A method for preparing positive electrode material by regenerating waste sodium ion batteries

By separating the nickel-ferromanganese solution by using carbon thermal reduction and water-immersion-acid leaching method in sodium ion battery recycling, and sintering with sodium carbonate, high-performance positive electrode material is prepared, which solves the problem of large energy consumption, long cycle and The problem of secondary pollution has achieved green and efficient recycling and excellent electrochemical performance of positive electrode materials.

CN116102080BActive Publication Date: 2024-11-26GUANGZHOU UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211636592.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-20
Publication Date
2024-11-26
Estimated Expiration
2042-12-20

AI Technical Summary

Technical Problem

The prior art has problems such as large energy consumption of pyrometallurgy, long biometallurgy cycle and secondary pollution of wet metallurgy in the recovery of sodium ion batteries, resulting in a great impact on recycling efficiency and environmental.

Method used

The high-purity nickel-ferromanganese solution was separated by carbon-thermal reduction treatment and water-immersion-acid leaching method of waste sodium ion batteries. By sintering the precursor and sodium carbonate, NaNi0.4Fe0.2Mn0.4O2 with excellent electrochemical performance was prepared. Positive electrode material, achieve green recycling.

Benefits of technology

This method achieves efficient recycling of used sodium ion batteries, reduces secondary pollution, is simple to operate, is suitable for large-scale industrial promotion, and the generated positive electrode material has good electrochemical performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116102080B_ABST
    Figure CN116102080B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of resource utilization of solid waste, and discloses a method for preparing positive electrode materials by regenerating waste sodium ion batteries, wherein waste positive electrode materials and negative electrode materials are subjected to carbon thermal reduction treatment, sodium is separated from metal by water leaching, sodium in the leaching solution is evaporated and crystallized to obtain sodium carbonate, metal leaching residue after water leaching is separated by acid leaching to obtain high-purity nickel-manganese-iron solution and leaching residue, a precursor is prepared by using the nickel-manganese-iron solution, and the precursor is mixed with sodium carbonate and sintered in a muffle furnace to obtain NaNi with excellent electrochemical performance. 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material. This scheme is applicable to general waste sodium ion batteries, making full use of the components in waste sodium ion batteries, and using nickel-manganese-iron solution to regenerate NaNi with good electrochemical performance 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material achieves green recycling, is easy to operate, has low equipment requirements, and can be promoted on a large scale in industrialization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste resource utilization, and in particular to a method for preparing positive electrode materials by regenerating waste sodium ion batteries. Background Art

[0002] In recent years, sodium-ion batteries have attracted widespread attention from countries around the world as a new type of energy storage device. Due to the widespread distribution of sodium resources around the world, sodium-ion batteries have become an important energy storage device to assist lithium-ion batteries. Considering that the abundant sodium resources in the world can significantly reduce the cost of sodium-ion batteries, many companies have begun to produce and apply sodium-ion batteries. Like lithium-ion batteries, sodium-ion batteries also have a certain service life. When sodium-ion batteries are scrapped, the used sodium-ion batteries contain a large amount of valuable substances, such as sodium, manganese, nickel, cobalt, etc. If they are not handled properly, they will have a serious impact on the environment. Therefore, recycling them can not only prevent them from causing damage to the environment, but also recycle the valuable substances inside them.

[0003] At present, the recycling methods of waste sodium-ion batteries are mainly divided into pyrometallurgy, hydrometallurgy and biometallurgy. Pyrometallurgy has strong adaptability to raw materials and rapid reaction, but it consumes a lot of energy and produces toxic gases. The bacteria required for biometallurgy have high environmental requirements and a long metal extraction cycle, which is rarely mentioned in general industry. Hydrometallurgy has attracted widespread attention due to its advantages such as mild conditions, low energy consumption and high selectivity for metals, such as organic or inorganic reduction acid leaching and reduction ammonia leaching, but the secondary pollution caused has become its biggest application barrier. Therefore, it is particularly important to reduce the problem of secondary pollution in hydrometallurgy. Based on this, the pyrometallurgical roasting-hydrometallurgy combined method is selected as a breakthrough point, which can not only achieve the purpose of alleviating the secondary pollution problem caused by hydrometallurgy, but also realize the preferential extraction of Li and the transformation between valuable metal structures. For this reason, we propose a method for preparing positive electrode materials by regenerating waste sodium-ion batteries. Summary of the invention

