A core-wrapped yarn and its preparation method and application

Through the combination of fixed-length heat-setting filaments and low-melting point fibers, the problem of reduced braid yarn and wearing comfort of core-spun wrapped yarns when the wear resistance is improved is solved, and high strength, wear resistance and good wearing comfort are achieved. Preparation of core-spun yarn for comfort.

CN116084068BActive Publication Date: 2024-10-22FUJIAN NEW HUAYUAN TEXTILE GRP CO LTD +4
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310061591.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-19
Publication Date
2024-10-22
Estimated Expiration
2043-01-19

AI Technical Summary

Technical Problem

When existing core-spun wrapped yarns reduce the short fiber content and increase the twisting effect to improve wear resistance, it is easy to cause problems such as braided yarns and reduced wearing comfort during yarn processing.

Method used

The fixed-length heat-set filament I is used as the core filament, and the blended yarn of short fiber and low-melting point fiber is used as the sheath. Through heat treatment, the outer filament II undergoes greater thermal shrinkage to enhance the wrapping effect. At the same time, the mixed yarn The low melting point fiber softens to form a bonding effect, which improves the bonding between fibers to reduce short fiber slippage.

Benefits of technology

While ensuring the mechanical properties of the yarn, it can significantly reduce the phenomenon of braided yarn and improve the wear resistance of the yarn, while maintaining good wearing comfort and environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116084068B_ABST
    Figure CN116084068B_ABST
Patent Text Reader

Abstract

The present invention relates to a core-wrapped yarn and a preparation method and application thereof. The core-wrapped yarn is composed of a core yarn and a filament II wrapped on the core yarn and in a tightened state. The core yarn has a core-wrapped structure, and the core yarn has a filament I as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath. The preparation method is: firstly prepare a yarn with a core-wrapped structure, with a filament I that has been heat-set at a fixed length as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath, and use it as the core yarn, wrap the filament II on its surface to obtain a core-wrapped yarn, and then heat-treat the core-wrapped yarn to obtain a core-wrapped yarn; and the application is to combine and twist two of the above core-wrapped yarns to form a composite yarn. The technology of the present invention is simple and easy to implement, green and environmentally friendly, and can improve the wear resistance of the core-wrapped yarn while ensuring good wearing comfort of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of spinning and relates to a core-wrapped yarn and a preparation method and application thereof. Background Art

[0002] The long / short composite yarn processed from filament and staple fiber has the advantages of good mechanical properties of filament and good wearability of staple fiber, and is widely used in various types of clothing and home textile products. The most common filament / short fiber composite yarn includes: core-spun yarn composed of outer staple fiber and core filament, and wrapped yarn formed by entanglement of filament and staple fiber. In recent years, with the improvement of yarn performance requirements for outdoor sportswear, special clothing and other products, the processing technology of core-spun wrapped composite yarn has developed rapidly.

[0003] Patent CN 105133118 A discloses a yarn with a core-wrapped and wrapped structure, a manufacturing method and a manufacturing device, and reduces the content of staple roving that wraps the core yarn to less than 30wt%. The specific process is: the first step: through the covering movement, the staple roving wraps the core yarn to form the core-wrapped yarn; the second step: through the wrapping movement, the core-wrapped yarn formed in the first step is wrapped by the wrapped yarn to form the core-wrapped wrapped yarn; wherein, the wrapped yarn and the core yarn are fed into the front roller through the transmission roller and the double guide roller, the staple roving is fed into the front roller through the rear roller and the middle roller, the staple roving wraps the core yarn at the front roller jaws to form the core-wrapped yarn, the wrapped yarn wraps the core-wrapped yarn formed in the first step at the front roller jaws at a certain interval to form the core-wrapped wrapped yarn, and then is wound onto the tube yarn.

[0004] Patent CN 109594167 A discloses a double-filament core-spun wrapped yarn production device and a production method thereof. A negative pressure gathering system is installed between a front drafting roller pair and an output roller pair. Front and rear suction ports are provided on the upper surface of the negative pressure tube. The same roving is pressed and fed by the rear drafting roller pair, and the same left and right whiskers are output after being drafted. The left and right core yarns pass through the inner and outer rollers of the front and rear yarn guide assemblies in an S shape, respectively, and then are pressed by the front roller and output together with the whiskers. The left and right core yarns are first subjected to the negative pressure of the rear suction port to achieve parallel gathering of the fibers in the whiskers toward the middle, and then are subjected to the negative pressure of the front suction port to achieve flipping and gathering, so that the whiskers wrap the core yarns for the first time. After being output by the output roller pair, they are first subjected to weak twisting respectively, so that the whiskers wrap the core yarns for the second time, so that the left and right core-spun yarns are respectively obtained, and then the two are mutually twisted and plied into yarns under the action of strong twisting.

[0005] Patent CN 111793866 A discloses a double-filament double-ply yarn, a fabric made of the double-filament double-ply yarn and a production method thereof. The double-filament double-ply yarn is a double-ply yarn having a core-wrapped yarn made of two nylon filaments and cotton fibers, and the cotton-nylon mass ratio is 1:0.9-1.1. In the spinning process, the long-staple cotton roving is drafted, and at the front roller of the drafting zone, two N40D / 12F nylon filaments passing through the guide wheel are fed in parallel, one filament is used as a core yarn and wrapped inside the cotton fiber, and the other filament is wrapped outside the cotton fiber and twisted, and the twist coefficient is 363 twists / 10cm.

