Titanium dioxide coated kaolin and its preparation method and application
Titanium dioxide is coated on kaolin by chemical deposition, and ethylene glycol or ethylenediamine is used as modifiers to solve the resource and cost of titanium dioxide, and achieve performance substitution and economic benefits. Suitable for coatings and papermaking industries.
Patent Information
- Application Number
- CN202211446270.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-11-18
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2042-11-18
AI Technical Summary
Existing titanium dioxide has many challenges in terms of resources, environment and cost, and no new inorganic substances can be found that can completely replace their properties, especially in terms of surface refractive index, hiding, tone and light stability, it is difficult to achieve the properties of natural crystalline TiO2. .
Chemical deposition method is used to use calcined kaolin and titanium dioxide as raw materials, and chemical grafting reaction is carried out through egregious acid, ethylene glycol or ethylenediamine as modifiers to form titanium dioxide coated kaolin, which meets the properties of whiteness and oil absorption. Indicators to reduce product costs.
It has realized the replacement of titanium dioxide, reduced production costs, and applied in coatings, papermaking and other industries, improving the performance and economic benefits of products.
Smart Images

Figure CN116102057B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of composite titanium dioxide, and more specifically to titanium dioxide coated kaolin and a preparation method and application thereof. Background Art
[0002] The main component of titanium dioxide is white metal titanium dioxide, which is recognized as one of the most widely used natural white metal oxides with excellent chemical structure and performance characteristics in nature. It is currently the white pigment with the best performance and the most stable structure in nature. It has three crystal forms in nature: rutile, anatase and brookite. The brookite type is unstable. Above 650°C, it will quickly decompose and turn into rutile. Anatase material can remain relatively stable at room temperature, but at high temperature, it is very likely to turn into rutile, and its stability and strength often depend on its calcination process conditions. Among these crystals, the rutile crystal form is the most stable and dense. At high temperatures, its hardness, density and refractive index are relatively high. Due to the high dielectric constant of titanium dioxide, it has high photoconductivity, good stability and good durability; however, since titanium dioxide has the conductivity of other high-temperature semiconductor materials, and at the same time, its own unique ultra-low conductivity can increase significantly with the continuous rise in the temperature of the surrounding air, at low temperatures, the oxygen-deficient discharge characteristics may also be particularly sensitive. Moreover, the titanium dioxide material itself is a low-conductivity material with good low-temperature thermal stability. Titanium dioxide has very stable electrochemical properties and is a slightly acidic amphoteric metal oxide. At room temperature, it is difficult to react with other inorganic elements and compounds. It has no direct effect on oxygen, hydrogen sulfide, carbon dioxide, and sulfur dioxide. It cannot be directly dissolved in aqueous electrolytes, and is completely insoluble in most dilute acid solutions and various inorganic acids and alkalis. It only dissolves in hydrofluoric acid. However, under the irradiation of ultraviolet light, the surface of titanium alloy can quickly undergo a series of stable photoredox reactions with multiple photochemical activities, especially under the irradiation of strong ultraviolet rays, and this is especially true for the synthesis of anatase titanium dioxide. This chemical property makes the titanium dioxide surface not only a catalyst for photosensitive oxidation, but also a preparation for some inorganic metal transition compounds.
[0003] At present, there are still serious bottleneck problems in the development of titanium dioxide and its production and the application and promotion of composite materials, such as resources, environment, demand growth and inverted resource cost prices, which are becoming increasingly prominent. Therefore, developing a composite material technology that can basically replace the original titanium dioxide production capacity or reduce the actual consumption level of existing TiO2 is undoubtedly an effective solution to these key problems.
[0004] So far, no new inorganic substance has been found in this research field that can have the same or infinitely close performance as natural crystalline TiO2 based on the determination of its surface refractive index, hiding power, hue and light stability, which are the most important measurement indicators. Therefore, titanium dioxide substitute materials are no longer composed of a single substance, but refer to a composite processing of this crystalline TiO2 compound and one or more other synthetic materials. The earliest titanium dioxide substitutes appeared earlier than the industrialization of titanium dioxide and the initial application of production technology. In 1912, the American "Titanium Pigment Company" discovered that a composite titanium dioxide composed of type A titanium dioxide containing only more than 25% chromium and other barium sulfate powder containing less than 75% chromium, which can be produced by sulfuric acid process, has a relatively high degree of optical hiding power and chemical stability. Before high-purity TiO2 pigments began to be widely used by humans in the early 20th century in Europe, it was considered to be a leading product in the pigment market.
