A biomass / carbon nanotube wet electrical fiber based on skin-core structure and its preparation method and application

Through the biomass/carbon nanotube wet-electric fibers based on the skin core structure, the coaxial wet spinning technology is adopted to solve the problems of low output power and high production cost of existing wet-electric materials, and high output power density and continuous Coaxial hygroscopic power generation fibers produced by chemical production are suitable for flexible wear and sustainable power generation.

CN116084059BActive Publication Date: 2024-12-03DALIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310038724.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-12
Publication Date
2024-12-03
Estimated Expiration
2043-01-12

AI Technical Summary

Technical Problem

The output power of existing wet-electric materials is low, the production process is complex and the cost is high, making it difficult to achieve industrial production and low-cost high-humidity fibers.

Method used

Using biomass/carbon nanotube wet-electric fibers based on the skin core structure, sodium alginate/PEDOT:PSS is prepared as the cortical active material and multi-wall carbon nanotubes are used to form the core layer inner electrode material. Coaxial hygroscopic power generation fiber with high output power.

Benefits of technology

It has achieved high output power density and continuous production of coaxial hygroscopic power generation fibers, with a maximum instantaneous output power density of 6.15W/m2, suitable for flexible wear and sustainable power generation fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004050415310000041
    Figure BDA0004050415310000041
  • Figure BDA0004050415310000042
    Figure BDA0004050415310000042
  • Figure BDA0004050415310000091
    Figure BDA0004050415310000091
Patent Text Reader

Abstract

The present invention belongs to the field of hygroscopic power generation fibers, and discloses a biomass / carbon nanotube wet power fiber based on a skin-core structure, a preparation method and an application. It includes a skin active material and an electrode material in the core layer, and a coaxial hygroscopic power generation fiber with a skin-core structure is prepared by coaxial wet spinning. Preferably, sodium alginate / PEDOT:PSS is used as the skin active material, and multi-walled carbon nanotubes are used as the electrode material in the core layer, and a coaxial hygroscopic power generation fiber with a skin-core structure is prepared by coaxial wet spinning. The preparation method prepares a coaxial hygroscopic power generation fiber with high power, low process cost and the potential for continuous production, and has high output power. The fiber hygroscopic generator (FMEG) provided by the present invention can spontaneously generate a water concentration difference in the radial direction of the fiber based on its skin-core structure, and provide a better path for proton migration.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of moisture-absorbing power generation fibers, and relates to a biomass / carbon nanotube wet electricity fiber based on a skin-core structure, a preparation method and an application thereof. Background Art

[0002] Faced with the dual pressures of energy shortage and environmental destruction, obtaining energy from the environment is considered an effective way to solve energy and environmental problems. Some typical energy acquisition technologies, such as thermoelectricity, piezoelectricity, and triboelectricity, require the conversion of thermal energy and mechanical energy into electrical energy, and therefore can only work under specific conditions. In addition, the above-mentioned power generation devices usually involve complex structures, fine materials, and high costs. Compared with other energy acquisition technologies, wet electricity has certain advantages. On the one hand, the materials and preparation processes are simple, so the cost is low; on the other hand, wet electricity can directly use water vapor in the air to generate electricity without the need for specific conditions. However, the main problem limiting commercial applications at this stage is low output power, so it is very important to increase the output power of wet electricity materials.

[0003] At present, most wet electric materials are 2D and 3D materials. Compared with 2D and 3D materials, fibers have a larger aspect ratio, which can enhance the interaction between fibers and water, thereby improving wet electric performance. At the same time, fibers can be prepared into 2D and 3D materials through textile processing technology. However, due to the constraints of process, cost and wet electric performance, there are not many studies on wet electric fibers. For example, Chen et al. used wet spinning to prepare cellulose / carbon nanotube hygroscopic power generation fibers. However, its maximum instantaneous output power density is low (3.77x10 -2 W / m 2 ) and other shortcomings. For example, Shao et al. used silver wire as the inner electrode material, adopted the layer-by-layer dipping method to prepare hygroscopic power generation fibers, and wound silver wire around the outside of the fiber as the outer electrode. However, it is difficult to produce continuously by dipping layer by layer, and the price of silver wire is high. The maximum instantaneous power density is low (0.241W / m 2 ) and other shortcomings. For example, Liang et al. used wet spinning to prepare graphene oxide fibers, and used laser reduction and wet electrical annealing to prepare wet electrical fibers with a gradient distribution of oxygen functional groups. However, the laser reduction and wet electrical annealing processes are relatively complicated and the production cost is high. With the development of flexible wearable and self-powered industries, the development of a fiber hygroscopic generator that can be industrially produced, is low-cost and has high wet electrical performance is still a difficult problem that needs to be overcome. Summary of the Invention

[0004] In order to overcome the shortcomings of the existing technology, the present invention provides a biomass / carbon nanotube wet electric fiber based on a skin-core structure and a preparation method and application. The preparation method produces a coaxial hygroscopic power generation fiber with low process cost and the potential for continuous production and high output power.