[0006] The preparation of the above core-wrapped composite yarn has the following problems:

[0007] Reducing the staple fiber content and increasing the twisting effect of the yarn to reduce the slippage of the staple fibers in the yarn and thereby improve the wear resistance of the yarn often leads to the generation of small braided yarns during the yarn processing and reduced wearing comfort of the final product. Therefore, it is necessary to provide a method for preparing core-wrapped yarn that can solve the above technical problems. Summary of the invention

[0008] The purpose of the present invention is to solve the problems existing in the prior art and provide a core-wrapped yarn and a preparation method and application thereof.

[0009] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0010] A method for preparing a core-wrapped yarn comprises first preparing a yarn having a core-wrapped structure, with a filament I that has been heat-set to a fixed length as the core and a blended yarn of a short fiber and a low-melting-point fiber as the sheath, and using the yarn as the core yarn, wrapping a filament II on the surface of the yarn to obtain a core-wrapped yarn, and then heat-treating the core-wrapped yarn to obtain the core-wrapped yarn;

[0011] The hot air shrinkage of the filament I after fixed-length heat setting is 5% to 30% less than that of the filament II. The temperature of the yarn heat treatment is both greater than the glass transition temperature of the filament II and higher than the melting point of the low-melting-point fiber, and less than 190°C. This can cause the outer filament II to undergo greater thermal shrinkage, thereby improving its wrapping effect on the yarn body.

[0012] The short fiber content of the core-spun wrapped yarn is 45-68wt%, the twist coefficient of the spun yarn is 300-360, the small braid yarn defect is ≤1 per 100,000 meters, and the yarn wear times are ≥200. Under the condition of ensuring the quality of the yarn, the twist coefficient of the spun yarn can be reduced by 5-20%, thereby reducing the small braid yarn phenomenon caused by strong twist of the core-spun wrapped yarn.

[0013] As the preferred technical solution:

[0014] In the preparation method of a core-spun wrapped yarn as described above, filament II is polyester filament, polyamide filament or polyolefin filament; filament I is polyester filament, polyamide filament or polyolefin filament; staple fiber is natural fiber and / or regenerated cellulose fiber, which can achieve high strength while ensuring good wearing comfort and green environmental protection of the product; low-melting point fiber is low-melting point polyester fiber, low-melting point polyamide fiber or low-melting point PE fiber.

[0015] In the preparation method of a core-wrapped yarn as described above, the mass ratio of the low-melting point fiber to the short fiber is 1:5-20; the ratio of the mass of the short fiber to the total mass of the filament II and the filament I is 50:50-70:30, and the higher mass ratio of the short fiber provides good wearing comfort for the fabric; the mass ratio of the filament II to the filament I is 50:50, which ensures a good core-wrapping effect of the yarn.

[0016] The method for preparing the core-wrapped yarn as described above comprises the following steps:

[0017] (1) Raw material selection: short fibers, low melting point fibers, filament I, and filament II are selected as raw materials;

[0018] (2) Fiber pretreatment and premixing: The short fibers are stored in a warehouse for curing and premixed with low melting point fibers;

[0019] (3) Carding: The premixed fibers are further mixed and combed into strips through a carding machine;

[0020] (4) Drawing: The slivers made by the carding machine are drawn through three drawing frames;

[0021] (5) roving; the mixed sliver obtained in the drawing process is drawn and twisted to form roving;

[0022] (6) Fiber length setting: The filament I is heat-set to a fixed length;

[0023] (7) Spun yarn: After the filament I that has been heat-set to a certain length is used as the core yarn and is covered by the coarse yarn to form a core-wrapped structure, the filament II that has not been heat-set is used as the wrapping yarn and is intertwined with the core-wrapped structure to form a core-wrapped yarn;

[0024] (8) Yarn heat treatment: The core-wrapped yarn is heat treated.

[0025] According to the method for preparing core-spun wrapped yarn as described above, in step (3), the carding machine has a sliver delivery speed of 100-110 m / min; in step (4), the first sliver is fed with 6 mixed slivers, and the drafting multiple is 5.5-6.1 times; the second sliver is fed with 6 mixed slivers, and the drafting multiple is 5.5-6.0 times; the third sliver is fed with 5 mixed slivers, and the drafting multiple is 6.0-6.3, and the sliver delivery speed is 300-320 m / min; in step (5), the roving twist coefficient is not less than 110, and the roving elongation is controlled to be below 1.2%.

[0026] The present invention also provides a core-wrapped yarn prepared by the preparation method of a core-wrapped yarn as described in any of the above items, which is composed of a core yarn and a filament II wrapped on the core yarn and in a tightened state, the core yarn having a core-wrapped structure, the core yarn having the filament I as the core, and a blended yarn of short fibers and low-melting-point fibers as the sheath; the short fiber content of the core-wrapped yarn is 45-68wt%, the spun yarn twist coefficient is 300-360, the braid yarn defect is ≤1 per 100,000 meters, and the yarn wear resistance times are ≥200. While ensuring the quality of the yarn, the spun yarn twist coefficient can be reduced by 5-20%, thereby reducing the braid yarn phenomenon caused by strong twist of the core-wrapped yarn.

[0027] As the preferred technical solution:

[0028] In a core wrap yarn as described above, the low melting point fiber is bonded together with other fibers in the core wrap yarn.

[0029] In the core-spun wrapped yarn as described above, filament II is polyester filament, polyamide filament or polyolefin filament; filament I is polyester filament, polyamide filament or polyolefin filament; staple fiber is natural fiber and / or regenerated cellulose fiber, which can achieve high strength while ensuring good wearing comfort and green environmental protection of the product; low-melting point fiber is low-melting point polyester fiber, low-melting point polyamide fiber or low-melting point PE fiber.

