A layered nanostructured mineral material prepared by high-temperature sintering of antibiotic fermentation residue, and its preparation method and application

The preparation of layered nanostructured mineral materials by treating antibiotic fermentation bacteria residue powder through high-temperature sintering treatment, solves the problem of antibiotic fermentation bacteria residue treatment, achieves efficient adsorption and fixation of heavy metals, provides a new method for removing heavy metals in water and soil, and is excellent performance and application value.

CN116099488BActive Publication Date: 2024-11-26BIOGAS SCI RES INST MIN OF AGRI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111322769.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-09
Publication Date
2024-11-26
Estimated Expiration
2041-11-09

AI Technical Summary

Technical Problem

It is difficult to treat antibiotic fermentation bacterial residues, and it is difficult to achieve harmless and resource-based utilization. The existing physical and chemical treatment efficiency is unstable. The incineration method does not pay attention to mineral components and resource-based utilization potential, resulting in secondary pollution.

Method used

The antibiotic fermentation bacteria residue powder was processed by high temperature sintering (600-1200℃, 0.5-24 hours), and layered nanostructured mineral materials were prepared for adsorption and fixing heavy metals. The method was simple and no additional combustion aids and oxygen was required.

Benefits of technology

Obtain high-performance layered nanostructured mineral materials with excellent heavy metal capture capabilities, especially materials that are sintered for a long time at lower temperatures, showing excellent fixation and adsorption effects, providing a solution for removing heavy metals in water and soil , has broad application prospects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116099488B_ABST
    Figure CN116099488B_ABST
Patent Text Reader

Abstract

The present invention provides a layered nanostructured mineral material, which is a product obtained by sintering antibiotic fermentation residue at a high temperature of 600 to 1200°C for 0.5 to 24 hours, and has excellent absorption and fixation of heavy metals, and can be used for the removal and fixation of heavy metals in water or soil. The present invention provides a method for preparing the layered nanostructured mineral material by high-temperature sintering, which is simple and easy to implement, effectively realizes the harmlessness and high-value conversion and utilization of antibiotic residues, and has good economic benefits and promotion and application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of organic solid waste treatment, and specifically relates to a layered nanostructured mineral material prepared by high-temperature sintering of antibiotic fermentation residue, and a preparation method and application thereof. Background Art

[0002] China is the world's largest producer and exporter of antibiotic raw materials, producing more than 2 million tons of antibiotic fermentation residues each year. Antibiotic fermentation residues are composed of mycelial biomass, metabolites, fermentation substrates and residual antibiotics. Because of its high water content, easy corruption and excessive antibiotic residues, it is easy to pollute the environment. Since 2008, it has been included in China's national hazardous waste catalog. However, it is still rich in reusable resources, such as bacterial proteins and unused nutrients.

[0003] For a long time, many scholars have studied methods that can simultaneously achieve the harmlessness and resource reuse of antibiotic fermentation residues through biological treatment (such as anaerobic digestion and composting), thermal treatment (such as incineration, hydrothermal treatment, microwave heating and pyrolysis), and physical and chemical treatment (such as advanced oxidation, irradiation) and other technical means. However, biological treatment has a long reaction cycle, the abundance of resistance genes increases due to microbial metabolism during the fermentation process, and the subsequent waste residue is difficult to reprocess; physical and chemical treatment has defects such as unstable efficiency. High-temperature (about 1000℃) incineration is a simple operation that can effectively inactivate antibiotics and resistance genes, but the commonly used incineration method does not pay attention to the mineral composition and resource utilization potential of the incineration products, and directly discarding them in the environment will cause secondary pollution. How to achieve the harmlessness and reuse of antibiotic fermentation residues is a major difficulty in the resource treatment of antibiotic fermentation residues.

