Preparation method and application of modified polyurethane emulsion with high acrylic acid content

CN116102695BActive Publication Date: 2024-12-03WANHUA CHEM GRP CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310012341.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-05
Publication Date
2024-12-03
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

It is difficult for the prior art to stabilize the preparation of modified polyurethane emulsions with high acrylic acid content without using solvents, and the traditional process has problems of poor environmental protection and low economicality.

Method used

Using prepolymerization reaction and dispersion chain diffuser technology, the modified polyurethane emulsion with high acrylic acid content is achieved by using acrylic monomers instead of solvents in the prepolymerization stage, and dispersing evenly under high shear conditions. Preparation.

Benefits of technology

It has achieved solvent-free preparation of high acrylic content modified polyurethane emulsion, which has improved the manual polishing performance of the paint film and reduced production costs. The emulsion has a small particle size and a transparent appearance, which meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004038128280000071
    Figure BDA0004038128280000071
  • Figure BDA0004038128280000081
    Figure BDA0004038128280000081
  • Figure BDA0004038128280000091
    Figure BDA0004038128280000091
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a modified polyurethane emulsion with a high acrylic acid content. The method comprises the following steps: putting polymer polyol a, polyisocyanate b, hydrophilic chain extender c, non-hydrophilic alcohol chain extender d, non-ionic hydrophilic compound e containing NCO reactive group and part of acrylic acid ester monomer f into a prepolymerization reactor to obtain NCO-terminated prepolymer after reaction; adding part of acrylic acid ester monomer f and neutralizer and mixing; dropping part of emulsifier solution, adding polyamine after uniform dispersion to carry out chain extension reaction to obtain crude emulsion a; 4) adding remaining acrylic acid ester monomer f and emulsifier into the crude emulsion a under high-speed shearing conditions to obtain crude emulsion b with a high acrylic acid content; 5) transferring the crude emulsion b to a polymerization reactor to initiate polymerization, cooling and filtering to obtain the modified polyurethane emulsion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a modified polyurethane emulsion, in particular to a preparation method and application of a modified polyurethane emulsion with a high acrylic acid content. Background Art

[0002] There are two main types of clear primers for the outer coating of solid wood furniture: oil-based UV clear primer and water-based clear primer. Traditional oil-based UV coatings have high viscosity of oligomers, so diluents must be added to adjust rheology and viscosity to improve the performance of the coating. The added diluents include reactive diluent monomers or cross-linking agents, which have a strong irritating effect on the eyes, and skin contact can easily cause allergies, affecting the health of the operator. Water-based clear primer uses water as a dispersion medium. Compared with oil-based UV clear primer, it has the advantages of being non-toxic, non-flammable, non-polluting, energy-saving, safe and reliable, and has become a development trend in recent years.

[0003] In addition, for the purpose of outer coating of solid wood furniture, due to the limitation of finished products, acrylic emulsion is more inclined to be selected in resin selection. However, the film fullness of pure acrylic emulsion is low, while polyurethane emulsion has good adhesion and fullness, but its water resistance and weather resistance are generally poor. Therefore, acrylic modified polyurethane came into being, which has both the low cost of acrylic emulsion and the good toughness and good coating fullness of polyurethane emulsion.

[0004] In order to obtain better coating effects, the solid wood furniture industry usually paints multiple times, during which the paint surface undergoes multiple manual polishing to enhance the luxurious high-gloss effect of the original wood. This requires that the acrylic acid content in the modified polyurethane emulsion be as high as possible, while ensuring that the product appearance is transparent and stable without residue. For those skilled in the art, it is quite difficult to prepare a water-based modified polyurethane emulsion with a high acrylic acid content.

[0005] Patent CN105315415A provides a water-based acrylic modified polyurethane emulsion with a high carboxylic acid content. After the polyurethane oligomer is prepared, it is capped with a hydroxy acrylic monomer, and then the obtained macromonomer M is subjected to free radical copolymerization with an acrylate monomer, a hydroxy monomer containing a functional group, or a carboxylic acid monomer in a solvent to obtain an acrylic modified polyurethane polymer with a grafted structure. Finally, an alkali is added for neutralization and water is added dropwise for phase inversion to obtain an acrylic modified polyurethane aqueous dispersion. However, this process still uses acetone as a solvent, which is environmentally friendly; and the solid content of the emulsion can only be 30%, which is economically poor. Summary of the invention

[0006] In order to solve the above technical problems, the present invention provides a preparation method and application of a modified polyurethane emulsion with a high acrylic acid content. The present invention can stably prepare a modified polyurethane emulsion with a high acrylic acid content without adding a solvent, and obtain excellent manual polishing performance of the paint film.