[0004] 1. Technical issues to be solved

[0005] In view of the shortcomings of the prior art, the present invention provides a method for preparing positive electrode materials by regenerating waste sodium ion batteries, which comprises the following steps: using waste positive electrode materials and negative electrode materials for carbon thermal reduction treatment, separating sodium from metal by water leaching, evaporating and crystallizing the sodium in the leaching solution to obtain sodium carbonate, using acid leaching to separate high-purity nickel-manganese-iron solution and leaching residue from the metal leaching residue after water leaching, using the nickel-manganese-iron solution to prepare a precursor, and then mixing the precursor with sodium carbonate and sintering in a muffle furnace to obtain NaNi with excellent electrochemical performance. 0.4 Fe 0.2 Mn 0.4O2 positive electrode material, this scheme is suitable for general waste sodium ion batteries, making full use of the components in waste sodium ion batteries, and using nickel manganese iron solution to regenerate NaNi with good electrochemical performance 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material achieves green recycling, is easy to operate, has low equipment requirements, and can be promoted on a large scale in industrialization.

[0006] (II) Technical solution

[0007] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a method for preparing positive electrode materials by regenerating waste sodium ion batteries, comprising the following steps:

[0008] Step 1: Use the waste NaNi x Mn 1-x O2、NaNi x Mn y Fe z The waste positive electrode NaNi was obtained after O2 battery discharge, splitting and organic solvent dissolution x Mn 1-x O2 and NaNi x Mn y Fe z O2 mixed powder and negative electrode powder, the above two powders are ball-milled and mechanically mixed and then carbon thermal reduction treatment is performed, the mass ratio of waste positive electrode powder and negative electrode powder is 3-12:1, and the ball milling time is 3-9h;

[0009] Step 2: water leaching, carbon thermal reduction and powder, separation of leaching solution and leaching residue after leaching, evaporation, concentration and crystallization of the leaching solution to obtain sodium carbonate product;

[0010] The third step: using acid leaching to separate the leached residue after water leaching, separating the leached solution and the leached residue after acid leaching to obtain the leached solution and leached residue rich in high-purity valuable metal nickel, manganese and iron;

[0011] Step 4: Add acetate of Ni, Mn and Fe to the leaching solution to adjust Ni 2+ , Fe 3+ , Mn 2+ The molar ratio of 4:2:4 was set, and a precipitant was added, the pH was kept between 10.4 and 10.6, stirring and heating were maintained, and the mixture was aged for 24 hours. After the reaction, the mixture was filtered and washed several times, and then dried in a drying oven at 90°C to obtain Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 Precursor;

[0012] Step 5: Sodium carbonate and Ni 0.4 Fe 0.2 Mn0.4 (OH) 0.2 The precursors are ball-milled and mixed uniformly, and sintered in a muffle furnace to obtain NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material.

[0013] Preferably, the organic solvent in the first step is NMP, and the dissolution temperature is 70-90°C;

[0014] The mass ratio of waste positive electrode powder to negative electrode powder is 5-10:1, the roasting temperature is 500-800°C, and the roasting time is 2-5h.