[0004] In recent years, heavy metal-contaminated wastewater discharged from industries such as electroplating, metallurgy, leather making and textile printing and dyeing, as well as agricultural waste containing heavy metals, have become important pollutants of the ecological environment and have caused great harm to human health directly or indirectly. Compared with traditional heavy metal ion removal methods, biosorption uses organisms and their derivatives for adsorption, which has a wide range of sources and shows great advantages in terms of raw material costs and environmental protection, and has received more attention; therefore, researchers have tried to use antibiotic residues for heavy metal adsorption, but found that their adsorption capacity is very limited. Although further physical and chemical modification methods are used to modify antibiotic fermentation residues to expose more active groups, which is conducive to improving the adsorption capacity of heavy metal ions, the steps are cumbersome and the adsorption amount still needs to be improved (Sun Xining. Modification of antibiotic residues and research on their heavy metal adsorption performance [D]. Northwest Agriculture and Forestry University, 2015.). Therefore, if a simple operation method for treating antibiotic fermentation residues can be studied to obtain products with excellent heavy metal adsorption and fixation capabilities, it will not only be beneficial to the reuse of antibiotic fermentation residues, but also provide a new option for the removal of heavy metals in water and soil, which will have very good economic benefits and application value. Summary of the invention

[0005] In order to solve the problem that antibiotic fermentation residue is difficult to handle and reuse, the present invention provides a layered nanostructured mineral material, which is a product obtained by high-temperature sintering of antibiotic fermentation residue powder, wherein the high-temperature sintering temperature is 600-1200°C and the high-temperature sintering time is 0.5-24h.

[0006] Furthermore, the high temperature sintering temperature is 600-800° C., and the high temperature sintering time is 2-24 hours.

[0007] Furthermore, the high temperature sintering temperature is 600° C., and the high temperature sintering time is 24 hours.

[0008] Preferably, the above-mentioned antibiotic fermentation residue powder is oxytetracycline fermentation residue powder and / or streptomycin fermentation residue powder.

[0009] The present invention also provides a method for preparing the above-mentioned layered nanostructured mineral material by high-temperature sintering of antibiotic fermentation residue, comprising the following steps:

[0010] The antibiotic fermentation residue powder is sintered at a high temperature of 600-1200°C for 0.5-24 hours to obtain the product.

[0011] Furthermore, the high temperature sintering is carried out under high temperature sintering conditions in an air atmosphere.

[0012] Furthermore, the high temperature sintering temperature is 600-800° C.; and / or the high temperature sintering time is 2-24 hours; preferably, the high temperature sintering temperature is 600° C., and the high temperature sintering time is 24 hours.

[0013] Preferably, the above-mentioned antibiotic fermentation residue powder is oxytetracycline fermentation residue powder and / or streptomycin fermentation residue powder.

[0014] The present invention also provides the use of the layered nanostructured mineral material for adsorbing, fixing or recovering heavy metals in water or soil.

[0015] Furthermore, the heavy metal is at least one of lead, copper and uranium.

[0016] The present invention provides a method for removing heavy metals from water, comprising the following steps:

[0017] (1) adding the above-mentioned layered nanostructured mineral material into water for adsorption;

[0018] (2) filtering to obtain a filtrate, which is water free of heavy metals;

[0019] The heavy metal is a heavy metal ion.

[0020] The present invention also provides a method for removing heavy metals in soil, comprising the following steps: adding the above-mentioned layered nanostructured mineral material into the soil for fixation; the heavy metals are heavy metal ions.

[0021] The "high temperature sintering" mentioned in the present invention is a process of heating powder or powder compact to form a dense structure.

[0022] Beneficial effects of the present invention:

[0023] 1. The present invention uses high-temperature treatment to harmlessly treat antibiotic fermentation residue while preparing high-performance layered nanostructured mineral materials, which are rich in calcium salts, calcium oxide and / or phosphates and can be used for the adsorption, fixation or recovery of various heavy metal pollutants.

[0024] 2. The layered nanostructured mineral material obtained by the present invention has excellent heavy metal capture ability and can remove heavy metals by sedimentation collection; in particular, the material obtained by high temperature sintering at a relatively low temperature (600°C) for a long time (24h) has a very excellent fixation / uranium removal effect and a high adsorption capacity;

[0025] 3. The high-temperature sintering process of the present invention does not require the addition of additional combustion aids and oxygen, and the preparation method and equipment are simple.