[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a modified polyurethane emulsion with a high acrylic acid content comprises the following steps:

[0009] 1) putting polymer polyol a, polyisocyanate b, hydrophilic chain extender c, non-hydrophilic alcohol chain extender d, non-ionic hydrophilic compound e containing NCO reactive group and part of acrylate monomer f into a prepolymerization reactor, completing chain extension and end-capping reaction at 60-100° C. to obtain NCO-terminated prepolymer;

[0010] 2) adding part of the acrylic ester monomer f and the neutralizing agent to the NCO-terminated prepolymer, mixing and transferring to a dispersion chain extension kettle;

[0011] 3) adding part of the emulsifier solution to the dispersion and chain extension kettle, adding polyamine to carry out chain extension reaction after uniform dispersion, and obtaining a crude emulsion a;

[0012] 4) adding the remaining acrylic acid ester monomer f and the emulsifier to the crude emulsion a under high-speed shearing conditions to obtain a crude emulsion b with a high acrylic acid content;

[0013] 5) The crude emulsion b is transferred to a polymerization kettle, and part of the redox agent 1 is added dropwise at a temperature of 20-40° C. in the kettle, and the addition time is controlled to be 5-20 min. After the addition is completed, the remaining redox agent 2 is continued to be added dropwise for 10-40 min; the temperature is lowered and filtered to obtain the modified polyurethane emulsion.

[0014] In the process of the present invention, acrylate monomers are used in place of solvents in the prepolymerization stage to obtain a narrower number average molecular weight, and in addition, a portion of acrylate monomers are added in the early stage of dispersion, and the dispersion process is completed after the addition of anionic nonionic emulsifiers, and finally the remaining acrylate monomers are added under high shear conditions to quickly complete swelling, and then initiate polymerization to obtain a modified polyurethane emulsion, thereby achieving the goal of obtaining a modified polyurethane emulsion with a high acrylic acid content without using a solvent.

[0015] As a preferred embodiment of the present invention, in step 1), the amounts of raw materials used are, in parts by mass, respectively:

[0016] Polymer polyol a 90-120 parts, preferably 100-110 parts,

[0017] Polyisocyanate b 60-80 parts, preferably 65-75 parts,

[0018] Hydrophilic chain extender c 10-20 parts, preferably 11-15 parts,

[0019] Non-hydrophilic alcohol chain extender d 0.1-3 parts, preferably 2-3 parts,

[0020] Nonionic hydrophilic compound e 0.1-3 parts, preferably 1-2 parts,

[0021] Acrylate monomer f 10-45 parts, preferably 20-30 parts,

[0022] In step 2), the amount of the acrylic acid ester monomer f is 100-200 parts by mass, preferably 150-170 parts; the amount of the neutralizing agent is 5-15 parts by mass, preferably 8-10 parts;

[0023] In step 3), the amount of the emulsifier is 5-15 parts by mass, preferably 8-10 parts; the amount of the polyamine is 2-5 parts by mass, preferably 2-4 parts;

[0024] In step 4), the amount of the acrylic acid ester monomer f is 40-70 parts by mass, preferably 50-60 parts; the amount of the emulsifier is 3-10 parts by mass, preferably 3-5 parts;

[0025] In step 5), the amount of redox agent 1 is 0.08-0.30 parts by mass, preferably 0.10-0.20 parts; the amount of redox agent 2 is 0.65-0.85 parts by mass, preferably 0.65-0.75 parts.

[0026] As a preferred embodiment of the present invention, the polymer polyol a is a polyester polyol and / or a polyether polyol having a functionality of 2-4 and a weight average molecular weight of 500-4000, preferably one or more of polyether polyol, polytetramethylene glycol, polycarbonate diol, polycaprolactone diol, polypropylene glycol, polybutylene adipate diol, polyneopentyl adipate diol, polyhexanediol adipate diol, and polypropylene glycol, and more preferably one or more of polyether polyol DL2000, polyether polyol DL3000, and polyether polyol DL4000;

[0027] Preferably, the polyisocyanate b is an aliphatic diisocyanate and / or an aromatic diisocyanate, preferably one or more of toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, cyclohexane dimethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate;

[0028] Preferably, the hydrophilic chain extender c is one or more of carboxyl diol, sulfonate diamine and polyethylene glycol, preferably carboxyl diol, more preferably dimethylol propionic acid and / or dimethylol butyric acid;

