is 3000 mpa·s and the coating amount is 450 g / m 2 ;

[0074] The main drying process, the drying temperature curve is: 65℃-25min, 80℃-25min, 92℃-25min, 102℃-25min, 110℃-25min;

[0075] The winding process is hot winding, and the winding temperature is 113°C;

[0076] The curing process has a curing temperature curve of: temperature 113°C, time 4 h;

[0077] After the solidified product is kneaded, it can be formed into a large roll of sandpaper. The specific schematic diagram is as follows Figure 2 shown.

[0078] Embodiment 2:

[0079] An elastic composite abrasive comprises, by mass percentage, 320-mesh black silicon carbide: 40%, 120-mesh styrene-butadiene rubber particles: 25%, stage A water-soluble phenolic resin: 15%, cryolite: 2.5%, potassium fluoroborate: 2.5%, wollastonite: 5%, calcium stearate: 3%, talc powder: 3%, sodium lignin sulfonate: 1.5%, silane coupling agent KH550: 1.5%, and carbon black: 1%.

[0080] The rest is the same as Example 1.

[0081] Embodiment 3:

[0082] An elastic composite abrasive comprises, by mass percentage, 320-mesh brown corundum: 50%, 120-mesh nitrile rubber particles: 15%, stage A water-soluble phenolic resin: 15%, cryolite: 2.5%, potassium fluoroborate: 2.5%, wollastonite: 5%, calcium stearate: 3%, talc powder: 3%, sodium lignin sulfonate: 1.5%, silane coupling agent KH550: 1.5%, and carbon black: 1%.

[0083] The rest is the same as Example 1.

[0084] Embodiment 4:

[0085] An elastic composite abrasive comprises, by mass percentage, 320-mesh brown corundum: 40%, 120-mesh nitrile rubber particles: 25%, stage A water-soluble phenolic resin: 15%, cryolite: 2.5%, potassium fluoroborate: 2.5%, wollastonite: 5%, calcium stearate: 3%, talc powder: 3%, sodium lignin sulfonate: 1.5%, silane coupling agent KH550: 1.5%, and carbon black: 1%.

[0086] The rest is the same as Example 1.

[0087] Embodiment 5:

[0088] An elastic composite abrasive comprises, by mass percentage, 320-mesh black silicon carbide: 50%, 120-mesh oak particles: 15%, stage A water-soluble phenolic resin: 15%, cryolite: 2.5%, potassium fluoroborate: 2.5%, wollastonite: 5%, calcium stearate: 3%, talc powder: 3%, sodium lignin sulfonate: 1.5%, silane coupling agent KH550: 1.5%, and carbon black: 1%.

[0089] The rest is the same as Example 1.

[0090] Embodiment 6:

[0091] An elastic composite abrasive comprises, by mass percentage, 320-mesh black silicon carbide: 40%, 120-mesh oak particles: 25%, stage A water-soluble phenolic resin: 15%, cryolite: 2.5%, potassium fluoroborate: 2.5%, wollastonite: 5%, calcium stearate: 3%, talc powder: 3%, sodium lignin sulfonate: 1.5%, silane coupling agent KH550: 1.5%, and carbon black: 1%.

[0092] The rest is the same as Example 1.

[0093] Embodiment 7:

[0094] An elastic composite abrasive comprises, by mass percentage, 320-mesh brown corundum: 50%, 120-mesh oak particles: 15%, stage A water-soluble phenolic resin: 15%, cryolite: 2.5%, potassium fluoroborate: 2.5%, wollastonite: 5%, calcium stearate: 3%, talc powder: 3%, sodium lignin sulfonate: 1.5%, silane coupling agent KH550: 1.5%, and carbon black: 1%.

[0095] The rest is the same as Example 1.

[0096] Embodiment 8:

[0097] An elastic composite abrasive comprises, by mass percentage, 40% of 320-mesh brown corundum, 25% of 120-mesh oak particles, 15% of stage A water-soluble phenolic resin, 2.5% of cryolite, 2.5% of potassium fluoroborate, 5% of wollastonite, 3% of calcium stearate, 3% of talc, 1.5% of sodium lignin sulfonate, 1.5% of silane coupling agent KH550 and 1% of carbon black.