[0005] With the progress of industrial technology and the rapid development of social economy, titanium dioxide products with a TiO2 content of more than 90% have been widely used, but the market has always paid attention to and expected low-priced titanium dioxide substitutes. Composite materials composed of composite particles with TiO2 as the surface layer of the particles and other inorganic materials as the core of the particles have the same or similar properties as TiO2, which can reduce the use of titanium dioxide, thereby reducing costs and maximizing benefits. Therefore, the present invention provides a new idea for preparing titanium dioxide coated kaolin to replace the original titanium dioxide. Summary of the invention
[0006] In view of the above problems, the present invention provides a titanium dioxide coated kaolin and a preparation method and application thereof, providing a new idea for replacing titanium dioxide.
[0007] The first object of the present invention is to provide a method for preparing titanium dioxide coated kaolin, which is prepared according to the following steps:
[0008] Step 1, calcined kaolin is added to water to prepare a slurry solution, heated to 80-90° C., and then an organic solution is added as a modifier to undergo an intercalation reaction to obtain a modified calcined kaolin solution;
[0009] Step 2: adding the titanium dioxide solution into the modified calcined kaolin solution and stirring until uniform coating is achieved, then aging the solution, washing the solution with water, drying the solution and calcining the solution to obtain the titanium dioxide coated kaolin.
[0010] Preferably, in step 1, the organic solution is one of ethylene glycol, oxalic acid and ethylenediamine.
[0011] Preferably, in step 1, the modifier solution obtained by diluting the organic solution is added to the slurry solution; wherein the volume ratio of the slurry solution to the modifier solution is 100:5-20, and the mass percentage ratio of the slurry solution to the modifier solution is 5%-20%:5%-7%; and the modification time is 30-40min.
[0012] Preferably, in step 2, the stirring time is 10-15 min.
[0013] Preferably, in step 2, the volume ratio of the modified calcined kaolin to the titanium dioxide solution is 5:1, and the mass percentage ratio of the modified calcined kaolin to the titanium dioxide solution is 5%-20%:3%.
[0014] Preferably, in step 2, the aging treatment is performed at 80-90° C. for 4-5 hours.
[0015] Preferably, in step 2, the calcination treatment is performed at 750-850° C. for 3-5 hours.
[0016] The second object of the present invention is to provide titanium dioxide coated kaolin prepared by the above preparation method.
[0017] The third object of the present invention is to provide the use of the above-mentioned titanium dioxide coated calcined kaolin in the preparation of coatings and papermaking.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention adopts a chemical deposition method, uses calcined kaolin and titanium dioxide as raw materials, uses oxalic acid, ethylene glycol or ethylenediamine as a modifier to modify the calcined kaolin, and a chemical grafting reaction occurs, so that the titanium dioxide is hydrolyzed on its surface and forms a uniform crystal coating, thereby preparing titanium dioxide coated kaolin. On the premise of meeting various performance indicators such as whiteness and oil absorption value, the amount of calcined kaolin is continuously increased to reduce the product cost;
[0020] The titanium dioxide-coated kaolin prepared by the invention can replace titanium dioxide, thereby reducing production costs and can be used in coating, papermaking, printing and other industries. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is the particle size distribution diagram of titanium dioxide;
[0022] Figure 2 is the particle size distribution diagram of calcined kaolin;
[0023] Figure 3 The performance of titanium dioxide coated kaolin prepared by different modifiers when the slurry solution is 5%, among which, Figure 3 a is the whiteness value, Figure 3 b is the oil absorption value;
[0024] Figure 4 The performance of titanium dioxide coated kaolin prepared by different modifiers when the slurry solution is 10%, among which, Figure 4 a is the whiteness value, Figure 4 b is the oil absorption value;
[0025] Figure 5 The performance of titanium dioxide coated kaolin prepared by different modifiers when the slurry solution is 15%, among which, Figure 5 a is the whiteness value, Figure 5 b is the oil absorption value;
[0026] Figure 6 The performance of titanium dioxide coated kaolin prepared by different modifiers when the slurry solution is 20%, among which, Figure 6 a is the whiteness value, Figure 6 b is the oil absorption value;
[0027] Figure 7 This is the XRD pattern of titanium dioxide coated kaolin prepared using oxalic acid as a modifier in Example 14;