[0015] Preferably, the carbon thermal reducing agent for the carbon thermal reduction treatment in the first step is waste negative electrode graphite, and the waste negative electrode graphite is directly recovered and reduced and roasted to reduce the waste positive electrode material, which is in line with the concept of green environmental protection;

[0016] The mass fraction of the waste negative electrode graphite is 10-20%, so as to facilitate reduction roasting to obtain metal and metal oxide;

[0017] The mass fraction of waste negative electrode graphite is 10, 12, 14, 16, 18, and 20%;

[0018] When the mass fraction of waste negative electrode graphite is lower than 10%, the waste positive electrode material cannot be fully calcined, resulting in part of the positive electrode material not being reduced. When the mass fraction of waste negative electrode graphite is higher than 20%, there is still graphite residue after carbon thermal reduction calcination, which is not conducive to subsequent water leaching and acid leaching.

[0019] Preferably, in the second step, the water immersion solid-liquid ratio is 5-20 g / L, the time is 1-3 h, and the leaching solution and leaching residue are separated after water immersion. The water immersion step is repeated 3-5 times, and the evaporation crystallization temperature is 70-90 ° C.

[0020] Evaporation at 70-90°C is beneficial to obtain sodium carbonate, which can be used to prepare NaNi by subsequent calcination. 0.4 Fe 0.2 Mn 0.4 O2 positive electrode.

[0021] Preferably, the acid in the third step is any one of acetic acid, citric acid, malic acid, succinic acid, ascorbic acid, aspartic acid, oxalic acid, tartaric acid, maleic acid or lactic acid, and the concentration is 2-5 mol / L;

[0022] Liquid-to-solid ratio is 5-10ml / g;

[0023] The acid leaching temperature is 50-90°C and the reaction time is 3-6h.

[0024] Preferably, in the fourth step, the precipitant is a mixture of NaOH solution and ammonia water, and the volume ratio of NaOH solution to ammonia water is 7:3.

[0025] Preferably, in the fifth step, the sintering temperature is 400-1000° C. and the sintering time is 16-20 hours.

[0026] (III) Beneficial effects

[0027] Compared with the prior art, the present invention provides a method for preparing positive electrode materials by regenerating waste sodium ion batteries, which has the following beneficial effects:

[0028] The method for preparing positive electrode materials by regenerating waste sodium ion batteries is applicable to general waste sodium ion batteries, fully utilizing the components in waste sodium ion batteries, and utilizing nickel-manganese-iron solution to regenerate NaNi with good electrochemical performance. 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material achieves green recycling, is easy to operate, has low equipment requirements, and can be promoted on a large scale in industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The NaNi prepared in Example 1 0.4 Fe 0.2 Mn 0.4 XRD pattern of O2;

[0030] Figure 2 The NaNi prepared in Example 1 0.4 Fe 0.2 Mn 0.4 SEM image of O2;

[0031] Figure 3 The NaNi of Examples 1-3 and Comparative Examples 0.4 Fe 0.2 Mn 0.4 Rate performance diagram of O2;

[0032] Figure 4 The NaNi of Examples 1-3 and Comparative Examples 0.4 Fe 0.2 Mn 0.4 Cycle life diagram of O2. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] Example 1

[0035] This embodiment provides a NaNi 0.4 Fe 0.2 Mn 0.4 The O2 positive electrode material is prepared according to the following steps:

[0036] (1) Carbon thermal reduction of waste sodium ion battery positive electrode materials: 16 g of waste positive electrode powder and 4 g of waste negative electrode graphite were placed in a ball mill and ball milled at 500 rpm for 3 h. The uniformly mixed powder was placed in a tube furnace and calcined at 650 °C for 2 h in a N2 atmosphere.

[0037] (2) Extraction of nickel-manganese iron: The powder after carbon thermal reduction is in the shape of bricks. Grind it into powder first. Take 10g of the powder after carbon thermal reduction and add it to a beaker containing 500ml of deionized water. The flow rate of carbon dioxide is 30ml / min. Bubble for 2h. After filtering, evaporate the water in the filtrate at 80℃ in a forced air drying oven to obtain sodium carbonate. The filter residue is dried at 120℃ in a vacuum drying oven. Dissolve 5g of the filter residue in 40ml of 3.5mol / L malic acid solution, stir at 85℃ and 400rmp for 3h, and centrifuge to obtain the supernatant.

