Lead-free solder alloy and tin spraying process thereof
By using a combination of lead-free solder alloy and specific flux, the problems of poor solder adhesion and contamination were solved, achieving uniform solder distribution and efficient production.
Patent Information
- Application Number
- CN202211557839.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-06
AI Technical Summary
In existing soldering processes, the adhesion between solder and printed circuit boards is poor, and the mixing of tin spraying material and copper remover can contaminate the solder, affecting solder quality. Suspended cooling increases floor space and reduces production efficiency.
It uses lead-free solder alloy containing appropriate amounts of copper, nickel, germanium and gallium, combined with specific proportions of flux (such as LCN-407, Dynol 604, CO 977) and solvent (ethylene glycol, acetone, butanediol), and controls the distribution of solder through the air knife system of the tin sprayer to improve the adhesion and uniformity of the solder.
It improves the adhesion between solder and printed circuit board, ensures uniform solder distribution, reduces flux contamination, and enhances solder quality and production efficiency.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a lead-free solder alloy and a tin spraying process thereof, in particular to the field of welding technology. Background Art
[0002] Printed circuit boards are important components of the electronics industry. From watches, mobile phones to computers, electronic communication equipment, and military weapons, printed circuit boards are indispensable. With the continuous advancement of technology, the size of electronic equipment is getting smaller and smaller, the circuit wiring density required is getting higher and higher, and the technical difficulty is getting greater and greater. Therefore, the soldering process of printed circuit boards requires more and more precise operations, and new requirements are put forward for the welding flatness and adhesion performance of printed circuit boards.
[0003] Chinese invention patent CN201811459393.7 discloses a PCB tin-spraying method for improving the surface smoothness of the tin-sprayed surface. By using a three-dimensional stirring method to effectively and fully mix the tin-spraying material and copper remover, the surface impurities of the PCB board are removed, the solderability of the PCB board is improved, and the surface smoothness of the board is improved. However, the adhesion performance between the solder and the PCB board is poor, and the mixing of the tin-spraying material and copper remover will contaminate the solder, affecting the soldering quality during long-term continuous operation. Chinese invention patent CN202111306901.X discloses a tin-spraying method for solving the warping problem of PCB boards. It adds suspension cooling to the PCB board after tin-spraying to reduce the problem of board warping caused by sudden temperature drops. However, suspension cooling increases the floor space and reduces production efficiency. Summary of the Invention
[0004] In order to improve the adhesion between the solder alloy and the printed circuit board and improve the flatness of the printed circuit board after tin spraying, the first aspect of the present invention provides a lead-free solder alloy. The raw materials for preparation include, by weight percentage, 0.05-0.09% copper, 0.05-0.3% nickel, 0.06-0.12% germanium, 0.0005-0.001% gallium, and tin makes up the balance.
[0005] As a preferred embodiment, the raw materials for preparation include, by weight percentage, 0.07% copper, 0.07-0.25% nickel, 0.09-0.11% germanium, 0.0006-0.009% gallium, and the balance is made up by tin.
[0006] As a preferred embodiment, the raw materials for preparation include, by weight percentage, 0.07% copper, 0.15% nickel, 0.1% germanium, 0.005% gallium, and the balance is made up by tin.
[0007] A second aspect of the present invention provides a process for tin-spraying using a lead-free solder alloy, comprising the following steps:
[0008] (1) Pickling, water washing and drying the printed circuit board;
[0009] (2) Immerse the dried printed circuit board in the flux tank for 1-3 seconds;
[0010] (3) The printed circuit board treated in step 2 is sprayed with lead-free solder alloy in a tin spraying machine. The tin bath temperature of the tin spraying machine is 250-270°C. The tin spraying machine is equipped with an air filter. It is necessary to evacuate the air before operation. The tin spraying machine removes excess tin through the air knife in the nozzle;
[0011] (4) Cool the printed circuit board after tin spraying, soak it in hot water and rinse it, then dry it.
[0012] As a preferred embodiment, the pickling in step 1 is hydrochloric acid pickling, and the mass fraction of hydrochloric acid is 8-15%.