[0030] As described above, the core-wrapped yarn has a mass ratio of low-melting point fiber to short fiber of 1:5-20; the mass ratio of short fiber to the total mass of filament II and filament I of 50:50-70:30, and the higher short fiber mass ratio provides good wearing comfort for the fabric; the mass ratio of filament II to filament I is 50:50, which ensures good core-wrapping effect of the yarn.

[0031] The present invention also provides a composite yarn, which is formed by combining and twisting two core-wrapped yarns on a do-for-do-not twister, and the core-wrapped yarn is a core-wrapped yarn as described in any one of the above items.

[0032] The principle of the present invention is as follows:

[0033] The present invention reduces the heat shrinkage rate of the filament I as the core filament by heat setting the filament I at a fixed length, and makes the heat shrinkage rate smaller than that of the filament II as the outer layer wrapping. When the core-wrapped wrapped yarn is subsequently heat-treated, due to the difference in heat shrinkage rate between the outer layer wrapping filament II that has not been fixed in length and the core layer filament I that has been fixed in length and shaped, the outer layer filament shrinks and tightens due to heat, and the wrapping effect on the yarn is enhanced, so that the lateral bonding effect of the fibers in the yarn is increased; at the same time, the low-melting point fiber mixed in softens and melts after the yarn heat treatment, forming a bonding effect between the fibers. Through the above two aspects, the bonding effect between the fibers in the core-wrapped wrapped yarn is improved, the slippage of the short fibers is reduced, and the high-strength and wear-resistant effect of the yarn is achieved.

[0034] Beneficial effects:

[0035] By adopting the technology of the present invention, the twist coefficient of the spun yarn can be reduced by 5-20% while improving the mechanical properties of the yarn, thereby significantly reducing the phenomenon of small braid yarn caused by strong twist of the core-wrapped yarn. The technology of the present invention is simple and easy to implement, and natural fibers and regenerated cellulose fibers are selected as raw materials. While achieving high strength, it can ensure good wearing comfort and green environmental protection of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 It is a test diagram of the number of yarn abrasion resistance;

[0037] Among them, 1- sewing needle, 2- yarn, 3- weight. DETAILED DESCRIPTION

[0038] The production process of a core-wrapped yarn described in the present invention is further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

[0039] The testing methods of some performance indicators in the following embodiments are as follows:

[0040] Hot air shrinkage: Tested in accordance with GB / T 6505-2017 Test method for thermal shrinkage of chemical fiber filaments.

[0041] Breaking strength: Tested with reference to GB / T 3916-2013 "Determination of breaking strength and elongation at break of single yarn in textile packaged yarn".

[0042] The test method for the number of yarn abrasion resistance is: Figure 1As shown, a No. 18 sewing needle 1 is fixed at an angle of 45° on the test bench of the fabric wear tester. The yarn 2 sample passes through the eye of the sewing needle 1 made of high carbon steel. One end of the yarn 2 is connected to the swing arm of the fabric wear tester, and a weight 3 is hung on the other end to apply pre-tension (0.33 g / tex) to the yarn 2. The swing arm of the fabric wear tester moves back and forth, driving the yarn 2 and the sewing needle 1 to make friction motion. The number of frictions when the short fibers of the yarn are worn to expose the core filaments is recorded. Each sample is tested 20 times and the average value is taken as the yarn wear number.

[0043] The testing method for 100,000-meter braid yarn defects is: perform yarn defect detection on the package yarn according to FZ / T 01050-1997 "Classification and Test Methods for Textile Yarn Defects - Capacitive Type", cut off the yarn defects and place them on a blackboard for analysis.

[0044] Example 1

[0045] A method for preparing a core-wrapped yarn, comprising the following steps:

[0046] (1) Raw material selection: short fibers, low melting point fibers, filament I, and filament II are selected as raw materials;

[0047] The short fiber is cotton fiber, the manufacturer is Dongfang Qianhai, and the brand is grade 237;

[0048] The low melting point fiber is low melting point polyester fiber, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 1.56dtex×38mm;

[0049] Filament I is polyester POY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0050] Filament II is polyester FDY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0051] The mass ratio of the low-melting point fiber to the short fiber is 1:10, the mass ratio of the short fiber to the total mass of the filament II and the filament I is 50:50, and the mass ratio of the filament II to the filament I is 50:50;

[0052] (2) Fiber pretreatment and premixing: After loosening the short fibers, place them in a pile for 12 hours at 25°C and a relative humidity of not less than 60%, and then place them in a cotton box of a round disc plucker for premixing with low-melting-point fibers;

[0053] (3) Cleaning and carding: The premixed fibers are further mixed in a multi-bin blender and carded into slivers by a carding machine. The carding machine has a sliver output speed of 100 m / min.

[0054] (4) Drawing: The slivers made by the carding machine are drawn through three drawing frames, where the first drawing is fed with 6 mixed slivers, with a drafting ratio of 5.5 times; the second drawing is fed with 6 mixed slivers, with a drafting ratio of 5.5 times; the third drawing is fed with 5 mixed slivers, with a drafting ratio of 6, and the delivery speed is 300 m / min;

[0055] (5) roving; the mixed sliver obtained in the drawing process is fed into a roving frame for drawing and twisting to form roving, the roving twist coefficient is 110, and the roving elongation is controlled to be 1%;

[0056] (6) Length setting of filaments: filament I is heat set at a fixed length at a temperature of 100°C for 30 min. The hot air shrinkage of filament I after the fixed length heat setting is 8.2% less than that of filament II.