[0026] The invention has guiding significance for the harmless and resourceful treatment of antibiotic fermentation residues, and the obtained product has excellent performance and very broad application prospects.

[0027] Obviously, according to the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, other various forms of modification, replacement or change may be made.

[0028] The above contents of the present invention are further described in detail below through specific implementation methods in the form of embodiments. However, this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above contents of the present invention belong to the scope of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 : Scanning electron micrographs of mineral composite materials obtained by oxytetracycline fermentation strains under different temperature and time conditions. (a) Material obtained by high temperature treatment at 600°C for 2 hours (Example 1), (b) Material obtained by treatment at 600°C for 24 hours (Example 4), (c) Material obtained by treatment at 800°C for 2 hours (Example 2).

[0030] Figure 2 : Scanning electron microscope image of the mineral material (Example 7) obtained by sintering the streptomycin fermentation residue at 600°C for 2 hours.

[0031] Figure 3 : Energy spectra of mineral materials obtained from fermentation residues of two antibiotics and mineral materials obtained from rice straw.

[0032] Figure 4 : X-ray diffraction spectra of mineral composite materials obtained from oxytetracycline fermentation residue under different temperature and time conditions. (a) Material obtained by high temperature treatment at 600℃ for 2 hours, (b) Material obtained by treatment at 600℃ for 24 hours, (c) Material obtained by treatment at 800℃ for 2 hours.

[0033] Figure 5 :The removal effect of mineral materials obtained from oxytetracycline fermentation residue under different preparation conditions on uranium. "U(VI)removal" means "uranium removal rate", "U(VI)adsorption capacity" means "uranium adsorption capacity (mg uranium / g ash)", the number before "-" represents the treatment temperature, and the number after "-" represents the treatment time, such as "600-24" means "the burning temperature is 600℃ and the residence time is 24 hours.

[0034] Figure 6 : Adsorption kinetics (a) and adsorption isotherms (b) of uranium on mineral materials obtained from oxytetracycline fermentation residue under different temperature and time treatment conditions.

[0035] Figure 7: Comparison of uranium adsorption effects of mineral materials prepared from antibiotic fermentation residue and rice straw under different pH conditions. DETAILED DESCRIPTION

[0036] The raw materials and equipment used in the present invention are all known products, obtained by purchasing commercially available products. The antibiotic fermentation residue used in the present invention is provided by Hebei Shengxue Dacheng Pharmaceutical Co., Ltd.

[0037] Example 1: Preparation of layered nanostructured mineral material of the present invention

[0038] The oxytetracycline fermentation residue powder is placed in a muffle furnace and sintered at 600° C. for 2 hours in an air atmosphere to obtain the layered nanostructured mineral material of the present invention.

[0039] Example 2: Preparation of the layered nanostructured mineral material of the present invention

[0040] The oxytetracycline fermentation residue powder is placed in a muffle furnace and sintered at 800° C. for 2 hours in an air atmosphere to obtain the layered nanostructured mineral material of the present invention.

[0041] Example 3: Preparation of layered nanostructured mineral material of the present invention

[0042] The oxytetracycline fermentation residue powder is placed in a muffle furnace and sintered at 1000° C. for 0.5 hours in an air atmosphere to obtain the layered nanostructured mineral material of the present invention.

[0043] Example 4: Preparation of layered nanostructured mineral material of the present invention

[0044] The oxytetracycline fermentation residue powder is placed in a muffle furnace and sintered at 600° C. for 24 hours in an air atmosphere to obtain the layered nanostructured mineral material of the present invention.

[0045] Example 5: Preparation of layered nanostructured mineral material of the present invention

[0046] The oxytetracycline fermentation residue powder is placed in a muffle furnace and sintered at 800° C. for 12 hours in an air atmosphere to obtain the layered nanostructured mineral material of the present invention.

[0047] Example 6: Preparation of layered nanostructured mineral material of the present invention

[0048] The oxytetracycline fermentation residue powder is placed in a muffle furnace and sintered at 1200° C. for 2 hours in an air atmosphere to obtain the layered nanostructured mineral material of the present invention.