[0013] As a preferred embodiment, the soldering flux comprises, by weight percentage, 2-3.5% of an acidic activator, 0.1-1% of a surfactant, 1-3% of a cosolvent, 0.1-0.3% of a film former, and the balance made up of water.
[0014] As a preferred embodiment, the acidic activator is selected from one or a combination of succinic acid, glutaric acid, itaconic acid, sebacic acid, pimelic acid, malic acid, and citric acid.
[0015] As a preferred embodiment, the acidic activator is a combination of succinic acid, sebacic acid and itaconic acid.
[0016] As a preferred embodiment, the weight ratio of succinic acid, glutaric acid and itaconic acid is 1: (1-3): (0.3-1.5).
[0017] As a preferred embodiment, the surfactant is a nonionic surfactant, and preferably, the nonionic surfactant is an aliphatic nonionic surfactant.
[0018] As a preferred embodiment, the aliphatic nonionic surfactant is selected from one or a combination of fatty alcohol polyoxyethylene ether, alkylphenol polyoxyethylene ether, fatty acid polyoxyethylene ether, alkyl polyoxyethylene ether, and polyoxyethylene alkylamide.
[0019] As a preferred embodiment, the surfactant is a combination of alkyl polyoxyethylene ether, polyol polyoxyethylene ether and alkylphenol polyoxyethylene ether.
[0020] As a preferred embodiment, the surfactant is a combination of LCN-407, Dynol 604, and CO 977.
[0021] As a preferred embodiment, the weight ratio of LCN-407, Dynol 604, and CO 977 is 1:1:(3-5).
[0022] As a preferred embodiment, the weight ratio of LCN-407, Dynol 604, and Igepal CO 977 is 1:1:4.
[0023] As a preferred embodiment, the co-solvent is selected from one or a combination of ethanol, propanol, butanol, acetone, toluene isobutyl ketone, ethyl acetate, and butyl acetate.
[0024] As a preferred embodiment, the co-solvent is a combination of ethylene glycol, acetone and butanediol.
[0025] As a preferred embodiment, the weight ratio of ethylene glycol, acetone and butanediol is 1: (0.3-0.5): (0.5-1.5).
[0026] As a preferred embodiment, the weight ratio of ethylene glycol, acetone and butanediol is 1:0.4:1.
[0027] As a preferred embodiment, the film-forming agent is polyvinyl alcohol JL-25E.
[0028] During experiments, the applicant discovered that adding the solvent to the flux improves the wettability of the tin alloy on the printed circuit board (PCB), increases the adhesion of the solder to the PCB, and evenly distributes the solder on the PCB, resulting in a uniformly thick and flat sheet. Furthermore, the flux used is an inorganic flux with good volatility. After immersion in the flux, the flux liquid is easily evaporated and removed, reducing contamination of the tin liquid in subsequent steps. During experiments, the applicant discovered that the synergistic effect of LCN-407, Dynol 604, and CO 977 can improve the flow and wettability of the solder alloy on the PCB, reduce the surface tension of the PCB, and enhance the compatibility between the PCB and the solder alloy. Furthermore, the synergistic effect of LCN-407, Dynol 604, and CO 977 results in low foaming properties. After immersion in the PCB, foam is less likely to adhere to the board surface, further improving the adhesion between the solder alloy and the PCB. The cosolvent is a combination of ethylene glycol, acetone, and butanediol. This combination of ethylene glycol, acetone, and butanediol increases the solubility of the flux, allowing it to spread evenly across the surface of the printed circuit board, improving the uniformity of the board surface treatment. Furthermore, the introduction of the cosolvent increases the volatility of the flux, allowing it to evaporate quickly after the board is removed from the flux tank, preventing the flux from entering the tin bath and contaminating the solder.
[0029] As a preferred embodiment, the air flow rate in the air filter is 1.9-4m 3 / min, and the temperature of the front and rear air knives in the nozzle is 310-330°C.
[0030] As a preferred embodiment, the temperature of the front and rear air knives in the nozzle is 320°C.