[0005] The above-mentioned object of the present invention is achieved through the following technical solutions:

[0006] The first objective of the present invention is to provide a biomass / carbon nanotube wet electricity fiber with a skin-core structure. The fiber comprises a skin-layer active material and a core-layer electrode material, and is prepared by coaxial wet spinning. The skin-layer active material is a biomass material or a composite material of a biomass material and a conductive material. The biomass material is any one or more of sodium alginate, chitosan, cellulose, and silk protein. The conductive material is any one or more of PEDOT:PSS, carbon nanotubes, graphene, and silver nanowires. The preferred biomass material and conductive material are sodium alginate and PEDOT:PSS, respectively. The core-layer electrode material is multi-walled carbon nanotubes (MWCNTs).

[0007] The second purpose of the present invention is to protect the above-mentioned most preferred solution: a sodium alginate / carbon nanotube wet electric fiber based on a skin-core structure; sodium alginate / PEDOT:PSS is used as the skin active material, multi-walled carbon nanotubes (MWCNT) are used as the core electrode material, and coaxial wet spinning is used to prepare a coaxial hygroscopic power generation fiber with a skin-core structure.

[0008] The preparation method of the above-mentioned sodium alginate / carbon nanotube wet electrical fiber based on the skin-core structure; the specific steps are as follows:

[0009] S1. Preparation of PEDOT:PSS Aqueous Dispersion

[0010] EDOT was added to a 0.5-0.8 wt% solids aqueous solution of PSS and stirred at 500-1000 rpm to obtain a mixed aqueous solution of EDOT and PSS, wherein the mass ratio of EDOT to PSS was 1:2-1:4. The pH of the mixed aqueous solution of EDOT and PSS was adjusted to 2-3 with 1 mol / L hydrochloric acid, followed by the addition of 0.875-3.5 mmol of ammonium persulfate and 0.0125-0.025 mmol of ferric sulfate hydrate. Stirring was continued at 18-20°C and 500-1000 rpm for 30-60 hours to obtain a crude product. The crude product was placed in a dialysis bag with a molecular weight cut-off of 3000 and purified for 2 days to obtain a PEDOT:PSS aqueous dispersion.

[0011] The most preferred step is to add EDOT to a 0.5 wt% solids aqueous solution of PSS and stir at 500 rpm to obtain a mixed aqueous solution of EDOT and PSS, with a ratio of EDOT to PS of 1:3. The pH is adjusted to 2 with 1 mol hydrochloric acid, followed by the addition of 1.53 mmol of ammonium persulfate and 0.0125 mmol of ferric sulfate hydrate. Stirring is continued at 20°C and 500 rpm for 48 hours to obtain a crude product. The crude product is placed in a dialysis bag with a molecular weight cutoff of 3000 and purified for two days to obtain a PEDOT:PSS aqueous dispersion. The Z-average and solids content of the PEDOT:PSS aqueous dispersion are 569.3 nm and 0.23 wt%, respectively. The conductivity of the dry film of PEDOT:PSS is 10 s / cm.

[0012] S2. Preparation of sodium alginate / PEDOT:PSS solution for the fiber cortex;

[0013] A PEDOT:PSS aqueous dispersion with a solid content of 0.2-0.4 wt% is concentrated by magnetic stirring at 70-95° C. Sodium alginate is added to a PEDOT:PSS aqueous dispersion with a solid content of 0.24-1.5 wt% and stirred at 500-1500 rpm to obtain a fiber cortex sodium alginate / PEDOT:PS solution, wherein the solid content of sodium alginate in the cortex sodium alginate / PEDOT:PSS solution is 2-4 wt%, and the solid content of PEDOT:PSS in the cortex sodium alginate / PEDOT:PS solution accounts for 6-75% of the mass of the sodium alginate.

[0014] This step is most preferably performed by volatilizing a 0.23 wt% solids PEDOT:PSS aqueous dispersion at 80°C by magnetic stirring to a solids content of 0.9 wt%. Then, sodium alginate is added to the 0.9 wt% solids PEDOT:PSS aqueous dispersion and stirred at 500 rpm to obtain a fiber cortex sodium alginate / PEDOT:PS solution, wherein the solids content of PEDOT:PSS in the cortex sodium alginate / PEDOT:PSS solution is 30% by weight of the sodium alginate.

[0015] S3. Preparation of fiber core multi-walled carbon nanotube solution;

[0016] Sodium carboxymethyl cellulose is added to deionized water and stirred at 500-1000 rpm to obtain an aqueous solution of sodium carboxymethyl cellulose with a solid content of 0.15-1 wt%. Carbon nanotubes are added to a ball mill and ball-milled at 300-500 rpm for 0.5-1.5 hours. The ball-milled carbon nanotubes are then added to the sodium carboxymethyl cellulose aqueous solution and ultrasonicated at a power of 120-300 W for 0.5-1.5 hours to obtain an aqueous dispersion of carbon nanotubes with a solid content of 1-2 wt%, wherein the mass ratio of carbon nanotubes to sodium carboxymethyl cellulose is 20:3-2:1. The aqueous dispersion of carbon nanotubes with a solid content of 1-2 wt% is volatilized by magnetic stirring at 70-95°C to a solid content of 8-10 wt%, thereby obtaining a fiber core multi-walled carbon nanotube solution.

[0017] The most preferred method for this step is to add 0.3g of sodium carboxymethyl cellulose to 197.7g of deionized water and stir at 500 rpm. Separately, add 2g of carbon nanotubes to a ball mill and mill at 500 rpm for 1 hour. The milled carbon nanotubes are then added to the sodium carboxymethyl cellulose aqueous solution and ultrasonically treated at 120W for 1.5 hours to obtain a carbon nanotube aqueous dispersion with a solids content of 1wt%. This 1wt% carbon nanotube aqueous dispersion is then evaporated at 80°C using magnetic stirring to a solids content of 8-10wt%, thereby obtaining a fiber core multi-walled carbon nanotube solution.