[0049] Example 7: Preparation of layered nanostructured mineral material of the present invention

[0050] The streptomycin fermentation residue powder is placed in a muffle furnace and sintered at 600° C. for 2 hours in an air atmosphere to obtain the layered nanostructured mineral material of the present invention.

[0051] Comparative Example 1: Preparation of materials obtained by burning rice straw

[0052] The rice straw powder is placed in a muffle furnace and sintered at 600° C. for 2 hours in an air atmosphere to obtain the layered nanostructured mineral material of the present invention.

[0053] The beneficial effects of the present invention are demonstrated by experimental examples below.

[0054] Experimental Example 1: Microscopic morphology of the layered nanostructured mineral material of the present invention

[0055] The materials obtained in Example 1, Example 2, Example 4 and Example 7 were observed under a scanning electron microscope. Figure 1 , Figure 2 shown.

[0056] Depend on Figure 1 It can be seen that the mineral material obtained by high-temperature incineration of oxytetracycline fermentation residue has a layered nanostructure and is rich in nano-flaky particles on the surface.

[0057] Depend on Figure 2 It can be seen that the mineral material obtained by high-temperature incineration of streptomycin fermentation residue still has a layered nanostructure, and the surface is also rich in nano-flaky particles.

[0058] The above results show that the antibiotic fermentation residue can be used to prepare a sheet-like nanomaterial through the incineration method of the present invention. The present invention provides a simple and efficient method for preparing a nanosheet material.

[0059] Experimental Example 2: Composition Analysis of the Layered Nanostructured Mineral Material of the Present Invention

[0060] The materials obtained in Example 1, Example 7 and Comparative Example 1 were subjected to EDS spectrum analysis. The results obtained are as follows: Figure 3 As shown in the figure, it can be seen that the mineral material obtained by high-temperature sintering of antibiotic fermentation residue contains more calcium and phosphorus than the product obtained by high-temperature sintering of rice straw. The materials obtained in Example 1, Example 2 and Example 4 were further subjected to X-ray diffraction test, and the obtained X-ray diffraction spectrum is as shown in Figure 4 As shown, it can be seen that the phase of the mineral material obtained by treating the oxytetracycline fermentation residue at 600°C for 2 hours is mainly calcium carbonate, and the phase of the mineral material obtained after the time is extended (24h) is converted from calcium carbonate to calcium oxide and hydroxyapatite; when the temperature is increased from 600°C to 800°C, the phase of the mineral material is mainly hydroxyapatite.

[0061] Experimental Example 3: Heavy metal removal effect of the layered nanostructured mineral material of the present invention

[0062] 1. Uranium removal efficiency of the mineral material of the present invention:

[0063] The layered nanostructured mineral materials (0.25 g / L) of Examples 1 to 6 were added to a solution with an initial uranium concentration of 50 mg / L, and the pH was not adjusted during the experiment. The suspension was placed at room temperature and shaken for 24 hours. The suspension after adsorption equilibrium was filtered with a 0.45 μm filter membrane, and the uranium content in the filtrate was determined. The amount of adsorbed uranium was calculated by subtracting the uranium content measured in the filtrate from the initial amount of uranium, and the amount was divided by the amount of the mineral material to obtain the uranium removal efficiency.

[0064] from Figure 5 It can be seen that the layered nanostructured mineral materials obtained in the embodiments of the present invention have a high removal performance for heavy metal uranium in water. When burned at a relatively low temperature (e.g., 600°C) for a long time (more than 2h) or at a relatively high temperature (e.g., 1000°C) for a short time (0.5h), the adsorption and removal effect of uranium is very excellent.