[0028] Figure 8 This is the XRD pattern of titanium dioxide coated kaolin prepared using ethylene glycol as a modifier in Example 18;
[0029] Fig. 9 This is the XRD pattern of titanium dioxide coated kaolin prepared by using ethylenediamine as a modifier in Example 24; DETAILED DESCRIPTION
[0030] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] The calcined kaolin used in the present invention comes from Huairen, Shanxi Province, and the titanium dioxide is purchased from Henan Baililian New Materials Co., Ltd. and is prepared by the chlorination process. The particle size distribution of titanium dioxide and calcined kaolin is as follows: Figure 1-2 As shown by Figure 1 It can be seen that D10 = 0.099μm, D50 = 0.132μm, D90 = 0.175μm, and the particles with a particle size less than 0.175μm account for 90%, that is, the particle size of titanium dioxide is 0.175μm. Figure 2 It can be seen that D10 = 0.744 μm, D50 = 1.941 μm, D90 = 4.812 μm, and the particles with a particle size less than 0.175 μm account for 90%, that is, the particle size of calcined kaolin is 4.812 μm.
[0032] Test methods
[0033] (1) Take a certain amount of calcined kaolin, add water to make a suspension and stir it. At a certain temperature, prepare a certain concentration of organic modifier, then weigh a certain amount of modifier and add it to the calcined kaolin solution and control the temperature of the reaction process. Finally, add titanium salt solution with different percentages. After the reaction is completed, the product is dried, calcined, ground to a certain particle size, and then tested for whiteness, oil absorption value, etc. to find the best conditions.
[0034] (2) Under certain temperature conditions, calcined kaolin is treated with different modifiers, and then a certain amount of titanium salt solution is added and stirred continuously to explore the whiteness and oil absorption value, coating amount or coating rate, and find the optimal experimental conditions.
[0035] (3) According to the above test method, find out the best reaction conditions and influencing factors, perform image analysis, and determine the best conditions. Use UV XRD diffractometer to directly analyze the phase of the coated drug powder to detect the presence or morphology of titanium dioxide; use a desktop whiteness meter to measure the whiteness of the sample; use butyl phthalate to measure the oil absorption.
[0036] (1) Whiteness: Use a constant pressure powder forming machine to prepare finer coated samples, and then use a WSB-2 whiteness meter to measure the whiteness value of the samples. The greater the whiteness, the better the modified coating effect.
[0037] The whiteness determination method is as follows:
[0038] ①Preheating
[0039] Connect the power supply, press the power button behind the display, and wait for numbers to appear on the instrument display. The warm-up time is about 30 seconds.
[0040] ② Zero calibration
[0041] Place the black tube on the sample seat at the bottom of the instrument display screen. After the displayed value is basically stable, adjust the automatic zeroing display knob on the instrument panel so that the display value is 00.0.
[0042] ③Transfer the whiteness value of the working standard
[0043] Take out the black tube, put the working standard white plate on the sample holder, and after the digital display is completely stable, adjust the correction knob to make the value displayed on the digital display basically match the whiteness on the white plate, then remove the working white plate and put it on the reference standard white plate, and after the value displayed on the digital display is stable, you can record the whiteness. After that, it can be used as an important reference value for measuring and calibrating samples, and place the working standard white plate in a vacuum desiccator filled with silica gel medium liquid.
[0044] ④Calibration
[0045] Before each sample measurement, the standard black cylinder and the reference standard white plate should be adjusted and corrected respectively. These standard white plates have accurately transmitted the test results. If there are some continuous control samples that require high accuracy of the comparison data, then during the test, try to use the reference standard white plate for comparison and correction, so as to avoid repeated errors caused by changes in the display value of the instrument itself.
[0046] (2) Oil absorption rate: Weigh 1g of sample and place it on the glass base of the iron stand. Use a burette filled with dibutyl phthalate to titrate and measure the oil absorption rate of the sample. For inorganic fillers used in composite materials, the lower the oil absorption value, the easier it is to mix with the resin system or the filling ratio of the filler can be increased.