[0029] Preferably, the non-hydrophilic alcohol chain extender d is an aliphatic diol and / or aliphatic triol having a molecular weight of less than 500, preferably one or more of 1,2-propylene glycol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, diethylene glycol, and trimethylolpropane;

[0030] Preferably, the nonionic hydrophilic compound e is a polyethoxy ether containing a hydroxyl group or an amino group, preferably a monofunctional polyoxyethylene ether with a weight average molecular weight of 200-3000 and an ethylene oxide number of 4-200, more preferably a monomethyl polyoxyethylene ether with a weight average molecular weight of 500-3000 and an ethylene oxide number of 12-75, and further preferably polyethylene glycol monomethyl ether.

[0031] As a preferred embodiment of the present invention, the acrylate monomer f is one or more of hydroxyethyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, butyl methacrylate, phenyl methacrylate, ethyl acrylate, butyl acrylate, and trimethacrylate; preferably, in step 1), the acrylate monomer f contains at least 30wt% of hydroxyethyl acrylate, and the hydroxyl group contained in hydroxyethyl acrylate can react with the NCO group at the end of the polyurethane molecular chain to achieve a partial end-capping effect, so that the relative molecular mass of the chain segment after the prepolymerization is smaller, and in the subsequent shear emulsification process, the chain segments are easier to move relative to each other, easier to entangle into a ball, and shear emulsification is easier to achieve. At the same time, since hydroxyethyl acrylate is introduced into the polyurethane chain segment, the double bond group it has can be free-radical polymerized with other added acrylate monomers in the subsequent free radical polymerization process, truly completing the acrylate copolymerization modification from the molecular design, making the polymerization process more stable and the application performance better.

[0032] Preferably, the neutralizing agent is one or more of triethylamine, triethanolamine, tripropylamine, ammonia water, sodium hydroxide, potassium hydroxide, and dimethylethanolamine.

[0033] As a preferred embodiment of the present invention, the emulsifier is an anionic nonionic emulsifier with a molecular weight of less than 10,000, preferably one or more of sodium dodecyl sulfate SDS, sodium dodecylbenzene sulfonate SDBS, ethoxylated alkyl sulfate sodium salt CM30, isomeric tridecyl alcohol sulfate sodium salt 2030S, and rhamnolipid, more preferably rhamnolipid;

[0034] Preferably, the polyamine is one or more of ethylenediamine, hexamethylenediamine, 4,4-dicyclohexylmethanediamine, isophoronediamine and diethylenetriamine.

[0035] As a preferred embodiment of the present invention, the redox agent 1 and the redox agent 2 are independently selected from at least one of tert-butyl hydroperoxide, tert-amyl hydroperoxide, sodium bisulfite, sodium dithionite and isoascorbic acid, preferably tert-butyl hydroperoxide and / or isoascorbic acid.

[0036] As a preferred embodiment of the present invention, in step 2), the mid-terminal NCO prepolymer is cooled to 60-70° C. before adding the acrylic ester monomer f;

[0037] Preferably, in step 3), the dropwise addition time of the emulsifier solution is controlled within 10-30 min; the reaction temperature after adding the polyamine is 25-40° C., and the reaction time is 5-20 min.

[0038] As a preferred embodiment of the present invention, in step 4), the high-speed shearing condition is: stirring at 1500-3000 rpm for 5-10 min.

[0039] It should be noted that during the preparation of the emulsion provided by the present invention, a polymerization catalyst and an inhibitor can be optionally added. Among them, the catalyst can be selected from bis(dimethylaminoethyl)ether, pentamethyldiethylenetriamine, dimethylcyclohexylamine, dibutyltin dilaurate, organic bismuth, triazine trimerization catalyst, preferably dibutyltin dilaurate and organic bismuth, to promote the reaction of hydroxyl and isocyanate, or to ensure that the reaction reaches the end point; the inhibitor is selected from hydroquinone, hydroquinone methyl ether, dibutyl dithiocarbamate copper, phenothiazine, piperidinol, copper salt, manganese acetate, preferably piperidinol and hydroquinone methyl ether, to avoid self-polymerization of each monomer during a long reaction time, thereby reducing the reaction conversion rate.