[0065] 2. Experimental analysis of adsorption kinetics and adsorption isotherms of the mineral materials of the present invention:

[0066] The layered nanostructured mineral materials of Example 1, Example 2, and Example 4 were subjected to adsorption kinetics experiments. The initial concentration of the kinetics experiment was 50 mg / L, the adsorbent concentration was 0.25 g / L, the initial pH was 5.0, and the adsorption operation process was referred to the above description. The uranium removal efficiency was measured and calculated at different time points within 24 hours. Figure 6 a It can be seen that the adsorption rate of uranium by the mineral materials obtained from oxytetracycline fermentation residue under different conditions is relatively fast, and the adsorption equilibrium can be reached within 2 hours;

[0067] The layered nanostructured mineral materials of Example 1, Example 2, and Example 4 were subjected to an adsorption isotherm experiment. The initial pH of the adsorption isotherm experiment was 5.0, the adsorbent concentration was 0.25 g / L, the initial uranium concentration was 0-300 mg / L, and the reaction time was 24 hours. The adsorption operation process was described above. Figure 6b It can be seen that at a lower uranium concentration, the adsorption capacity of sample 800-2 (Example 2) for uranium is higher, but with the increase of equilibrium concentration, the adsorption capacity of 800-2 for uranium does not increase, but the adsorption capacity of 600-2 (Example 1) and 600-24 (Example 4) for uranium gradually increases. The fitting results of the Langmuir model show that the maximum adsorption capacity of 600-24 (Example 4) for uranium can reach 695 mg / g, the maximum adsorption capacity of 600-2 (Example 1) for uranium can reach 309 mg / g, and the maximum adsorption capacity of 800-2 for uranium is only 141 mg / g (Table 1). It can be seen that, unlike the high temperature treatment (generally around 1000°C) used in traditional fungus slag incineration, the present invention proves that it is not that the higher the temperature is, the more conducive it is to prepare high-performance mineral adsorption materials, but that the longer treatment time at a lower temperature is conducive to obtaining high-performance mineral adsorption materials, which not only has a fast adsorption rate and a high maximum adsorption capacity, but also has an excellent heavy metal removal effect.

[0068] Table 1 The fitting results of the isothermal adsorption curve of uranium by mineral materials produced by oxytetracycline fermentation strains. The Langmuir model and Freundlich model were used to simulate the isothermal adsorption, where Q max Represents the maximum adsorption capacity

[0069]

[0070] 3. Effect of pH on the heavy metal removal effect of the mineral material of the present invention:

[0071] Under different pH conditions, the materials of Example 1, Example 7 and Comparative Example 1 were used to perform uranium removal experiments with reference to the adsorption operation described above, and the uranium removal efficiency was calculated. The results obtained are as follows: Figure 7 As shown. It can be seen that the mineral material obtained from the antibiotic bacterial residue of the present invention can efficiently adsorb uranium under various pH conditions, while the uranium adsorption capacity of the mineral material obtained by high-temperature sintering of rice straw is much weaker than that of the mineral material obtained by high-temperature sintering of the antibiotic fermentation bacterial residue of the present invention. The present invention treats the antibiotic bacterial residue by a high-temperature sintering method at a specific temperature and time to obtain a mineral material with a lamellar nanostructure, achieving a better heavy metal removal effect than other high-temperature sintering products such as rice straw.

[0072] In summary, the present invention provides a layered nanostructured mineral material, which is prepared by high-temperature sintering of antibiotic fermentation residue under specific conditions, and has excellent effects of adsorbing and fixing heavy metals; the method of the present invention is simple and easy to implement, realizes the reuse of antibiotic fermentation residue, and has good economic benefits and promotion and application value.

Claims

1. An application of a layered nanostructured mineral material in adsorbing, fixing or recovering heavy metals in water or soil, characterized in that: The layered nanostructured mineral material is a product obtained by high-temperature sintering of antibiotic fermentation residue powder, wherein the high-temperature sintering temperature is 600° C. and the high-temperature sintering time is 24 h. The high-temperature sintering is high-temperature sintering under air atmosphere conditions; the heavy metal is at least one of lead, copper and uranium; the layered nanostructured mineral material is mainly calcium oxide and hydroxyapatite; the antibiotic fermentation residue powder is oxytetracycline fermentation residue powder and / or streptomycin fermentation residue powder.

2. The use according to claim 1, characterized in that The steps include: (1) adding the layered nanostructured mineral material described in claim 1 to water for adsorption; (2) filtering to obtain a filtrate, which is water from which heavy metals have been removed.

3. The use according to claim 1, characterized in that The method comprises the following steps: adding the layered nanostructured mineral material described in claim 1 into the soil for fixation.