[0031] As a preferred embodiment, the air knife in the nozzle has a spacing of 0.25-0.3mm, the angle between the front air knife and the air knife is 1-3°, the spacing between the front air knife and the rear air knife is 12-30mm, the front air knife is 3-5mm higher than the rear air knife, and the air knife pressure is 2-6kg / cm 2 The front air knife has a pressure 0.1-0.5kg / cm2 less than the rear air knife. 2 .
[0032] Compared with the prior art, the present invention has the following effects:
[0033] (1) The lead-free solder alloy of the present invention does not contain lead. The synergistic effect of copper, nickel, germanium and gallium in a suitable weight ratio can assist tin metal in achieving good welding, avoid the participation of lead metal, and improve the safety of the processing process.
[0034] (2) The tin-spraying process of the lead-free solder alloy of the present invention increases the wetting effect of the solder on the printed circuit board, increases the spreading uniformity of the solder on the surface of the printed circuit board, and improves the adhesion between the solder and the printed circuit board by introducing LCN-407, Dynol604, and CO 977 into the flux.
[0035] (3) The lead-free solder alloy tin spraying process of the present invention improves the volatility of the flux by introducing a combination of ethylene glycol, acetone and butanediol into the flux, so that the printed circuit board can evaporate quickly after being soaked in the flux, thereby reducing the flux from being brought into the tin bath, contaminating the tin, and reducing the soldering quality of the printed circuit board during long-term continuous soldering. DETAILED DESCRIPTION
[0036] The present invention is described in detail below by way of examples. It is necessary to point out that the following examples are only used to further illustrate the present invention and are not to be construed as limiting the scope of protection of the present invention. Any non-essential improvements and adjustments made by professionals in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.
[0037] In addition, unless otherwise stated, all raw materials used were commercially available.
[0038] Example 1
[0039] A lead-free solder alloy is prepared from raw materials comprising, by weight percentage, 0.07% copper, 0.15% nickel, 0.1% germanium, 0.005% gallium, and the balance being made up of tin.
[0040] A process for tin spraying using a lead-free solder alloy comprises the following steps:
[0041] (1) Pickling, water washing and drying the printed circuit board;
[0042] (2) Immerse the dried printed circuit board in the flux tank for 2 seconds;
[0043] (3) The printed circuit board treated in step 2 is sprayed with lead-free solder alloy in a tin spraying machine. The tin bath temperature of the tin spraying machine is 260°C. The tin spraying machine is equipped with an air filter. It is necessary to evacuate the air before operation. The tin spraying machine removes excess tin through the air knife in the nozzle;
[0044] (4) Cool the printed circuit board after tin spraying, soak it in hot water and rinse it, then dry it.
[0045] The pickling in step 1 is carried out by performing hydrochloric acid pickling, and the mass fraction of hydrochloric acid is 10%.
[0046] The soldering flux comprises, by weight percentage, 2.8% of an acidic activator, 0.5% of a surfactant, 2% of a cosolvent, 0.2% of a film-forming agent, and the balance is made up of water.
[0047] The acidic activator is a combination of succinic acid, sebacic acid and itaconic acid in a weight ratio of 1:2:1.
[0048] The surfactant is a combination of LCN-407, Dynol 604, and Igepal CO 977 in a weight ratio of 1:1:4. The LCN-407 is purchased from Qingdao Hailan Chemical Technology Co., Ltd., the Dynol 604 is purchased from Evonik (Air Chemicals, USA), and the Igepal CO 977 is purchased from Solvay.
[0049] The cosolvent is a combination of ethylene glycol, acetone and butanediol in a weight ratio of 1:0.4:1.
[0050] The film-forming agent is polyvinyl alcohol JL-25E, purchased from JVP Co., Ltd. of Shin-Etsu Group of Japan.
[0051] The air flow rate in the air filter is 2.5m 3 / min, and the temperature of the front and rear air knives in the nozzle is 320℃.
[0052] The air knife in the nozzle has a spacing of 0.28mm, the angle between the front air knife and the air knife is 2°, the spacing between the front air knife and the rear air knife is 15mm, the front air knife is 4mm higher than the rear air knife, and the air knife pressure is 5kg / cm 2 The front air knife has a pressure 0.4kg / cm lower than the rear air knife. 2 .