[0047] Oil absorption value determination
[0048] Weigh 1g of dry sample and place it on a clean and dry glass plate. Use an acid burette to evenly fill dibutyl phthalate and slowly and quantitatively add it dropwise into the dry sample container. At the same time, pay attention to stirring with a dry glass rod to make the dry sample quickly dissolve and mix with the free dibutyl phthalate mixture until it is uniform. When it is mixed into a mass and there is no small amount of free dry sample, it is determined as the titration end point.
[0049] Oil absorption rate calculation formula:
[0050] A=V / M(mL / g)
[0051] Where A—Oil absorption rate
[0052] V—Volume of dibutyl phthalate used
[0053] M—mass of the sample.
[0054] The specific embodiments are as follows.
[0055] Example 1
[0056] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 5 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0057] Example 2
[0058] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0059] Example 3
[0060] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0061] Example 4
[0062] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 20 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0063] Example 5
[0064] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 5 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0065] Example 6
[0066] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0067] Example 7
[0068] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0069] Example 8
[0070] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 20 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0071] Example 9
[0072] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 5 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0073] Example 10
[0074] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0075] Embodiment 11
[0076] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0077] Example 12
[0078] First, weigh the calcined kaolin, prepare 100 ml of 5% slurry solution with deionized water, heat it to 80°C, add 20 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0079] Depend on Figure 3 It can be seen that when the dosage of oxalic acid is 10mL, the modification coating effect is the best, the whiteness value is 92.2, and the oil absorption value is 40mL / 100g; when the dosage of ethylene glycol and ethylenediamine is 15mL, the whiteness values are 92.3 and 92.2 respectively, and the oil absorption values are both 35mL / 100g.
[0080] Embodiment 13
[0081] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 5 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0082] Embodiment 14
[0083] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0084] Embodiment 15
[0085] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0086] Example 16
[0087] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 20 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0088] Embodiment 17
[0089] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 5 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0090] Embodiment 18
[0091] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0092] Embodiment 19
[0093] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0094] Embodiment 20
[0095] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 20 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0096] Embodiment 21
[0097] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 5 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0098] Embodiment 22
[0099] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0100] Embodiment 23
[0101] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0102] Embodiment 24
[0103] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 80°C, add 20 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0104] Depend on Figure 4It can be seen that when the dosage of oxalic acid and ethylene glycol is 10mL, the modification and coating effect is the best, the whiteness value is 92.5, and the oil absorption value is 40mL / 100g; when the dosage of ethylenediamine is 20mL, the oil absorption value is 40mL / 100g.
[0105] Embodiment 25
[0106] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat to 80°C, add 5 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0107] Embodiment 26
[0108] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0109] Embodiment 27
[0110] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0111] Embodiment 28
[0112] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 20 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0113] Embodiment 29
[0114] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 5 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0115] Embodiment 30
[0116] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0117] Embodiment 31
[0118] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0119] Embodiment 32
[0120] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 20 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0121] Embodiment 33
[0122] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 5 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0123] Embodiment 34
[0124] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0125] Embodiment 35
[0126] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0127] Embodiment 36
[0128] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat to 80°C, add 20 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0129] Depend on Figure 5 It can be seen that when the dosage of the three modifying agents is 15mL, the modification effect is relatively good, the whiteness values are 92.4, 92.3 and 91.7 respectively, and the oil absorption values are 35mL / 100g, 35mL / 100g and 30mL / 100g respectively.
[0130] Embodiment 37
[0131] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat to 80°C, add 5 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0132] Embodiment 38
[0133] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0134] Embodiment 39
[0135] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0136] Embodiment 40
[0137] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat it to 80°C, add 20 ml of 5% oxalic acid modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0138] Embodiment 41
[0139] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat it to 80°C, add 5 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0140] Embodiment 42
[0141] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0142] Embodiment 43
[0143] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0144] Embodiment 44
[0145] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat to 80°C, add 20 ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0146] Embodiment 45
[0147] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat to 80°C, add 5 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0148] Embodiment 46
[0149] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat it to 80°C, add 10 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain a modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0150] Embodiment 47
[0151] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat it to 80°C, add 15 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0152] Embodiment 48
[0153] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat to 80°C, add 20 ml of 5% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 30 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0154] Depend on Figure 6 It can be seen that when the dosage of oxalic acid and ethylene glycol is 15mL, the modification effect is the best, the whiteness values are 92.5 and 92.4 respectively, and the oil absorption values are 40mL / 100g and 35mL / 100g respectively; when the dosage of ethylenediamine is 20mL, the whiteness value is 92.4 and the oil absorption value is 40mL / 100g.