[0018] S4. Preparation of a coaxial moisture-absorbing power generation fiber with a skin-core structure;

[0019] Use a coaxial spinneret (the inner diameter of the coaxial spinneret is 0.06 cm and the outer diameter is 0.16 cm) to simultaneously inject the fiber sheath sodium alginate / PEDOT:PSS solution prepared in step S2 and the fiber core layer multi-walled carbon nanotube solution prepared in step S3 into a CaCl2 coagulation bath with a solid content of 3-10wt%. After coagulation for 3-10 minutes, a coaxial hygroscopic power generation fiber with a skin-core structure is obtained after washing and drying.

[0020] The most preferred method for this step is: use a coaxial spinneret (the inner diameter of the coaxial spinneret is 0.06 cm and the outer diameter is 0.16 cm) to simultaneously inject the fiber sheath sodium alginate / PEDOT:PSS solution prepared in step S2 and the fiber core layer multi-walled carbon nanotube solution prepared in step S3 into a CaCl2 coagulation bath with a solid content of 5wt%. After coagulation for 5 minutes, the fiber is washed and dried to obtain a coaxial hygroscopic power generation fiber with a skin-core structure.

[0021] The application of the coaxial hygroscopic power generation fiber with a skin-core structure prepared by the above preparation method is specifically as follows: multi-walled carbon nanotubes and sodium alginate / PEDOT:PSS are used as the core layer inner electrode and the skin layer active material, respectively. The fiber hygroscopic power generation generator (FMEG) is assembled by connecting the two ends of the test electrode to the multi-walled carbon nanotubes and sodium alginate / PEDOT:PSS, respectively. One end of the coaxial hygroscopic power generation fiber (1 cm) is immersed in a conductive silver paste to connect the multi-walled carbon nanotubes to the test circuit. The other end of the coaxial hygroscopic power generation fiber is directly connected to the test circuit to obtain a fiber hygroscopic power generation generator (FMEG) for wet electrical performance testing.

[0022] Calculation of power density

[0023] Power density: Power density is an important indicator for measuring wet electrical performance. The maximum instantaneous output power density (Pmi) and the maximum output power density can be calculated using formula (1) and formula (2) respectively.

[0024]

[0025] P mi represents the maximum instantaneous output power; Vmax represents the maximum open-circuit voltage; Imax represents the maximum short-circuit current; S represents the effective area of ​​FMEG.

[0026]

[0027] P mo Indicates the maximum output power; U0 indicates the voltage of the matching load; Rx indicates the resistance of the matching load; l indicates the length of the fiber; and D indicates the diameter of the fiber.

[0028] The coaxial moisture-absorbing power-generating fiber with a skin-core structure prepared by the above preparation method is applied to a flexible wearable fabric. Fifteen coaxial moisture-absorbing power-generating fibers, each 1 cm in length, are fixed to the fabric using polyester fiber. The circuit is connected in parallel (5) and series (3) using metal wires and conductive silver glue to obtain a flexible fabric FMEG. Moisture is used to stimulate the fabric FMEG to generate electricity, which lights up the LED in the circuit.

[0029] FMEG is able to generate a voltage of about 0.6V for up to 13 hours under ambient conditions (relative humidity = 61-64%, T = 21-23°C), due to its skin-core structure. With the help of textile processing technology, the fabric FMEG has an effective area of ​​0.615cm 2 The fabric FMEG is able to light up LED lamps without the need for capacitors. The maximum instantaneous output power density and maximum output power density of the FMEG are up to 6.15W / m 2 (Relative humidity = 90%) and 0.125W / m 2(Relative humidity = 63%), approaching the highest power density reported to date for similar MEG. The excellent wet electrical performance is due to the fiber's skin-core structure. This, on the one hand, provides greater power for proton migration due to the spontaneous water concentration difference formed in the radial direction of the fiber, and on the other hand, reduces the resistance to proton migration.

[0030] The beneficial effects of the present invention compared with the prior art are:

[0031] The sodium alginate / carbon nanotube wet electric fiber with a sheath-core structure provided by the present invention improves the hygroscopic power generation capacity by utilizing a defined sheath-core structure based on a coaxial hygroscopic power generation fiber. In the preparation method of the present invention, the core multi-walled carbon nanotube spinning solution concentration is 8-10wt%. If the concentration is lower than 8wt%, the core carbon nanotubes cannot be properly entangled, and the core electrode fibers are prone to breakage. If the concentration is higher than 10wt%, the core carbon nanotubes tend to gel, resulting in poor spinnability.

[0032] The fiber moisture-absorbing generator (FMEG) provided by the present invention can spontaneously generate a moisture concentration difference in the radial direction of the fiber based on its skin-core structure, and provide a better path for proton migration. The FMEG has high hygroelectric performance and can generate electricity continuously, with a maximum instantaneous output power density and a maximum power density of 6.15W / m 2 and 0.125W / m 2 , enough to power many commercial electronic devices. This flexible, multifunctional, high-performance coaxial fiber is undoubtedly highly competitive in the fields of flexible wearables and sustainable power generation. Serial production is expected. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 Schematic diagram of the preparation process of sodium alginate / carbon nanotube wet electrospinning fibers based on a skin-core structure. (a) Schematic diagram of the preparation of the fiber core solution and skin solution; (b) schematic diagram of the coaxial wet spinning process.