[0057] (7) Spun yarn: the roving of step (5) is drafted in a spun yarn drafting zone, and the filament II and the filament I subjected to fixed-length heat setting of step (6) are fed to the front roller through a guide hook and a guide wheel respectively, wherein the filament I subjected to fixed-length heat setting is used as a core filament to be coated by the roving whiskers to form a core-wrapped structure, and the filament II that has not been subjected to the setting treatment is used as a wrapping filament to be entangled with the aforementioned core-wrapped structure under the action of twisting to form a core-wrapped wrapped yarn, and the spun yarn twist coefficient is 300;

[0058] (8) Yarn heat treatment: The core-wrapped yarn is heat treated at a temperature of 160°C for 120 seconds.

[0059] The final core-wrapped yarn consists of a core yarn and a filament II wrapped on the core yarn and in a tightened state. The core yarn has a core-wrapped structure, with the filament I as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath. The low-melting-point fibers are bonded together with other fibers in the core-wrapped yarn. The final core-wrapped yarn has a linear density of 18.3tex, a breaking strength of 21.7cN / tex, a yarn wear resistance of 182, and 1 small braid yarn defect per 100,000 meters.

[0060] Comparative Example 1

[0061] A method for preparing a core-wrapped yarn is basically the same as that in Example 1, except that step (6) is omitted, and the "filament I that has been heat-set to a certain length" in step (7) is replaced by the filament I that has not been heat-set in step (1).

[0062] The final core-wrapped yarn has a linear density of 18.7 tex, a breaking strength of 18.1 cN / tex, a yarn abrasion resistance of 133 times, and 2 small braid yarn defects per 100,000 meters.

[0063] By comparing Example 1 with Comparative Example 1, it can be seen that the breaking strength and abrasion resistance of the yarn decrease, and the number of small braid yarn defects per 100,000 meters increases. This is because the filament I that has not been heat-set to a fixed length has poor structural stability. During the heat treatment in step (8), the change in the morphological structure of the filament I will cause a certain degree of damage to the core yarn structure, thereby resulting in a decrease in yarn performance.

[0064] Example 2

[0065] A method for preparing a core-wrapped yarn, comprising the following steps:

[0066] (1) Raw material selection: short fibers, low melting point fibers, filament I, and filament II are selected as raw materials;

[0067] The staple fiber is lyocell staple fiber, the manufacturer is Sateri, the brand is Asia Pacific Sembo 1.33dtex×38mm;

[0068] The low melting point fiber is low melting point PE fiber, the manufacturer is Jiangnan High Fiber, the brand is ES fiber 1.67dtex×38mm;

[0069] Filament I is polyester POY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0070] Filament II is polyester FDY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0071] The mass ratio of the low-melting point fiber to the short fiber is 1:10, the mass ratio of the short fiber to the total mass of the filament II and the filament I is 50:50, and the mass ratio of the filament II to the filament I is 50:50;

[0072] (2) Fiber pretreatment and premixing: After loosening the short fibers, place them in a pile for 12 hours at 25°C and a relative humidity of not less than 60%, and then place them in a cotton box of a round disc plucker for premixing with low-melting-point fibers;

[0073] (3) Cleaning and carding: The premixed fibers are further mixed in a multi-bin blender and carded into slivers by a carding machine. The carding machine has a sliver output speed of 110 m / min.

[0074] (4) Drawing: The slivers made by the carding machine are drawn through three drawing frames, where the first drawing is fed with 6 mixed slivers, with a drafting ratio of 6.1; the second drawing is fed with 6 mixed slivers, with a drafting ratio of 6; the third drawing is fed with 5 mixed slivers, with a drafting ratio of 6.3, and the delivery speed is 300 m / min;

[0075] (5) roving; the mixed sliver obtained in the drawing process is fed into a roving frame for drawing and twisting to form roving, the roving twist coefficient is 110, and the roving elongation is controlled to be 1%;

[0076] (6) Length setting of filaments: filament I is heat set at a fixed length at a temperature of 100°C for 30 min. The hot air shrinkage of filament I after the fixed length heat setting is 8.2% less than that of filament II.

[0077] (7) Spun yarn: the roving of step (5) is drafted in a spun yarn drafting zone, and the filament II and the filament I subjected to fixed-length heat setting of step (6) are fed to the front roller through a guide hook and a guide wheel respectively, wherein the filament I subjected to fixed-length heat setting is used as a core filament to be covered by the roving whiskers to form a core-wrapped structure, and the filament II that has not been subjected to the setting treatment is used as a wrapping filament to be entangled with the aforementioned core-wrapped structure under the action of twisting to form a core-wrapped wrapped yarn, and the spun yarn twist coefficient is 330;

[0078] (8) Yarn heat treatment: The core-wrapped yarn is heat treated at a temperature of 160°C for 120 seconds.

[0079] The final core-wrapped yarn consists of a core yarn and a filament II wrapped on the core yarn and in a tightened state. The core yarn has a core-wrapped structure, with the filament I as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath. The low-melting-point fibers are bonded together with other fibers in the core-wrapped yarn. The final core-wrapped yarn has a linear density of 18.2tex, a breaking strength of 24.3cN / tex, a yarn wear resistance of 171, and 1 small braid yarn defect per 100,000 meters.

[0080] Example 3

[0081] A method for preparing a core-wrapped yarn, comprising the following steps:

[0082] (1) Raw material selection: short fibers, low melting point fibers, filament I, and filament II are selected as raw materials;

[0083] The staple fiber is viscose staple fiber, the manufacturer is Jiangxi Sateri, the brand is Eco-Cosy 1.33dtex×38mm;

[0084] The low melting point fiber is low melting point PE fiber, the manufacturer is Jiangnan High Fiber, the brand is ES fiber 1.67dtex×38mm;

[0085] Filament I is polyester POY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0086] Filament II is polyester FDY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0087] The mass ratio of the low-melting point fiber to the short fiber is 1:20, the mass ratio of the short fiber to the total mass of the filament II and the filament I is 70:30, and the mass ratio of the filament II to the filament I is 50:50;

[0088] (2) Fiber pretreatment and premixing: After loosening the short fibers, place them in a pile for 12 hours at 25°C and a relative humidity of not less than 60%, and then place them in a cotton box of a round disc plucker for premixing with low-melting-point fibers;

[0089] (3) Cleaning and carding: The premixed fibers are further mixed in a multi-bin blender and carded into slivers by a carding machine. The carding machine has a sliver output speed of 110 m / min.