[0155] Embodiment 49
[0156] First, weigh the calcined kaolin, prepare 100 ml of 10% slurry solution with deionized water, heat it to 90°C, add 15 ml of 6% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 40 minutes to obtain the modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 15 minutes until uniform coating, age at 90°C for 4 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 750°C for 5 hours. That is, titanium dioxide coated kaolin is obtained.
[0157] Embodiment 50
[0158] First, weigh the calcined kaolin, prepare 100 ml of 15% slurry solution with deionized water, heat to 85°C, add 20 ml of 7% ethylenediamine modifier solution while stirring, stir for 10 minutes, and modify for 35 minutes to obtain modified calcined kaolin solution; then add 20 ml of 3% titanium dioxide solution, stir continuously for 12 minutes until uniform coating, age at 85°C for 4.5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 850°C for 4 hours. That is, titanium dioxide coated kaolin is obtained.
[0159] Comparative Example 1
[0160] First, weigh the calcined kaolin, prepare 100 ml of 20% slurry solution with deionized water, heat it to 80°C, then add 20 ml of 3% titanium dioxide solution, stir continuously for 10 minutes until uniform coating, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is, titanium dioxide coated kaolin is obtained.
[0161] Table 1 Blank control test
[0162] Detection indicators Whiteness Oil absorption value (mL / 1g) Comparative Example 1 90.9 0.5
[0163] It can be seen from Table 1 that when the unmodified calcined kaolin is used as the matrix and directly coated, its whiteness value is 90.9 and its oil absorption value is 50 mL / 100 g.
[0164] Comparative Example 2
[0165] Prepare 20 ml of 5% oxalic acid modifier solution, add 20 g calcined kaolin and 3 g titanium dioxide at 80°C, stir to make it fully react so that it is uniformly adsorbed on the surface of the calcined kaolin matrix, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. The titanium dioxide coated kaolin is obtained.
[0166] Comparative Example 3
[0167] Prepare 20 ml of 5% ethylene glycol modifier solution, add 20 g calcined kaolin and 3 g titanium dioxide at 80°C, stir to make it fully react so that it is uniformly adsorbed on the surface of the calcined kaolin matrix, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is to obtain titanium dioxide coated kaolin.
[0168] Comparative Example 4
[0169] Prepare 20 ml of 5% ethylenediamine modifier solution, add 20 g calcined kaolin and 3 g titanium dioxide at 80°C, stir to make it fully react so that it is uniformly adsorbed on the surface of the calcined kaolin matrix, age at 80°C for 5 hours, then centrifuge and wash, dry at 200°C for 2 hours, and calcine at 800°C for 3 hours. That is to obtain titanium dioxide coated kaolin.
[0170] Table 2 Mechanochemical modification coating test
[0171] Whiteness Oil absorption value (mL / 1g) Oxalic acid 89.7 0.5 Ethylene glycol 89.0 0.45 Ethylenediamine 88.8 0.5
[0172] It can be concluded from Table 2 that in Comparative Examples 2-4, no matter which modifier is used, the titanium dioxide coated kaolin obtained by mechanochemical coating (dry method) has a low whiteness value of 89 on average, and a high oil absorption value.
[0173] Comparative Example 5
[0174] First, weigh the calcined kaolin, prepare a 20% ore pulp solution with deionized water, heat it to 80°C, add 5ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, modify it for 30 minutes, then add 20ml of 3% titanium sulfate solution, stir continuously for 10 minutes until it is evenly coated, age it at 80°C for 5 hours, then wash it with centrifugal water, dry it at 200°C for 2 hours, and calcine it at 800°C for 3 hours. That is, titanium sulfate solution-coated kaolin is obtained.
[0175] Comparative Example 6
[0176] First, weigh the calcined kaolin, prepare a 20% ore pulp solution with deionized water, heat it to 80°C, add 10ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, modify it for 30 minutes, then add 20ml of 3% titanium sulfate solution, stir continuously for 10 minutes until it is evenly coated, age it at 80°C for 5 hours, then wash it with centrifugal water, dry it at 200°C for 2 hours, and calcine it at 800°C for 3 hours. That is, titanium sulfate solution-coated kaolin is obtained.