[0034] Figure 2 This is a schematic diagram of the application of sodium alginate / carbon nanotube wet electrical fiber based on skin-core structure.

[0035] Figure 3 The morphology of Coax-P30% fiber is shown in Figure 1. (a) is the surface, (b) is the knot, (c) is the cross section, (d) is the local magnified SEM, and (e) is the actual electron photo.

[0036] Figure 4 This is a schematic diagram of the application of fabric FMEG.

[0037] Figure 5 are scanning electron micrographs of the fiber surfaces and cross sections of Unif-P0%, Unif-P30%, and Coax-P30%.

[0038] Figure 6 This is the EDS spectrum of the skin and core layers of Coax-P30% coaxial hygroscopic power generation fiber.

[0039] Figure 7 Figures 1 and 2 show experimental research results. Figure (a) shows the stress-strain curves of uniform fibers and coaxial hygroscopic power generation fibers. Figure (b) shows the conductivity of uniform fibers with different PEDOT:PSS contents. Figure (c) shows the conductivity of Coax-P30% coaxial hygroscopic power generation fibers with different wiring methods. Figure (d) shows the conductivity of coaxial hygroscopic power generation fibers with different PEDOT:PSS contents using the "skin / core" wiring method.

[0040] Figure 8 Figures 1 and 2 show the results of a study on the wet electrical properties of FEMGs. (a) shows the output voltage detected on a Coax-P30% FMEG (1 cm) using different wiring methods under constant moisture stimulation (copper electrode). Figure (b) shows the maximum output voltage, current, and maximum instantaneous output power density (Pi) of uniform fibers with different ratios. Figure (c) shows the maximum output voltage, current, and Pi of coaxial hygroscopic power generation fibers (copper electrode) with different ratios. Figure (d) shows the effect of metal electrodes on the maximum output voltage, current, and Pi of Coax-P30% FMEG.

[0041] Figure 9 The graphs comparing the output voltage and current of Coax-P30% and Unif-P30% fibers under moisture stimulation are shown in Figure 1. (a) is the output voltage comparison graph; (b) is the current comparison graph.

[0042] Figure 10 Figures 1 and 2 show the results of a study on the wet electrical properties of Coax-P30% fibers. (a) shows the cyclability and memory properties of Coax-P30% fibers under wet and dry N2 stimulation for different durations. (b) shows the output voltage for different numbers of Coax-P30% fibers connected in series. (c) shows the output current for different numbers of Coax-P30% fibers connected in parallel. (d) demonstrates the long-term power generation capability of Coax-P30% fibers in an ambient environment (relative humidity = 61-64%, temperature = 21-23°C).

[0043] Figure 11 Figure (a) shows the dynamic changes of the output voltage and current of Coax-P30% fiber under moisture stimulation. Figure (b) shows the output power density of Coax-P30% fiber under different loads. DETAILED DESCRIPTION

[0044] The present invention is described in detail below by specific examples, but the scope of protection of the present invention is not limited. Unless otherwise specified, the experimental methods used in the present invention are all conventional methods, and the experimental equipment, materials, reagents, etc. used can be obtained from commercial channels.

[0045] Example 1

[0046] 64.46 g of a 0.23 wt% PEDOT:PSS aqueous dispersion was concentrated to 48.5 g under magnetic stirring at 80°C, resulting in a PEDOT:PSS solids content of 0.3 wt%. 1.5 g of SA was added and stirred until homogeneous, yielding cortical spinning solution A1 with a PEDOT:PSS solids content of 10% by mass of sodium alginate. 0.15 g of sodium hydroxymethylcellulose was dissolved in 98.85 g of aqueous solution under magnetic stirring. 1 g of multi-walled carbon nanotubes was ball-milled at 400 rpm for 1 hour and then added to the sodium hydroxymethylcellulose mixed solution. The solution was then ultrasonically treated at 120 W for 1.5 hours to yield a 1 wt% multi-walled carbon nanotube aqueous dispersion. This dispersion was then evaporated to 10 g under magnetic stirring at 80°C, yielding spinning solution B. Spinning solutions A1 and B were simultaneously extruded through a coaxial spinneret into a 5wt% calcium chloride aqueous solution. After coagulation for 5 minutes, the fibers were washed and dried at room temperature to produce Coax-P10% hygroscopic power generation fibers. Application: Multi-walled carbon nanotubes were connected to a copper test electrode at one end of the fiber using conductive silver glue. The copper test electrode was then directly connected to the fiber cortex at the other end to create a hygroscopic generator. Under moisture stimulation, the peak voltage and current were 0.52V and 5.09μA, respectively.