[0090] (4) Drawing: The slivers made by the carding machine are drawn through three drawing frames, where the first drawing is fed with 6 mixed slivers, with a drafting ratio of 6.1; the second drawing is fed with 6 mixed slivers, with a drafting ratio of 6; the third drawing is fed with 5 mixed slivers, with a drafting ratio of 6.3, and the delivery speed is 300 m / min;

[0091] (5) roving; the mixed sliver obtained in the drawing process is fed into a roving frame for drawing and twisting to form roving, the roving twist coefficient is 110, and the roving elongation is controlled to be 1%;

[0092] (6) Length setting of filaments: filament I is heat set at a fixed length at a temperature of 100°C for 30 min. The hot air shrinkage of filament I after the fixed length heat setting is 8.2% less than that of filament II.

[0093] (7) Spun yarn: the roving of step (5) is drafted in a spun yarn drafting zone, and the filament II and the filament I subjected to fixed-length heat setting of step (6) are fed to the front roller through a guide hook and a guide wheel respectively, wherein the filament I subjected to fixed-length heat setting is used as a core filament to be covered by the roving whiskers to form a core-wrapped structure, and the filament II that has not been subjected to the setting treatment is used as a wrapping filament to be entangled with the aforementioned core-wrapped structure under the action of twisting to form a core-wrapped wrapped yarn, and the spun yarn twist coefficient is 330;

[0094] (8) Yarn heat treatment: The core-wrapped yarn is heat treated at a temperature of 160°C for 120 seconds.

[0095] The final core-wrapped yarn consists of a core yarn and a filament II wrapped on the core yarn and in a tightened state. The core yarn has a core-wrapped structure, with the filament I as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath. The low-melting-point fibers are bonded together with other fibers in the core-wrapped yarn. The final core-wrapped yarn has a linear density of 31.1tex, a breaking strength of 19.5cN / tex, a yarn wear resistance of 167, and zero braid yarn defects per 100,000 meters.

[0096] Example 4

[0097] A method for preparing a core-wrapped yarn, comprising the following steps:

[0098] (1) Raw material selection: short fibers, low melting point fibers, filament I, and filament II are selected as raw materials;

[0099] The short fiber is cotton fiber, the manufacturer is Bazhou Guannong, and the brand is grade 237;

[0100] The low melting point fiber is low melting point PE fiber, the manufacturer is Jiangnan High Fiber, the brand is ES fiber 1.67dtex×38mm;

[0101] Filament I is polyester FDY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0102] Filament II is polyester FDY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0103] The mass ratio of the low-melting point fiber to the short fiber is 1:10, the mass ratio of the short fiber to the total mass of the filament II and the filament I is 60:40, and the mass ratio of the filament II to the filament I is 50:50;

[0104] (2) Fiber pretreatment and premixing: After loosening the short fibers, place them in a pile for 12 hours at 25°C and a relative humidity of not less than 60%, and then place them in a cotton box of a round disc plucker for premixing with low-melting-point fibers;

[0105] (3) Cleaning and carding: The premixed fibers are further mixed in a multi-bin blender and carded into slivers by a carding machine. The carding machine has a sliver output speed of 110 m / min.

[0106] (4) Drawing: The slivers made by the carding machine are drawn through three drawing frames, where the first drawing is fed with 6 mixed slivers, with a drafting ratio of 6.1; the second drawing is fed with 6 mixed slivers, with a drafting ratio of 6; the third drawing is fed with 5 mixed slivers, with a drafting ratio of 6.3, and the delivery speed is 320 m / min;

[0107] (5) roving; the mixed sliver obtained in the drawing process is fed into a roving frame for drafting and twisting to form roving, the roving twist coefficient is 115, and the roving elongation is controlled to be 1.1%;

[0108] (6) Length setting of filaments: filament I is heat set at a fixed length at a temperature of 180°C for 30 min. The hot air shrinkage of filament I after the length setting is 6.7% less than that of filament II.

[0109] (7) Spun yarn: the roving of step (5) is drafted in a spun yarn drafting zone, and the filament II and the filament I subjected to fixed-length heat setting of step (6) are fed to the front roller through a guide hook and a guide wheel respectively, wherein the filament I subjected to fixed-length heat setting is used as a core filament to be coated by the roving whiskers to form a core-wrapped structure, and the filament II that has not been subjected to the setting treatment is used as a wrapping filament to be entangled with the aforementioned core-wrapped structure under the action of twisting to form a core-wrapped wrapped yarn, and the spun yarn twist coefficient is 320;

[0110] (8) Yarn heat treatment: The core-wrapped yarn is heat treated at a temperature of 160°C for 120 seconds.

[0111] The final core-wrapped yarn consists of a core yarn and a filament II wrapped on the core yarn and in a tightened state. The core yarn has a core-wrapped structure, with the filament I as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath. The low-melting-point fibers are bonded together with other fibers in the core-wrapped yarn. The final core-wrapped yarn has a linear density of 23.2tex, a breaking strength of 21.1cN / tex, a yarn wear resistance of 185, and a braid yarn defect of 1 per 100,000 meters.