[0038] (3) Preparation of Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 Precursor: Weigh appropriate amounts of nickel acetate, manganese acetate and iron acetate to prepare an acetate solution. Mix the supernatant and the acetate solution to form solution A. Mix 10 mol / L NaOH solution and 0.2 mol / L ammonia water to form solution B (V NaOH溶液 :V 氨水 =7:3), add 400ml of deionized water to the beaker, then add ammonia water to make the pH value of the bottom liquid reach about 11.0, keep the temperature at 50°C, use a peristaltic pump to add solution A to the bottom liquid, the feeding rate is 100ml / h, and add solution B to control the pH of the system between 10.4-10.6. After the injection of solution A, maintain the pH value, continue heating and stirring, and age for 24h. After the aging is completed, the filter residue obtained by suction filtration and washing is placed in a blast drying oven at 90°C for drying.

[0039] (4) Preparation of NaNi0.4 Fe 0.2 Mn 0.4 O2 positive electrode material: Sodium carbonate and Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 The precursors were ball-milled and mixed uniformly, wherein the molar ratio was Na:M=1.05 (M=Ni, Mn, Fe), heated to 450°C in a muffle furnace and kept for 5 h, then heated to 900°C and kept for 15 h, and cooled to room temperature to obtain NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material.

[0040] Example 2

[0041] (1) Carbon thermal reduction of waste sodium ion battery positive electrode materials: 16 g of waste positive electrode powder and 4 g of waste negative electrode graphite were placed in a ball mill and ball milled at 500 rpm for 3 h. The uniformly mixed powder was placed in a tube furnace and calcined at 600 °C for 2 h in a N2 atmosphere.

[0042] (2) Extraction of nickel-manganese iron: The powder after carbon thermal reduction is in the shape of bricks. Grind it into powder first. Take 10g of the powder after carbon thermal reduction and add it to a beaker containing 500ml of deionized water. The flow rate of carbon dioxide is 30ml / min. Bubble for 2h. After filtering, evaporate the water in the filtrate at 80℃ in a forced air drying oven to obtain sodium carbonate. The filter residue is dried at 120℃ in a vacuum drying oven. Dissolve 5g of the filter residue in 40ml of 3mol / L citric acid solution, stir at 90℃ and 400rmp for 3h, and centrifuge to obtain the supernatant.

[0043] (3) Preparation of Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 Precursor: Weigh appropriate amounts of nickel acetate, manganese acetate and iron acetate to prepare an acetate solution. Mix the supernatant and the acetate solution to form solution A. Mix 10 mol / L NaOH solution and 0.2 mol / L ammonia water to form solution B (V NaOH溶液 :V 氨水 =7:3), add 400ml of deionized water to the beaker, then add ammonia water to make the pH value of the bottom liquid reach about 11.0, keep the temperature at 50°C, use a peristaltic pump to add solution A to the bottom liquid, the feeding rate is 100ml / h, and add solution B to control the pH of the system between 10.4-10.6. After the injection of solution A, maintain the pH value, continue heating and stirring, and age for 18h. After the aging is completed, the filter residue obtained by suction filtration and washing is placed in a blast drying oven at 90°C for drying.

[0044] (4) Preparation of NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material: Sodium carbonate and Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 The precursors were ball-milled and mixed uniformly, wherein the molar ratio was Na:M=1.1 (M=Ni, Mn, Fe), heated to 450°C in a muffle furnace and kept for 5 h, then heated to 850°C and kept for 15 h, and cooled to room temperature to obtain NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material.

[0045] Example 3

[0046] (1) Carbon thermal reduction of waste sodium ion battery positive electrode materials: 16 g of waste positive electrode powder and 4 g of waste negative electrode graphite were placed in a ball mill and ball milled at 500 rpm for 3 h. The uniformly mixed powder was placed in a tube furnace and calcined at 800 °C for 2 h in a N2 atmosphere.