[0047] Example 2

[0048] 193.38g of a PEDOT:PSS aqueous dispersion was concentrated to 48.5g under magnetic stirring at 80°C, resulting in a PEDOT:PSS solids content of 0.9wt%. 1.5g of SA was added and stirred until homogeneous, yielding a cortical spinning solution A2 with a PEDOT:PSS solids content of 30% by mass of sodium alginate. Spinning solution A2 and the aforementioned spinning solution B were simultaneously extruded through a coaxial spinneret into a 5wt% calcium chloride aqueous solution. After coagulation for 5 minutes, the solution was washed with water and dried at room temperature to yield a Coax-P30% hygroscopic power generation fiber. Application: The coaxial fiber was connected to a copper test electrode according to the method described in Example 1 to produce a hygroscopic generator. Under moisture stimulation, the peak voltage and current were 0.49V and 13.49μA, respectively.

[0049] Example 3

[0050] 322.30g of a PEDOT:PSS aqueous dispersion was concentrated to 48.5g under magnetic stirring at 80°C, resulting in a PEDOT:PSS solids content of 1.5wt%. 1.5g of SA was added and stirred until homogeneous, yielding a cortical spinning solution A3 with a PEDOT:PSS solids content of 30% by mass of sodium alginate. Spinning solution A3 and the aforementioned spinning solution B were simultaneously extruded through a coaxial spinneret into a 5wt% calcium chloride aqueous solution. After coagulation for 5 minutes, the solution was washed with water and dried at room temperature to yield a Coax-P50% hygroscopic power generation fiber. Application: The coaxial fiber was connected to a copper test electrode according to the method described in Example 1 to produce a hygroscopic generator. Under moisture stimulation, the maximum voltage and current were 0.09V and 0.53μA, respectively.

[0051] Example 4

[0052] Coax-P 30% hygroscopic power-generating fibers were obtained using the method described in Example 2. Application: Multi-walled carbon nanotubes were attached to an iron test electrode at one end of the fiber using conductive silver glue. The iron test electrode was then directly connected to the fiber's cortex at the other end to create a hygroscopic generator. Under moisture stimulation, the peak voltage and current were 1.20 V and 21.00 μA, respectively.

[0053] Application Example 1

[0054] Multi-walled carbon nanotubes (MWCNTs) and sodium alginate / PEDOT:PSS (sodium alginate / PEDOT:PSS) served as the core electrode and skin active material, respectively. A fiber-type hygroscopic generator (FMEG) was assembled by connecting the two ends of the test electrode to the MWCNTs and the alginate / PEDOT:PSS. One end of a coaxial hygroscopic generator fiber (1 cm) was immersed in a conductive silver paste to connect the MWCNTs to the test circuit. The other end of the coaxial hygroscopic generator fiber was directly connected to the test circuit to obtain the fiber-type hygroscopic generator (FMEG) for wet electrical performance testing.

[0055] Application Example 2

[0056] Simple devices were prepared to demonstrate the application of Coax-P30% FMEG, providing theoretical guidance for flexible wearable and electronic devices. Figure 4The application of FMEG based on Coax-P30% coaxial hygroscopic power generation fiber is shown. Fifteen coaxial hygroscopic power generation fibers with a length of 1 cm are fixed on the fabric using polyester fiber. The circuit is connected in parallel (5) and series (3) through metal wires and conductive silver glue to obtain a flexible fabric FMEG. Moisture is used to stimulate the fabric FMEG to generate electricity to light up the LED in the circuit. Under 1 minute of moisture stimulation, the LED can continue to emit light for nearly 7 minutes, showing good wet electrical performance and the ability to generate electricity continuously. Unlike most studies, the light emission of the LED does not rely on the capacitor, but is completely dependent on the fabric FMEG itself. It is worth noting that the effective length, area and volume of the FMEG used are only 15 cm, 0.615 cm, respectively. 2 and 0.020cm 3 This small, flexible, and high-power-density textile device provides strong theoretical support for the development of the Internet of Things and flexible wearables.

[0057] Comparative Example 1

[0058] The materials are sodium polyacrylate (PAAS) and graphene oxide (GO). The 3D foam material was prepared by freeze-drying method. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0059] Comparative Example 2

[0060] The material is sodium polystyrene sulfonate (PSS)-polyvinyl alcohol (PVA) / polydopamine (PDA). The film material is prepared by spraying. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0061] Comparative Example 3

[0062] Materials: graphene oxide (GO) and paper. The thin film material was prepared by screen printing. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0063] Comparative Example 4

[0064] The material is gelatin, and the thin film material is prepared by spin coating. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0065] Comparative Example 5

[0066] The material is sodium alginate (SA) / silicon dioxide (SiO2) / reduced graphene oxide (rGO), and the 3D foam material is prepared by freeze-drying method. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0067] Comparative Example 6

[0068] The material is natural wood. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0069] Comparative Example 7

[0070] The material is protein nanofiber, and the 3D foam material is prepared by freeze-drying method. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0071] Comparative Example 8

[0072] The material is corn stalks. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0073] Comparative Example 9

[0074] The material is cotton. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0075] Comparative Example 10

[0076] The material is cellulose paper. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0077] Comparative Example 11

[0078] The material is paper, and the electrodes are carved with a pencil to prepare the thin film material. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0079] Comparative Example 12

[0080] The materials are fabric and carbon black. The fabric material is prepared by dipping and coating methods. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0081] Comparative Example 13

[0082] The material is graphene oxide (GO), and the fiber material is prepared by dipping silver wire as the electrode material. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0083] Comparative Example 14

[0084] The material is graphene oxide (GO), and the fiber material is prepared by wet spinning, laser reduction and wet electrical annealing. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0085] Comparative Example 15

[0086] The materials are cellulose and carbon nanotubes (CNTs), and the fiber materials are prepared by wet spinning. The maximum instantaneous output power density and maximum output power density of power generation are shown in Table 1.