[0112] Example 5

[0113] A method for preparing a core-wrapped yarn, comprising the following steps:

[0114] (1) Raw material selection: short fibers, low melting point fibers, filament I, and filament II are selected as raw materials;

[0115] The staple fiber is cotton fiber, the manufacturer is the former Heizenong, and the brand is grade 229;

[0116] The low melting point fiber is low melting point PE fiber, the manufacturer is Jiangnan High Fiber, the brand is ES fiber 1.67dtex×38mm;

[0117] Filament I is polyester POY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0118] Filament II is high shrinkage polyester FDY filament, the manufacturer is Fujian Jinlun High Fiber, the brand is Jinlun 40D / 12F;

[0119] The mass ratio of the low-melting point fiber to the short fiber is 1:10, the mass ratio of the short fiber to the total mass of the filament II and the filament I is 50:50, and the mass ratio of the filament II to the filament I is 50:50;

[0120] (2) Fiber pretreatment and premixing: After loosening the short fibers, place them in a pile for 12 hours at 25°C and a relative humidity of not less than 60%, and then place them in a cotton box of a round disc plucker for premixing with low-melting-point fibers;

[0121] (3) Cleaning and carding: The premixed fibers are further mixed in a multi-bin blender and carded into slivers by a carding machine. The carding machine has a sliver output speed of 110 m / min.

[0122] (4) Drawing: The slivers made by the carding machine are drawn through three drawing frames, where the first drawing is fed with 6 mixed slivers, with a drafting ratio of 6.1; the second drawing is fed with 6 mixed slivers, with a drafting ratio of 6; the third drawing is fed with 5 mixed slivers, with a drafting ratio of 6.3, and the delivery speed is 320 m / min;

[0123] (5) roving; the mixed sliver obtained in the drawing process is fed into a roving frame for drafting and twisting to form roving, the roving twist coefficient is 115, and the roving elongation is controlled to be 1.1%;

[0124] (6) Length setting of filaments: filament I is heat set at a fixed length at a temperature of 100° C. for 30 min. The hot air shrinkage of filament I after the length setting heat setting is 30% less than that of filament II.

[0125] (7) Spun yarn: the roving of step (5) is drafted in a spun yarn drafting zone, and the filament II and the filament I subjected to fixed-length heat setting of step (6) are fed to the front roller through a guide hook and a guide wheel respectively, wherein the filament I subjected to fixed-length heat setting is used as a core filament to be covered by the roving whiskers to form a core-wrapped structure, and the filament II that has not been subjected to the setting treatment is used as a wrapping filament to be entangled with the aforementioned core-wrapped structure under the action of twisting to form a core-wrapped wrapped yarn, and the spun yarn twist coefficient is 330;

[0126] (8) Yarn heat treatment: The core-wrapped yarn is heat treated at a temperature of 160°C for 120 seconds.

[0127] The final core-wrapped yarn consists of a core yarn and a filament II wrapped on the core yarn and in a tightened state. The core yarn has a core-wrapped structure, with the filament I as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath. The low-melting-point fibers are bonded together with other fibers in the core-wrapped yarn. The final core-wrapped yarn has a linear density of 18.9tex, a breaking strength of 20.8cN / tex, a yarn wear resistance of 196, and zero braid yarn defects per 100,000 meters.

[0128] Example 6

[0129] A method for preparing a core-wrapped yarn, comprising the following steps:

[0130] (1) Raw material selection: short fibers, low melting point fibers, filament I, and filament II are selected as raw materials;

[0131] The staple fiber is cotton fiber, the manufacturer is Aksu Jin'a, and the brand is grade 237;

[0132] The low melting point fiber is a low melting point polyamide fiber, the manufacturer is Fujian Hengshen, and the brand is 1.67dtex×38mm;

[0133] Filament I is nylon 6 POY filament, the manufacturer is Fujian Hengshen, the brand is Hengshen 40D / 12F;

[0134] Filament II is nylon 6FDY filament, the manufacturer is Fujian Hengshen, the brand is Hengshen 40D / 12F;

[0135] The mass ratio of the low-melting point fiber to the short fiber is 1:10, the mass ratio of the short fiber to the total mass of the filament II and the filament I is 50:50, and the mass ratio of the filament II to the filament I is 50:50;

[0136] (2) Fiber pretreatment and premixing: After loosening the short fibers, place them in a pile for 12 hours at 25°C and a relative humidity of not less than 60%, and then place them in a cotton box of a round disc plucker for premixing with low-melting-point fibers;

[0137] (3) Cleaning and carding: The premixed fibers are further mixed in a multi-bin blender and carded into slivers by a carding machine. The carding machine has a sliver output speed of 110 m / min.

[0138] (4) Drawing: The slivers made by the carding machine are drawn through three drawing frames, where the first drawing frame uses 6 mixed slivers for feeding, with a drafting ratio of 5.8 times; the second drawing frame uses 6 mixed slivers for feeding, with a drafting ratio of 5.8 times; the third drawing frame uses 5 mixed slivers for feeding, with a drafting ratio of 6.1, and the delivery speed is 310 m / min;

[0139] (5) roving; the mixed sliver obtained in the drawing process is fed into a roving frame for drawing and twisting to form roving, the roving twist coefficient is 110, and the roving elongation is controlled to be 1%;

[0140] (6) Length setting of filaments: filament I is heat set at a fixed length at a temperature of 100°C for 30 min. The hot air shrinkage of filament I after the length setting is 5% less than that of filament II.