[0177] Comparative Example 7
[0178] First, weigh the calcined kaolin, prepare a 20% ore pulp solution with deionized water, heat it to 80°C, add 15ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, modify it for 30 minutes, then add 20ml of 3% titanium sulfate solution, stir continuously for 10 minutes until it is evenly coated, age it at 80°C for 5 hours, then wash it with centrifugal water, dry it at 200°C for 2 hours, and calcine it at 800°C for 3 hours. That is, titanium sulfate solution-coated kaolin is obtained.
[0179] Comparative Example 8
[0180] First, weigh the calcined kaolin, prepare a 20% ore slurry solution with deionized water, heat it to 80°C, add 20ml of 5% ethylene glycol modifier solution while stirring, stir for 10 minutes, modify it for 30 minutes, then add 20ml of 5% titanium sulfate solution, stir continuously for 10 minutes until it is evenly coated, age it at 80°C for 5 hours, then wash it with centrifugal water, dry it at 200°C for 2 hours, and calcine it at 800°C for 3 hours. That is, titanium sulfate solution-coated kaolin is obtained.
[0181] Table 3 Titanium sulfate solution coating test
[0182] Modifier (ethylene glycol / mL) 5 10 15 20 Whiteness 89.7 88.0 89.9 91.1 Oil absorption value 0.4 0.45 0.4 0.4
[0183] As shown in Table 3, in Comparative Examples 5-8, using different volumes of ethylene glycol as a modifier to treat calcined kaolin has little effect on the whiteness of the composite material, and the oil absorption value remains basically stable. That is, there is a problem of low whiteness value and high oil absorption value.
[0184] Figure 7-9 The XRD patterns of the titanium dioxide-coated kaolin prepared in Example 14, Example 18 and Example 24 are shown in FIG. Figure 7 It can be seen that the main components of the composite material prepared in Example 14 are andalusite Al2(SiO4)O, Ti4FeH 8.5 , Figure 8 It can be seen that the main component of the composite material prepared in Example 18 is Al2 (Al 2.8 Si 1.2 ) 9.6 、(FeO) 0.198 (MnO) 0.802 , Fig. 9 It can be seen that the main components of the composite material prepared in Example 24 are andalusite and saltpeter.
[0185] Although the preferred embodiments of the present invention have been described, those skilled in the art may make other changes and modifications to these embodiments once they have learned the basic creative concept. Therefore, the appended claims are intended to be interpreted as including the preferred embodiments and all changes and modifications that fall within the scope of the present invention.
[0186] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.
Claims
1. Preparation method of titanium dioxide coated kaolin, It is characterized in that Prepare according to the following steps: Step 1, calcined kaolin is added to water to prepare a slurry solution, and after heating to 80-90° C., a modifier solution obtained by diluting an organic solution is added to the slurry solution to cause an intercalation reaction to obtain a modified calcined kaolin solution; The organic solvent is one of ethylene glycol, oxalic acid and ethylenediamine; The volume ratio of the slurry solution to the modifier solution is 100:5-20, the mass percentage ratio of the slurry solution to the modifier solution is 5%-20%:5%-7%; the modification time is 30-40min; Step 2: Add the titanium dioxide solution to the modified calcined kaolin solution and stir until uniformly coated, then age at 80-90° C. for 4-5 hours, wash with water, dry and calcine to obtain titanium dioxide coated kaolin; the volume ratio of the modified calcined kaolin solution to the titanium dioxide solution is 5:1, and the mass percentage ratio of the modified calcined kaolin solution to the titanium dioxide solution is 5%-20%:3%.
2. The method for preparing titanium dioxide coated kaolin according to claim 1, It is characterized in that In step 2, the stirring time is 10-15 minutes.
3. The method for preparing titanium dioxide coated kaolin according to claim 1, It is characterized in that In step 2, the calcination treatment is performed at 750-850° C. for 3-5 hours.
4. A titanium dioxide-coated kaolin prepared by the preparation method according to any one of claims 1 to 3.
5. Use of the titanium dioxide coated kaolin according to claim 4 in the preparation of coatings and papermaking.