[0047] (2) Extraction of nickel-manganese iron: The powder after carbon thermal reduction is in the shape of bricks. Grind it into powder first. Take 10g of the powder after carbon thermal reduction and add it to a beaker containing 500ml of deionized water. The flow rate of carbon dioxide is 30ml / min. Bubble for 2h. After filtering, evaporate the water in the filtrate at 80℃ in a forced air drying oven to obtain sodium carbonate. The filter residue is dried at 120℃ in a vacuum drying oven. Dissolve 5g of the filter residue in 40ml of 3.5mol / L malic acid solution, stir at 90℃ and 400rmp for 3h, and centrifuge to obtain the supernatant.

[0048] (3) Preparation of Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 Precursor: Weigh appropriate amounts of nickel acetate, manganese acetate and iron acetate to prepare an acetate solution. Mix the supernatant and the acetate solution to form solution A. Mix 10 mol / L NaOH solution and 0.2 mol / L ammonia water to form solution B (V NaOH溶液 :V 氨水 =7:3), add 400ml of deionized water to the beaker, then add ammonia water to make the pH value of the bottom liquid reach about 11.0, keep the temperature at 70°C, use a peristaltic pump to add solution A to the bottom liquid, the feeding rate is 100ml / h, and add solution B to control the pH of the system between 10.4-10.6. After the injection of solution A, maintain the pH value, continue heating and stirring, and age for 12h. After the aging is completed, the filter residue obtained by suction filtration and washing is placed in a blast drying oven at 90°C for drying.

[0049] (4) Preparation of NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material: Sodium carbonate and Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 The precursors were ball-milled and mixed uniformly, wherein the molar ratio was Na:M=1.1 (M=Ni, Mn, Fe), heated to 450°C in a muffle furnace and kept for 5 h, then heated to 800°C and kept for 15 h, and cooled to room temperature to obtain NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material.

[0050] Comparative Example

[0051] This comparative example provides a NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material, the preparation method is as follows:

[0052] Prepare a sulfate solution A with a molar ratio of Ni:Fe:Mn=4:2:4, mix 10 mol / L NaOH solution and 0.2 mol / L ammonia water to form a solution B (V NaOH溶液 :V 氨水 =7:3), add 400ml of deionized water to the beaker, then add ammonia water to make the pH value of the bottom liquid reach about 11.0, keep the temperature at 70°C, use a peristaltic pump to add solution A to the bottom liquid, the feeding rate is 100ml / h, and add solution B to control the pH of the system between 10.4-10.6. After the injection of solution A, maintain the pH value, continue heating and stirring, and age for 24h. After the aging is completed, the filter residue obtained by suction filtration and washing is placed in a blast drying oven at 90°C for drying.

[0053] Sodium carbonate and Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 The precursors were ball-milled and mixed uniformly, wherein the molar ratio was Na:M=1.1 (M=Ni, Mn, Fe), heated to 450°C in a muffle furnace and kept for 5 h, then heated to 900°C and kept for 15 h, and cooled to room temperature to obtain NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material.

[0054] Test Example 1

[0055] The NaNi prepared in Example 1 0.4 Fe 0.2Mn 0.4 The O2 cathode material was subjected to XRD testing, and the results were as follows Figure 1 As shown. Figure 1 It can be seen that the sample of Example 1 has good crystallinity, and the diffraction peaks are basically consistent with the standard card, among which the main diffraction peaks are consistent with the NaNi 0.4 Fe 0.2 Mn 0.4 O2 corresponds to (space group PDF#00-053-0349), indicating the successful synthesis of NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material.

[0056] Test Example 2

[0057] The NaNi prepared in Example 1 0.4 Fe 0.2 Mn 0.4 The O2 cathode material was tested by SEM, and the results are as follows Figure 2 As shown. Figure 2 It can be seen that the sample of Example 1 is composed of irregular particles and has good crystallinity.