[0053] Example 2
[0054] A lead-free solder alloy and a tin spraying process thereof, wherein the specific steps are the same as those in Example 1, except that the acidic activator is a combination of succinic acid, glutaric acid, and itaconic acid.
[0055] Example 3
[0056] A lead-free solder alloy and a tin spraying process thereof. The specific steps are the same as those in Example 1, except that the surfactant is a combination of PEG-400 and Dynol 604.
[0057] Example 4
[0058] A lead-free solder alloy and a tin spraying process thereof. The specific steps are the same as those in Example 1, except that the cosolvent is a combination of ethylene glycol, glycerol and butanediol.
[0059] Performance Testing
[0060] 1. Adhesion test: Test the thickness of the IMC layer after soldering, then place the solder layer in a 150°C environment for 538 hours and observe the thickness change of the IMC layer.
[0061] 2. Flatness test: A solder layer was obtained using the solder alloys and tin spraying processes of Examples 1-4, and the surface flatness of the solder layer was observed.
[0062] The test results are shown in Table 1.
[0063] Table 1
[0064]
Claims
1. A lead-free solder alloy, characterized in that: The raw materials for preparation include, by weight percentage: 0.07% copper, 0.07-0.25% nickel, 0.09-0.11% germanium, 0.0006-0.009% gallium, and the balance is made up by tin; The process of using the lead-free solder alloy to spray tin comprises the following steps: (1) Pickling, water washing and drying the printed circuit board; (2) Immerse the dried printed circuit board in the flux tank for 1-3 seconds; (3) The printed circuit board treated in step 2 is sprayed with lead-free solder alloy in a tin spraying machine. The tin bath temperature of the tin spraying machine is 250-270°C. The tin spraying machine is equipped with an air filter. It is necessary to evacuate the air before operation. The tin spraying machine removes excess tin through the air knife in the nozzle; (4) Cool the printed circuit board after tin spraying, rinse it with hot water, and then dry it; The soldering flux comprises, by weight percentage, 2-3.5% of an acidic activator, 0.1-1% of a surfactant, 1-3% of a cosolvent, 0.1-0.3% of a film former, and the balance is supplemented by water; The surfactant is a combination of LCN-407, Dynol 604, and CO 977 in a weight ratio of 1:1:(3-5); The acidic activator is a combination of succinic acid, sebacic acid and itaconic acid in a weight ratio of 1:(1-3):(0.3-1.5); The co-solvent is a combination of ethylene glycol, acetone and butanediol in a weight ratio of 1:(0.3-0.5):(0.5-1.5).
2. A process for tin spraying using the lead-free solder alloy according to claim 1, characterized in that: The following steps are involved: (1) Pickling, water washing and drying the printed circuit board; (2) Immerse the dried printed circuit board in the flux tank for 1-3 seconds; (3) The printed circuit board treated in step 2 is sprayed with lead-free solder alloy in a tin spraying machine. The tin bath temperature of the tin spraying machine is 250-270°C. The tin spraying machine is equipped with an air filter. It is necessary to evacuate the air before operation. The tin spraying machine removes excess tin through the air knife in the nozzle; (4) Cool the tin-sprayed printed circuit board, rinse it with hot water, and then dry it.
3. The process for tin-spraying the lead-free solder alloy according to claim 2, characterized in that: The pickling in step 1 is carried out by hydrochloric acid pickling, and the mass fraction of hydrochloric acid is 8-15%.
4. The process for tin-spraying the lead-free solder alloy according to claim 2, characterized in that: The air flow rate in the air filter is 1.9-4m 3 / min, and the temperature of the front and rear air knives in the nozzle is 310-330°C.
5. The process for tin-spraying the lead-free solder alloy according to claim 2, characterized in that: The air knife in the nozzle has a spacing of 0.25-0.3mm, the angle between the front air knife and the air knife is 1-3°, the spacing between the front air knife and the rear air knife is 12-30mm, the front air knife is 3-5mm higher than the rear air knife, and the air knife pressure is 2-6kg / cm 2 The front air knife has a pressure 0.1-0.5kg / cm lower than the rear air knife. 2 .