[0098] The rest is the same as Example 1.

[0099] The large rolls of abrasive cloth prepared in Examples 1 to 8 were made into abrasive belts with the specifications of width * circumference = 800 mm * 2800 mm, and were put on a sanding machine for grinding. The working current of the sanding machine was 10-15 mA, the belt speed was 15 m / s, and the workpiece feed speed was 3 m / s. The grinding object was a TA15 titanium alloy plate with a width * length = 600 mm * 1000 mm, and the surface morphology of the workpiece after grinding was recorded. The surface morphology of the workpiece after grinding with the abrasive cloth prepared in Example 1 is as follows: Figure 3 As shown, the workpiece surface is smooth, without scratches, and the precision meets the processing requirements.

[0100] After grinding the workpieces in Example 1 to Example 8, the surface accuracy and morphology of the workpieces are as follows:

[0101] Table 1 Surface accuracy of workpiece after grinding

[0102]

[0103] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions for the specific implementation of the present invention rather than to limit it. Ordinary technicians in the relevant technical field should understand that any equivalent substitutions or obvious modifications to the implementation methods of the present invention without changing its performance or use, without violating the purpose of the present invention, should be included in the scope of protection requested by the present invention.

Claims

1. A method for preparing elastic composite abrasive cloth using elastic composite abrasive, characterized in that: The process is as follows: (1) Apply primer on the substrate. The primer viscosity is 1000~3500 mpa·s and the primer coating amount is 200~500 g / m 2 ; (2) Sand planting: elastic composite abrasive is planted on the base glue layer. The particle size of the elastic composite abrasive is 8~20 mesh, the particle size of the small particles that make up the elastic composite abrasive is 80~1200 mesh, and the amount of sand planting is 400~1000 g / m 2 ; (3) Pre-drying: Drying temperature curve: temperature 80~105℃, time 45~100 min (4) Smooth sand surface: Use a pair of squeezing rollers to squeeze and smooth the excess abrasive on the sand surface; (5) Glue coating: The viscosity of the glue is 1000~3500 mpa·s, and the coating amount of the glue is 200~500 g / m 2 ; (6) Main drying: The drying temperature curve is: temperature 65~115℃, time 60~120 min; (7) Winding: The winding method is hot winding, and the winding temperature is 105~115 ℃; (8) Curing: The curing temperature curve is: temperature 110~115℃, time 2~6 h; (9) Knead and roll the sandpaper into a large roll. The elastic composite abrasive is composed of the following components by mass percentage: abrasive: 40-55%, elastic unit: 15-30%, phenolic resin: 5-20%, active heat dissipation filler: 1-20%, inert grinding aid filler: 1-30%, lubricating material: 1-8%, plasticizer: 1-3%, coupling agent: 1-2%, pigment: 1-2%; the elastic unit is a granular substance with elasticity, which is rubber particles or cork particles; the rubber particles are one or a mixture of any proportion of styrene-butadiene rubber, nitrile rubber, and silicone rubber; the active heat dissipation filler is one or a mixture of any proportion of cryolite, potassium fluoroborate, and sodium fluoroborate ; The inert grinding aid filler is one of calcium carbonate and wollastonite or a mixture of two of them in any proportion; the lubricating material is one of talc, graphite, zinc stearate, calcium stearate or a mixture of two or more of them in any proportion; the plasticizer is lignin sulfonate or naphthalene sulfonate; the coupling agent is one of silane coupling agents KH550 and KH570 or a mixture of two of them in any proportion; the abrasive is corundum abrasive and silicon carbide abrasive; the phenolic resin is a stage A water-soluble phenolic resin; the pigment is black iron oxide, red iron oxide or carbon black; the abrasive particle size is 320~1200 mesh; the rubber particles or sawdust particles have a particle size of 80~240 mesh; The elastic composite abrasive is obtained by the