[0058] Test Example 3

[0059] The NaNi provided in Examples 1-3 0.4 Fe 0.2 Mn 0.4 O2 and NaNi provided by the comparative example 0.4 Fe 0.2 Mn 0.4 O2 was used as the positive electrode material to prepare sodium ion batteries.

[0060] The specific assembly process is as follows:

[0061] Preparation of positive electrode sheet: 160 mg of positive electrode material, 20 mg of superP (conductive agent) and 20 mg of PVDF (binder) were weighed and put into an agate mortar. After hand grinding with an agate mortar rod for 10 minutes, NMP was added and grinding continued for 10 minutes to form a uniformly mixed slurry. Subsequently, the uniformly mixed slurry was coated on aluminum foil with a 50 μm film puller and placed in a vacuum drying oven at 70 ° C for vacuum drying. The dried material was cut into 12 mm diameter discs with a slicer, weighed and placed in a sealed bag for later use.

[0062] Sodium-ion battery assembly:

[0063] First, ensure that the materials required for battery assembly are dry, open the enclosed space in the tool to facilitate vacuuming and place it in the transition chamber of the glove box, tighten the door, and perform a cycle of vacuuming-argon filling steps for 3-4 cycles, with each cycle time not less than 10 minutes. After the end, open the transition chamber from the inside of the glove box, move all materials and tools to the main chamber, close the door of the transition chamber, and vacuum the transition chamber again to ensure the vacuum state of the transition chamber;

[0064] Use tweezers to place the working electrode sheet in the middle of the positive battery shell, and measure 35 μL of electrolyte and drop it on the electrode sheet;

[0065] After the electrolyte is completely spread, cover it with a diaphragm and then drop 35 μL of electrolyte on it;

[0066] After the electrolyte completely soaks the diaphragm, use a vacuum pen to suck the conductive steel sheet and stick it to the prepared sodium sheet, and place it in the center of the diaphragm;

[0067] A metal gasket is added to the conductive steel sheet to ensure that the battery can be pressed tightly to prevent poor contact between the various parts and cause a short circuit in the battery.

[0068] Test Example 4

[0069] The sodium ion battery prepared in Experimental Example 3 was cycled 5 times at rates of 0.1C, 0.2C, 0.5C, 1C, 2C, 5C and 0.1C, and the rate performance of the sodium ion battery was measured. The results are as follows: Figure 3 As shown. Figure 3 It can be seen that compared with the NaNi 0.4 Fe 0.2 Mn 0.4 Compared with the sodium ion battery prepared by O2, the NaNi 0.4 Fe 0.2 Mn 0.4 The sodium ion batteries prepared by O2 are similar in rate performance. When the charge and discharge rate is increased to 5C, the NaNi 0.4 Fe 0.2 Mn 0.4 The discharge capacity of the sodium ion battery prepared by O2 positive electrode material is 110.5 mAh g -1 , NaNi provided in Example 1 0.4 Fe 0.2 Mn 0.4 The discharge capacity of the sodium ion battery prepared by O2 positive electrode material is 108.7 mAh g -1 .

[0070] Test Example 5

[0071] Figure 4 The NaNi provided for the comparative example 0.4 Fe 0.2 Mn 0.4 The sodium ion battery prepared by O2 and the NaNi provided in Examples 1-3 0.4 Fe 0.2 Mn 0.4 Cycle life diagram of sodium ion battery prepared by O2. Figure 4 It can be seen that the NaNi provided in Example 1 0.4 Fe 0.2 Mn 0.4 The sodium ion battery prepared by O2 showed 140.74 mAh·g at 1C rate. -1 After 100 cycles, the capacity retention rate was 85%. The sodium ion battery prepared in Example 2 showed 119.87 mAh·g -1 After 100 cycles, the capacity retention rate was 91.7%. The sodium ion battery prepared in Example 3 showed 110.74 mAh·g -1 , the capacity retention rate after 100 cycles is 93.1%, which is higher than the control example (81%).