[0040] Preferably, the amount of the catalyst is 300-800 ppm based on the total mass of the polymer polyol a, polyisocyanate b, non-hydrophilic alcohol chain extender d and non-ionic hydrophilic compound e in step 1;

[0041] Preferably, the amount of the polymerization inhibitor is 300-500 ppm based on the total mass of the acrylic acid ester monomer f in step 1;

[0042] As a preferred embodiment of the present invention, the solid content of the modified polyurethane emulsion is not less than 40%, preferably 40-42wt%, the pH value is 6-10, and the particle size is 50-150nm.

[0043] Application of a modified polyurethane emulsion with a high acrylic acid content prepared by the method described above in the field of solid wood furniture coating.

[0044] The preparation method of the modified polyurethane emulsion provided by the present invention has the following advantages:

[0045] 1. The present invention does not use solvents in the production process, thus saving production costs, achieving green and environmentally friendly production, and eliminating the safety risks brought by solvents in the production process.

[0046] 2. The present invention adds acrylate monomers three times to reach the highest acrylic acid content allowed by the formula, thereby ensuring excellent manual polishing performance.

[0047] 3. The use of anionic non-ionic emulsifiers, especially rhamnolipids, for phase transition dispersion solves the phase transition problem of solvent-free dispersion. At the same time, the addition of emulsifiers after dispersion makes the final emulsion particle size small and transparent in appearance. Since the yellow color of rhamnolipid appears in the emulsion, it gives the emulsion an orange-yellow appearance, which is favored by customers in the solid wood processing field.

[0048] 4. The segmented addition of redox agent not only ensures the normal initiation of the early implosion reaction, but also solves the problems of slag discharge and high fineness caused by the traditional implosion process, making the emulsion 1250 mesh filter bag filter smooth and with extremely low fineness. DETAILED DESCRIPTION

[0049] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.

[0050] The main raw material information involved in the following embodiments of the present invention is as follows:

[0051] Table 1. Main raw material information

[0052]

[0053]

[0054] Unless otherwise specified, other raw materials and reagents were purchased from commercial products.

[0055] [Example 1]

[0056] (1) 100 g DL2000 (Mw=2000), 65.6 g IPDI, 13.5 g DMPA, 2.29 g BDO, 2 g polyethylene glycol monomethyl ether (Mw=1200), 30 g MMA, 10 g HEA, 0.08 g BI8108 and 0.02 g TEMPO were placed in a prepolymerization reactor and reacted at 75° C. until the NCO content reached a theoretical value of 2.88%, thereby obtaining a terminal NCO prepolymer.

[0057] (2) The NCO-terminated prepolymer was cooled to 60°C, and then 161 g MMA and 9 g DMEA were added. After mixing evenly, the mixture was transferred to a dispersion chain extension kettle.

[0058] (3) 344 g of water and 10 g of rhamnolipid were mixed to obtain an emulsifier solution, which was added dropwise to a dispersion and chain extension kettle within 10 min. After uniform dispersion, the kettle temperature was controlled to 30° C., 3 g of ethylenediamine and 1.6 g of diethylenetriamine were added to carry out a chain extension reaction, and the reaction was continued for 10 min to obtain a crude emulsion a.

[0059] (4) under high-speed shear conditions with a stirring speed of 1500 rpm, the remaining 60 g of MMA, 30 g of water and 5 g of rhamnolipid were added to the crude emulsion a within 5 min to obtain a crude emulsion b with a high acrylic acid content;

[0060] (5) The crude emulsion b was transferred to a polymerization kettle, and the temperature in the kettle was controlled at 30°C. 1.1 g of 10% TBHP solution and 7.83 g of 1% sodium pyrosulfite solution were simultaneously added dropwise into the polymerization kettle within 5 minutes. At this time, the temperature in the kettle gradually increased significantly. After reaching the highest temperature, no temperature control treatment was performed. 4.4 g of 10% t-BHP aqueous solution and 31.32 g of 1% sodium pyrosulfite aqueous solution were simultaneously added dropwise into the polymerization kettle within 30 minutes to complete the elimination of residual substances. After the reaction was completed, the temperature was lowered and the emulsion was filtered using a 1250 mesh filter bag to obtain a modified polyurethane emulsion.

[0061] In the modified polyurethane emulsion prepared in this embodiment, the solid content of the emulsion is 40wt%, the particle size is 75nm, and the pH is 7.9; the slag content filtered out through a 100-mesh metal filter is 13ppm, and the fineness is 5μm.