[0141] (7) Spun yarn: the roving of step (5) is drafted in a spun yarn drafting zone, and the filament II and the filament I subjected to fixed-length heat setting of step (6) are fed to the front roller through a guide hook and a guide wheel respectively, wherein the filament I subjected to fixed-length heat setting is used as a core filament to be covered by the roving whiskers to form a core-wrapped structure, and the filament II that has not been subjected to the setting treatment is used as a wrapping filament to be entangled with the aforementioned core-wrapped structure under the action of twisting to form a core-wrapped wrapped yarn, and the twist coefficient of the spun yarn is 360;

[0142] (8) Yarn heat treatment: The core-wrapped yarn is heat treated at a temperature of 180°C for 150 seconds.

[0143] The final core-wrapped yarn consists of a core yarn and a filament II wrapped on the core yarn and in a tightened state. The core yarn has a core-wrapped structure, with the filament I as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath. The low-melting-point fibers are bonded together with other fibers in the core-wrapped yarn. The final core-wrapped yarn has a linear density of 18.4tex, a breaking strength of 22.5cN / tex, a yarn wear resistance of 202, and zero braid yarn defects per 100,000 meters.

[0144] Example 7

[0145] A method for preparing a core-wrapped yarn, comprising the following steps:

[0146] (1) Raw material selection: short fibers, low melting point fibers, filament I, and filament II are selected as raw materials;

[0147] The staple fiber is viscose staple fiber, the manufacturer is Fujian Sateri, the brand is EcoCosy 1.33dtex×38mm;

[0148] The low melting point fiber is low melting point PE fiber, the manufacturer is Jiangnan High Fiber, the brand is ES fiber 1.67dtex×38mm;

[0149] Filament I is PTT POY filament, the manufacturer is Taicang Hongyi, the brand is Hongyi 40D / 12F;

[0150] Filament II is PTT FDY filament, the manufacturer is Taicang Hongyi, the brand is Hongyi 40D / 12F;

[0151] The mass ratio of the low-melting point fiber to the short fiber is 1:5, the mass ratio of the short fiber to the total mass of the filament II and the filament I is 50:50, and the mass ratio of the filament II to the filament I is 50:50;

[0152] (2) Fiber pretreatment and premixing: After loosening the short fibers, place them in a pile for 12 hours at 25°C and a relative humidity of not less than 60%, and then place them in a cotton box of a round disc plucker for premixing with low-melting-point fibers;

[0153] (3) Cleaning and carding: The premixed fibers are further mixed in a multi-bin blender and carded into slivers by a carding machine. The carding machine has a sliver output speed of 110 m / min.

[0154] (4) Drawing: The slivers made by the carding machine are drawn through three drawing frames, where the first drawing is fed with 6 mixed slivers, with a drafting ratio of 6.1; the second drawing is fed with 6 mixed slivers, with a drafting ratio of 6; the third drawing is fed with 5 mixed slivers, with a drafting ratio of 6.3, and the delivery speed is 310 m / min;

[0155] (5) roving; the mixed sliver obtained in the drawing process is fed into a roving frame for drafting and twisting to form roving, the roving twist coefficient is 120, and the roving elongation is controlled to be 1%;

[0156] (6) Length setting of filaments: filament I is heat set at a temperature of 95°C for 30 min. The hot air shrinkage of filament I after the heat setting is 7.8% less than that of filament II.

[0157] (7) Spun yarn: the roving of step (5) is drafted in a spun yarn drafting zone, and the filament II and the filament I subjected to fixed-length heat setting of step (6) are fed to the front roller through a guide hook and a guide wheel respectively, wherein the filament I subjected to fixed-length heat setting is used as a core filament and is covered by the roving whiskers to form a core-wrapped structure, and the filament II that has not been subjected to the setting treatment is used as a wrapping filament under the action of twisting and is entangled with the aforementioned core-wrapped structure to form a core-wrapped wrapped yarn, and the spun yarn twist coefficient is 350;

[0158] (8) Yarn heat treatment: The core-wrapped yarn is heat treated at a temperature of 160°C for 120 seconds.

[0159] The final core-wrapped yarn consists of a core yarn and a filament II wrapped on the core yarn and in a tightened state. The core yarn has a core-wrapped structure, with the filament I as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath. The low-melting-point fibers are bonded together with other fibers in the core-wrapped yarn. The final core-wrapped yarn has a linear density of 18.3tex, a breaking strength of 18.6cN / tex, a yarn wear resistance of 169, and 1 small braid yarn defect per 100,000 meters.

[0160] Example 8

[0161] A composite yarn is formed by combining and twisting two core-wrapped yarns of Example 5 on a two-for-one twister.

[0162] The linear density of the composite yarn is 38.2tex, the breaking strength is 30.5cN / tex, the yarn abrasion resistance is 255 times, and the number of small braid yarn defects in 100,000 meters of yarn defects is 1.

[0163] Example 9

[0164] A composite yarn is formed by combining and twisting two core-wrapped yarns of Example 6 on a two-for-one twister.

[0165] The linear density of the composite yarn is 37.0tex, the breaking strength is 32.2cN / tex, the yarn abrasion resistance is 270 times, and the number of small braid yarn defects in 100,000 meters of yarn defects is 1.

[0166] Example 10

[0167] A composite yarn is formed by combining and twisting two core-wrapped yarns of Example 7 on a two-for-one twister.

[0168] The linear density of the composite yarn is 36.8tex, the breaking strength is 29.7cN / tex, the yarn abrasion resistance is 220 times, and the number of small braid yarn defects in 100,000 meters of yarn defects is 1.