[0072] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing positive electrode materials by regenerating waste sodium ion batteries, characterized in that: The following steps are involved: Step 1: Use waste NaNi x Mn 1-x O2、NaNi x Mn y Fe z The waste positive electrode NaNi was obtained after O2 battery discharge, splitting and organic solvent dissolution x Mn 1-x O2 and NaNi x Mn y Fe z O2 mixed powder and negative electrode powder, the above two powders are ball-milled and mechanically mixed and then carbon thermal reduction treatment is performed, the mass ratio of waste positive electrode powder and negative electrode powder is 3-12:1, and the ball milling time is 3-9h; Step 2: water leaching, carbon thermal reduction and powder, separation of leaching solution and leaching residue after leaching, evaporation, concentration and crystallization of the leaching solution to obtain sodium carbonate product; The third step: using acid leaching to separate the leached residue after water leaching, separating the leached solution and the leached residue after acid leaching to obtain the leached solution and leached residue rich in high-purity valuable metal nickel, manganese and iron; Step 4: Add acetate of Ni, Mn and Fe to the leaching solution to adjust Ni 2+ , Fe 3+ , Mn 2+ The molar ratio of 4:2:4 was set, and a precipitant was added, the pH was kept between 10.4 and 10.6, stirring and heating were maintained, and the mixture was aged for 24 hours. After the reaction, the mixture was filtered and washed several times, and then dried in a drying oven at 90°C to obtain Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 Precursor, the precipitant is a mixture of NaOH solution and ammonia water, the volume ratio of NaOH solution to ammonia water is 7:3; Step 5: Sodium carbonate and Ni 0.4 Fe 0.2 Mn 0.4 (OH) 0.2 The precursors are ball-milled and mixed uniformly, and sintered in a muffle furnace to obtain NaNi 0.4 Fe 0.2 Mn 0.4 O2 positive electrode material.

2. The method for preparing positive electrode materials by regenerating waste sodium ion batteries according to claim 1, characterized in that: The organic solvent in the first step is NMP, and the dissolution temperature is 70-90°C.

3. The method for preparing positive electrode materials by regenerating waste sodium ion batteries according to claim 1, characterized in that: The mass ratio of the waste positive electrode powder to the negative electrode powder in the first step is 5-10:1, and the waste positive electrode powder is calcined in a N2 atmosphere at a temperature of 600°C, 650°C or 800°C for 2 hours.

4. The method for preparing positive electrode materials by regenerating waste sodium ion batteries according to claim 1, characterized in that: The carbon thermal reducing agent for the carbon thermal reduction treatment in the first step is waste negative electrode graphite, and the mass fraction of the waste negative electrode graphite is 10-20%.

5. The method for preparing positive electrode materials by regenerating waste sodium ion batteries according to claim 1, characterized in that: In the second step, the solid-liquid ratio of water immersion is 5-20g / L, the time is 1-3h, and the leaching solution and leaching residue are separated after water immersion. The water immersion step is repeated 3-5 times, and the temperature of evaporation and crystallization is 70-90℃.

6. The method for preparing positive electrode materials by regenerating waste sodium ion batteries according to claim 1, characterized in that: The acid in the third step is any one of acetic acid, citric acid, malic acid, succinic acid, ascorbic acid, aspartic acid, oxalic acid, tartaric acid, maleic acid or lactic acid, and the concentration is 2-5 mol / L; Liquid-to-solid ratio is 5-10ml / g; The acid leaching temperature is 50-90°C and the reaction time is 3-6h.

7. The method for preparing positive electrode materials by regenerating waste sodium ion batteries according to claim 1, characterized in that: In the fifth step, the sintering temperature is 400-1000°C and the sintering time is 16-20h.