[0087] Comparative Example 16 is the test result of Example 4 at 90% humidity; Comparative Example 17 is the test result of Example 4 at 63% humidity.

[0088] Table 1 Maximum instantaneous output power density and maximum output power density of MEG in different studies

[0089]

[0090]

[0091] Experimental research data:

[0092] Uniform fibers containing only SA and PEDOT:PSS were prepared using a conventional uniaxial spinneret using a wet spinning method. Four types of fibers were prepared: SA uniform fibers without PEDOT:PSS, uniform fibers with a PEDOT:PSS ratio of 10% by weight, uniform fibers with a PEDOT:PSS ratio of 30% by weight, and uniform fibers with a PEDOT:PSS ratio of 50% by weight. The SA uniform fibers without PEDOT:PSS were designated Unif-P0%. Uniform fibers with PEDOT:PSS ratios of 10%, 30%, and 50% by weight were designated Unif-P10%, Unif-P30%, and Unif-P50%, respectively.

[0093] Coaxial hygroscopic power-generating fibers were prepared using a wet spinning method. Three types of fibers were prepared: one with a PEDOT:PSS ratio of 10% to the SA mass, one with a PEDOT:PSS ratio of 30% to the SA mass, and one with a PEDOT:PSS ratio of 50% to the SA mass. The fibers with 10%, 30%, and 50% PEDOT:PSS ratios were designated Coax-P10%, Coax-P30%, and Coax-P50%, respectively.

[0094] The morphology, mechanical properties, electrical conductivity and wet electrical properties of the coaxial hygroscopic electricity-generating fibers were evaluated by scanning electron microscopy, X-ray WAXD / SAXS system, mechanical tensile testing machine and digital source meter.

[0095] 1. Morphology of uniform fibers and coaxial hygroscopic electricity-generating fibers

[0096] The morphology of Coax-P30% coaxial hygroscopic power generation fiber is as follows Figure 3 As shown. A groove structure was observed on the fiber surface of Coax-P30% coaxial moisture-absorbing power generation fiber ( Figure 3 (a)), which is due to the uneven shrinkage of the fiber cortex caused by double diffusion during wet spinning, compared with the uniform fiber ( Figure 5), it can be seen that the coaxial hygroscopic power generation fiber has deeper and fewer grooves. This is due to the different solids content of the spinning solution in the sheath and core layers of the SA / PEDOT:PSS coaxial hygroscopic power generation fiber, resulting in inconsistent shrinkage of the sheath and core layers during drying. The core resistance of a 1cm long Coax-P30% coaxial hygroscopic power generation fiber changes from 33Ω to 35Ω after knotting, indicating that the core MWCNTs in the Coax-P30% fiber have not broken.

[0097] The cross section of Coax-P30% coaxial moisture-absorbing power generation fiber is as follows: Figure 3 (c) where position “1” and position “3” represent the cortex and core respectively, which can be Figure 6 The relative ratio of carbon to oxygen in the EDS spectrum is used to confirm the result. The cross section of the Coax-P30% coaxial hygroscopic power generation fiber is elliptical, and its local magnification clearly shows the entanglement between the multi-walled carbon nanotubes. There is a clear interface in the coaxial hygroscopic power generation fiber, but there is no obvious separation between the skin and the core (position 2). In the laboratory, a 40 cm long coaxial hygroscopic power generation fiber ( Figure 3 (e)).

[0098] 2. Mechanical properties of uniform fibers and coaxial hygroscopic power generation fibers

[0099] Figure 7 Figure (a) shows the stress-strain curves of uniform fibers and coaxial hygroscopic power generation fibers. The addition of PEDOT:PSS reduces the tensile strength and elongation at break of the uniform fibers. As a conductive polymer, PEDOT:PSS itself has lower tensile strength and elongation at break than SA, which results in the addition of PEDOT:PS reducing the mechanical properties of the uniform fibers. For the coaxial hygroscopic power generation fibers, as the PEDOT:PSS content increases, their tensile strength and elongation at break gradually decrease, and the change trend is consistent with that of the uniform fibers. This shows that the mechanical properties of the coaxial hygroscopic power generation fibers are mainly contributed by the fiber cortex of SA / PEDOT:PSS, and the multi-walled carbon nanotubes in the core layer are not tightly wound.

[0100] 3. Electrical conductivity of uniform fibers and coaxial hygroscopic power generation fibers