[0169] Embodiment 11

[0170] A method for preparing a core-wrapped yarn is basically the same as that in Example 1, except that the low-melting-point fiber in Example 1 is replaced with conventional polyester staple fiber, the manufacturer of the conventional polyester staple fiber is Fujian Jinlun High Fiber Co., Ltd., and the specification is Jinlun 1.56dtex×38mm.

[0171] The final core-wrapped yarn has a linear density of 18.2tex, a breaking strength of 19.8cN / tex, a yarn abrasion resistance of 158, and 2 braid yarn defects per 100,000 meters.

[0172] In summary, the present invention performs a fixed length and shaping treatment on the filaments used as the core yarn to form a difference in heat shrinkage between the filaments and the outer layer of the filaments, and then performs a heat treatment on the spun core-wrapped yarn to increase the lateral bonding effect of the fibers in the yarn through the heat shrinkage of the outer layer of filaments; at the same time, the low-melting point fibers mixed in form a bonding effect between the fibers, and the combined effect of these two aspects achieves the effect of improving the strength of the core-wrapped yarn and reducing the slippage of the short fibers. The present invention is simple and easy to operate, green and environmentally friendly, and can improve the wear resistance of the core-wrapped yarn while ensuring good wearing comfort of the product.

Claims

1. A method for preparing a core-wrapped yarn, characterized in that: First, a yarn with a core-wrapped structure is prepared, with a filament I that has been heat-set to a fixed length as the core and a blended yarn of a short fiber and a low-melting-point fiber as the sheath, and the filament I is used as the core yarn, and the filament II is wrapped on the surface of the core-wrapped yarn to obtain the core-wrapped yarn, and then the core-wrapped yarn is heat-treated to obtain the core-wrapped yarn; The hot air shrinkage of the filament I after fixed-length heat setting is 5% to 30% less than that of the filament II. The temperature of the yarn heat treatment is both greater than the glass transition temperature of the filament II and higher than the melting point of the low-melting-point fiber, and less than 190°C. The short fiber content of the core-wrapped yarn is 45-68wt%, and the twist coefficient of the spun yarn is 300-360.

2. The method for preparing a core-wrapped yarn according to claim 1, characterized in that: Filament II is polyester filament, polyamide filament or polyolefin filament; filament I is polyester filament, polyamide filament or polyolefin filament; staple fiber is natural fiber and / or regenerated cellulose fiber; low melting point fiber is low melting point polyester fiber, low melting point polyamide fiber or low melting point PE fiber; the mass ratio of low melting point fiber to staple fiber is 1:5-20; the ratio of the mass of staple fiber to the total mass of filament II and filament I is 50:50-70:30; the mass ratio of filament II to filament I is 50:

50.

3. The method for preparing a core-wrapped yarn according to claim 1, characterized in that: The following steps are involved: (1) Raw material selection: short fibers, low melting point fibers, filament I, and filament II are selected as raw materials; (2) Fiber pretreatment and premixing: The short fibers are stored in a warehouse for curing and premixed with low melting point fibers; (3) Carding: The premixed fibers are further mixed and combed into strips through a carding machine; (4) Drawing: The slivers made by the carding machine are drawn through three drawing frames; (5) roving; the mixed sliver obtained in the drawing process is drawn and twisted to form roving; (6) Fiber length setting: The filament I is heat-set to a fixed length; (7) Spun yarn: After the filament I that has been heat-set to a certain length is used as the core yarn and is covered by the coarse yarn to form a core-wrapped structure, the filament II that has not been heat-set is used as the wrapping yarn and is intertwined with the core-wrapped structure to form a core-wrapped yarn; (8) Yarn heat treatment: The core-wrapped yarn is heat treated.

4. The method for preparing a core-wrapped yarn according to claim 3, characterized in that: In step (3), the carding machine has a sliver delivery speed of 100 to 110 m / min; in step (4), the first draw uses 6 mixed slivers for feeding, and the drafting multiple is 5.5 to 6.1 times; the second draw uses 6 mixed slivers for feeding, and the drafting multiple is 5.5 to 6.0 times; the third draw uses 5 mixed slivers for feeding, and the drafting multiple is 6.0 to 6.3, and the sliver delivery speed is 300 to 320 m / min; in step (5), the roving twist coefficient is not less than 110, and the roving elongation is controlled to be below 1.2%.

5. A core-wrapped yarn obtained by the method for preparing a core-wrapped yarn according to any one of claims 1 to 4, characterized in that: The invention is composed of a core yarn and a filament II which is wrapped around the core yarn and in a tightened state. The core yarn has a core-wrapped structure, with the filament I as the core and a blended yarn of short fibers and low-melting-point fibers as the sheath. The short fiber content of the core-wrapped yarn is 45-68wt%, and the twist coefficient of the spun yarn is 300-360.

6. A core-wrapped yarn according to claim 5, characterized in that: The low melting point fibers are bonded together with the other fibers in the core wrap yarn.

7. A core-wrapped yarn according to claim 6, characterized in that: Filament II is polyester filament, polyamide filament or polyolefin filament; Filament I is polyester filament, polyamide filament or polyolefin filament; Staple fiber is natural fiber and / or regenerated cellulose fiber; Low melting point fiber is low melting point polyester fiber, low melting point polyamide fiber or low melting point PE fiber.

8. A core-wrapped yarn according to claim 6 or 7, characterized in that: The mass ratio of the low melting point fiber to the short fiber is 1:5-20; the mass ratio of the short fiber to the total mass of the filament II and the filament I is 50:50-70:30; the mass ratio of the filament II to the filament I is 50:

50.

9. A composite yarn, characterized in that: The core-wrapped yarn is formed by merging and twisting two core-wrapped yarns, and the core-wrapped yarn is a core-wrapped yarn as described in any one of claims 5 to 8.