following process: (1) Mixing: Add abrasive, elastic unit, active heat dissipation filler, inert grinding aid filler, lubricating material, plasticizer, coupling agent and pigment into a mixer in sequence and stir. After the powder is evenly stirred, add phenolic resin to the powder under stirring. After the phenolic resin is evenly mixed, add 1-20% of the total mass of the raw materials, and stir evenly. (2) Granulation: Granulate the mixed material using a granulator to obtain a composite abrasive, dry the composite abrasive in an oven at 70-110°C for 5-8 hours, crush and sieve the dried composite abrasive to obtain an elastic composite abrasive; The base glue composition is: by mass percentage, phenolic resin: 35-50%, polyurethane: 10-15%, filler: 32-52%, penetrant: 1-2%, silane coupling agent: 1-2%; the phenolic resin is a stage A water-soluble phenolic resin; the polyurethane is a water-soluble polyurethane; the filler is one of calcium carbonate and wollastonite or a mixture of two of them in any proportion; the penetrant is fatty alcohol polyoxyethylene ether; the silane coupling agent is one of KH550 and KH570 or a mixture of two of them in any proportion; The primer is obtained by the following process: Add phenolic resin and polyurethane to the mixing pot, turn on the stirrer, the stirrer speed is 600 r / min, the stirring time is 3-5 minutes, after mixing evenly, add penetrant and silane coupling agent, continue stirring for 3-5 minutes, then add filler, stir for 10-15 minutes, after the filler is completely mixed, add water, and adjust the viscosity of the base rubber to the process value; The composition of the composite glue is as follows: by mass percentage: phenolic resin: 35-50%, polyurethane: 5-10%, toughening agent: 1-5%, filler: 45-65%, leveling agent: 1-2%, silane coupling agent: 1-2%, pigment: 1-2%; the phenolic resin is a stage A water-soluble phenolic resin; the polyurethane is a water-soluble polyurethane; the toughening agent is one or a mixture of any two or more of liquid nitrile rubber, polyvinyl butyral, polyether sulfone, and polyphenylene ether ketone in any proportion; the filler is one or a mixture of any two or more of wollastonite, cryolite, potassium fluoroborate, and sodium fluoroborate in any proportion; the leveling agent is one or a mixture of any two or more of polydimethylsiloxane, polymethylphenylsiloxane, and organic modified polysiloxane in any proportion; the silane coupling agent is one or a mixture of any two of KH550 and KH570 in any proportion; the pigment is black iron oxide or red iron oxide; The compound glue is obtained by the following process: adding phenolic resin and polyurethane into a batch glue pot, turning on the stirrer, the stirrer speed is 600 r / min, the stirring time is 3-5 minutes, after mixing evenly, adding leveling agent, silane coupling agent and toughening agent in sequence, continuing to stir for 3-5 minutes, then adding filler, stirring for 10-15 minutes, after the filler is completely mixed, adding pigment, stirring for 25-35 minutes, and finally adding water to adjust the viscosity of the compound glue to the process value.

2. The method for preparing elastic composite abrasive cloth according to claim 1, characterized in that: The substrate is one of treated polyester cloth, pure cotton cloth, and polyester-cotton blended cloth; the unit weight of the substrate is 200-800 g / m 2 .

3. The elastic composite abrasive cloth prepared by the method of claim 1 or 2.

Citation Information

Patent Citations

  • Organic bond accumulative grinding material and method for preparing abrasive cloth by organic bond accumulative grinding material

    CN102729158B

  • Inorganic binding agent stacked abrasive and method for manufacturing abrasive cloth from same

    CN102732215B

  • A multilayer abrasive for coated abrasives, its preparation method, and the coated abrasive itself.

    CN108972382B

  • Organic bond accumulative grinding material and method for preparing abrasive cloth by organic bond accumulative grinding material

    CN102729158A

  • Thermoplastic elastomer grinding material for polishing and production method thereof

    CN107674294A