[0101] Figure 7 (b) shows the effect of PEDOT:PSS content on the conductivity of uniform fibers. As can be seen, since PEDOT is a conductive polymer, the conductivity of uniform fibers increases significantly with increasing PEDOT:PSS content. Figure 7(c) shows the conductivity of the Coax-P30% coaxial hygroscopic power generation fiber using different wiring methods. The Coax-P30% coaxial hygroscopic power generation fiber has the highest conductivity, reaching 3317.783 S / m, with the "core / core" wiring method, significantly exceeding the other two wiring methods. This is because MWCNTs are highly conductive. In the "core / core" wiring method, electrons migrate along the fiber core (MWCNTs), resulting in the highest conductivity. (Although the core-core connection has the highest conductivity, conductivity is not the only factor determining wet electrical performance. The best wet electrical performance is achieved in the skin-core connection.) Comparing the "skin / core" and "skin / skin" wiring methods, it can be noted that the "skin / core" connection method has a higher conductivity. This is because in the "skin / core" connection method, electrons tend to migrate first along the radial direction of the coaxial hygroscopic power generation fiber and then along the axial direction (MWCNTs). Therefore, due to the lower electron migration resistance, the conductivity is higher. In this study, the low resistance migration path of electrons is caused by the skin-core structure of the coaxial hygroscopic electricity-generating fiber. Figure 7 As shown in (d), the conductivity of coaxial hygroscopic power generation fibers with different PEDOT:PSS contents under the "skin / core" wiring method was studied. It is obvious that the conductivity of the coaxial hygroscopic power generation fibers increases with the increase of PEDOT:PSS content.

[0102] 4. Wet electrical properties of FEMG for application

[0103] A 1 cm long coaxial hygroscopic power generation fiber was selected as the basic unit for power generation to study the hygroelectric performance of FMEG. Figure 8(a) illustrates the output voltage variation of the FMEG in coaxial hygroscopic fiber optics (FMEGs) with different wiring configurations (skin / skin, core / core, and skin / core) under constant moisture stimulation. The output voltage of the Coax-P30% FMEG in the skin / core wiring increases, then decreases, and finally stabilizes with moisture stimulation, reaching a peak voltage of approximately 0.5V, significantly higher than the other two wiring configurations. The peak voltage of the Coax-P30% FMEG in the skin / skin wiring reaches 0.19V, while the voltage of the Coax-P30% FMEG in the core / core wiring shows little response to moisture stimulation, reaching approximately 0V. This is because the core / core wiring configuration can be considered to use only MWCNTs as the active material, and the high conductivity and low functional group content of MWCNTs result in very low output voltages. However, when the skin / core and skin / skin configurations are compared, the hygroelectric performance differs in two aspects. On the one hand, the skin-core structure of the coaxial fiber allows water to first interact with the surface layer and then gradually penetrate into the fiber, resulting in a water concentration difference in the radial direction of the fiber. Under the action of the water concentration difference, protons are transported from the fiber surface to the interior along the radial direction of the fiber, resulting in higher electrical output. On the other hand, the proton migration paths of the two wiring methods are different. In the skin / core wiring method, proton migration encounters less resistance and tends to first move along the radial direction of the coaxial fiber and then along the fiber axis (MWCNT).

[0104] Pi was calculated by the maximum values ​​of the output voltage and current of FMEGs under constant moisture stimulation, which was used as a criterion for evaluating the wet electrical performance of FMEGs. Figure 8 (bc) shows the extreme output voltage, current and Pi of coaxial and uniform FMEG with different SA / PEDOT:PSS contents under moisture stimulation. Pi is calculated from the extreme voltage and current according to Ohm's law. It can be seen that with the increase of PEDOT:PSS content, the maximum instantaneous power output of uniform and coaxial FMEG tends to increase and then decrease. When the PEDOT:PSS content is 30wt%, the uniform and coaxial FMEG have the best power generation performance of 10.14nW and 6.61μW. This is because PEDOT:PSS increases the conductivity of the active material and reduces the resistance to charge movement, thereby improving its power generation performance. At the same time, the increase of PEDOT:PSS reduces the relative content of polar groups in the active material, resulting in a decrease in power generation performance. Comparison Figure 8 It can be found in (bc) that the maximum instantaneous output power of the coaxial FMEG is almost 1000 times that of the uniform FMEG, which proves the advantage of coaxial fiber in wet electrical research. Comparing the output voltage and current of Unif-P30% and Coax-P30% FMEG under moisture stimulation can also prove the advantage of coaxial fiber in wet electrical research ( Figure 9 ). Figure 8(d) shows the wet electrical performance of Coax-P30% FMEG under constant moisture stimulation when using silver, copper, and iron as external electrodes. It can be seen that FMEG with iron as the external electrode has the best wet electrical performance.

[0105] Coax-P30% FMEG exhibits good cycling ability and memory effect under constant humidity and dry N2 stimulation, indicating that FMEG has environmental adaptability and cyclic power generation capability, which is beneficial for practical applications. Figure 10 As shown in (bc), five Coax-P30% FMEG units connected in series and in parallel can generate an output voltage of approximately 6V and an output current of approximately 100μA, respectively. When the dry Coax-P30% FMEG is placed in a room with a temperature of 21-23°C and a humidity of 61-64%, its output voltage rises from 0V to approximately 0.63V and finally stabilizes at 0.60V for 13 hours ( Figure 10 (d) This continuous power generation capability depends on the unique skin-core structure, which enables the coaxial fiber to spontaneously form a water concentration difference in the radial direction.

[0106] Power density is the main indicator for measuring wet electrical performance. At present, the calculation of power density in wet electrical research is divided into maximum instantaneous output power density and maximum output power density, which are calculated by formulas (1) and (2) respectively. Figure 11 (a) illustrates the dynamic changes in the output voltage and current of the Coax-P30% FMEG under constant humidity stimulation. It can be seen that the output voltage and maximum current values ​​are 1.2 V and 21.0 μA, respectively (relative humidity = 90%). According to Ohm's law, Pi can be calculated as 25.2 μW. The effective area of ​​the Coax-P30% FMEG can be calculated based on the fiber diameter (4.1 x 10 -4 m) and length (0.01 m) is calculated as 4.1×10 -6 m 2 The maximum instantaneous output power density can be calculated using formula (1) as 6.15W / m 2 (Relative humidity = 90%). Figure 11 (b) shows the output power density of the FMEG with Coax-P30% under different loads (RH=63%). When matched with a suitable load (40KΩ), the maximum output power density is 0.125W / m 2 Table 1 shows the maximum instantaneous output power density and maximum output power density of MEG in other studies. It can be found that the FMEG prepared in this study far exceeds the values ​​reported in most studies.

[0107] The abbreviations and material names involved in the present invention are as follows:

[0108]

[0109] The above-described embodiments are only preferred embodiments of the present invention, and are not intended to be all feasible embodiments of the present invention. Any obvious modifications made by a person skilled in the art without departing from the principles and spirit of the present invention should be considered to be included within the scope of protection of the claims of the present invention.

Claims

1. A method for preparing sodium alginate / carbon nanotube wet electrical fiber based on skin-core structure, characterized in that: S1. Preparation of PEDOT:PSS aqueous dispersion; Add EDOT to a PSS aqueous solution with a solid content of 0.5-0.8wt%, and stir evenly at 500-1000 rpm to obtain a mixed aqueous solution of EDOT and PSS, wherein the mass ratio of EDOT to PSS is 1:2-1:4; adjust the pH of the mixed aqueous solution of EDOT and PSS to 2-3 with 1 mol / L hydrochloric acid, and continue to add 0.875-3.5 mmol of ammonium persulfate and 0.0125-0.025 mmol of ferric sulfate hydrate; continue stirring at 18-20° C. and 500-1000 rpm for 30-60 hours to obtain a crude product; place the crude product in a dialysis bag with a molecular weight cutoff of 3000, and purify for 2 days to obtain a PEDOT:PSS aqueous dispersion; S2. Preparing a fiber cortex sodium alginate / PEDOT: PSS solution; concentrating a PEDOT: PSS aqueous dispersion having a solid content of 0.2-0.4wt% at 70-95°C by magnetic stirring; adding sodium alginate to a PEDOT: PSS aqueous dispersion having a solid content of 0.24-1.5wt% and stirring at 500-1500 rpm to obtain a fiber cortex sodium alginate / PEDOT: PS solution, wherein the solid content of sodium alginate in the cortex sodium alginate / PEDOT: PSS solution is 2-4wt%, and the solid content of PEDOT: PSS in the cortex sodium alginate / PEDOT: PS solution accounts for 6-75% of the mass of sodium alginate; S3. Preparation of fiber core multi-walled carbon nanotube solution; Add sodium carboxymethyl cellulose to deionized water, and stir evenly at 500-1000 rpm to obtain an aqueous solution of sodium carboxymethyl cellulose with a solid content of 0.15-1wt%; add carbon nanotubes to a ball mill, and ball mill at 300-500 rpm for 0.5-1.5h, add the ball-milled carbon nanotubes to the above sodium carboxymethyl cellulose aqueous solution, and ultrasonicate at a power of 120-300W for 0.5-1.5h to obtain a carbon nanotube aqueous dispersion with a solid content of 1-2wt%, wherein the mass ratio of carbon nanotubes to sodium carboxymethyl cellulose is 20:3-2:1; volatilize the above carbon nanotube aqueous dispersion with a solid content of 1-2wt% at 70-95°C by magnetic stirring to a solid content of 8-10wt%, to obtain a fiber core multi-walled carbon nanotube solution; S4. Preparation of coaxial moisture-absorbing power-generating fibers having a skin-core structure; The sodium alginate / PEDOT:PSS solution of the fiber sheath prepared in step S2 and the multi-walled carbon nanotube solution of the fiber core prepared in step S3 are simultaneously injected into a CaCl2 coagulation bath using a coaxial spinneret. After coagulation, the coaxial hygroscopic power generation fiber with a skin-core structure is obtained by washing and drying.

2. A sodium alginate / carbon nanotube wet electrical fiber based on a skin-core structure prepared by the preparation method according to claim 1, characterized in that: Coaxial hygroscopic power generation fibers with a skin-core structure were prepared by coaxial wet spinning, with sodium alginate / PEDOT:PSS as the skin active material and multi-walled carbon nanotubes as the core electrode material.

3. Application of the sodium alginate / carbon nanotube wet electrical fiber based on skin-core structure prepared by the preparation method according to claim 1, characterized in that: Specifically: multi-walled carbon nanotubes and sodium alginate / PEDOT:PSS are used as core layer inner electrodes and skin layer active materials, respectively; a fiber hygroscopic generator is assembled by connecting the two ends of the test electrode to the multi-walled carbon nanotubes and sodium alginate / PEDOT:PSS, respectively; one end of the coaxial hygroscopic power generation fiber is immersed in conductive silver paste to connect the multi-walled carbon nanotubes to the test circuit; the other end of the coaxial hygroscopic power generation fiber is directly connected to the test circuit to obtain a fiber hygroscopic generator for wet electrical performance testing.

4. Application of sodium alginate / carbon nanotube wet electrical fiber based on skin-core structure prepared by the preparation method as claimed in claim 1 on flexible wearable fabrics.