[0062] [Example 2-8]

[0063] A modified polyurethane emulsion with a solid content of 40 wt% was prepared according to the same process conditions as in Example 1, except that the raw materials and their amounts and process parameters in Table 2 were different:

[0064] Table 2. Raw materials and their amounts (g), process parameters in each example

[0065]

[0066]

[0067]

[0068] [Comparative Example 1]

[0069] The modified polyurethane emulsion was prepared in substantially the same manner as in Example 1, except that the anionic nonionic emulsifier rhamnolipid in step (3) was replaced by a nonionic polyether emulsifier LCN407 of the same mass.

[0070] During the process of this comparative example, during the dispersion process in step (3), the emulsion phase transition was difficult and the material showed obvious thickening, indicating that the dispersion failed.

[0071] [Comparative Example 2]

[0072] The modified polyurethane emulsion was prepared in a method substantially the same as in Example 1, except that the MMA content in step (2) was adjusted to 221 g, and step (4) was deleted, so that the crude emulsion a obtained in step (3) was directly transferred to the polymerization reactor in step (5) to initiate polymerization.

[0073] In the process of this comparative example, during the dispersion process of step (3), the emulsion phase transition viscosity was very large, and 150 g of water was additionally added to obtain a crude emulsion. The modified polyurethane emulsion prepared in this comparative example was extremely difficult to filter and remove residues.

[0074] [Comparative Example 3]

[0075] The modified polyurethane emulsion was prepared in a method substantially the same as that in Example 1, except that step (4) was deleted and the crude emulsion a obtained in step (3) was directly transferred to the polymerization reactor in step (5) to initiate polymerization, thereby obtaining a modified polyurethane emulsion with a low acrylic acid content.

[0076] [Comparative Example 4]

[0077] A modified polyurethane emulsion was prepared in a method substantially the same as that in Example 1, except that step (5) was modified as follows: the crude emulsion b was transferred to a polymerization kettle, the temperature in the kettle was controlled at 30° C., 5.5 g of a 10% TBHP aqueous solution and 39.15 g of a 1% sodium metabisulfite aqueous solution were simultaneously added dropwise into the polymerization kettle over a period of 5 minutes, the temperature in the kettle was cooled down after the reaction was completed until the temperature in the kettle no longer increased, and the emulsion was filtered using a 1250 mesh filter bag to obtain a modified polyurethane emulsion.

[0078] The modified polyurethane emulsions obtained in the embodiments and comparative examples were tested as shown in Table 3, and the results are as follows:

[0079] Table 3. Emulsion parameter test

[0080]

[0081]

Application examples

[0082] Using the modified polyurethane emulsion provided in each embodiment and comparative example, different test varnishes were prepared according to the varnish formula in Table 4.

[0083] Table 4, varnish formula

[0084] Polyurethane emulsion 80g Silicone defoamer BYK-024 0.4g Bick Wetting agent Tego-245 0.3g Digo Wetting agent Tego-270 0.3g Digo Propylene glycol methyl ether 4g Dow Dipropylene glycol butyl ether 4g Dow Polyurethane thickener U605 0.4g Wanhua Thickener water 10.6g / total 100g

[0085] Spray the prepared varnishes on the oak board with a spraying amount of 80g / m 2 , baked at 50℃ for 30min, taken out and placed at room temperature, and then tested after 50 times of reciprocating sandpaper with 400-grit sandpaper. According to the difficulty of breaking the skin during sanding, the amount of powder, the degree of sticking to sandpaper, and the state of the paint film after sanding, the scores were rated respectively. Each test was divided into 1-5 points from poor to excellent, and 3 points was qualified. The test results are shown in Table 5:

[0086] Table 5. Test results of paint film abrasion resistance

[0087]

[0088]

[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a modified polyurethane emulsion with a high acrylic acid content, characterized in that: The following steps are involved: 1) Put polymer polyol a, polyisocyanate b, hydrophilic chain extender c, non-hydrophilic alcohol chain extender d, non-ionic hydrophilic compound containing NCO reactive group e and part of acrylate monomer f into a prepolymerization reactor, complete chain extension and end-capping reaction at 60-100°C to obtain NCO-terminated prepolymer; 2) Add part of the acrylic ester monomer f and the neutralizing agent to the NCO-terminated prepolymer, mix and transfer to a dispersion chain extension kettle; 3) Add part of the emulsifier solution to the dispersion and chain extension kettle, add polyamine after uniform dispersion to carry out chain extension reaction, and obtain a crude emulsion a; 4) adding the remaining acrylic acid ester monomer f and the emulsifier to the crude emulsion a under high-speed shearing conditions to obtain a crude emulsion b with a high acrylic acid content; 5) transferring the crude emulsion b to a polymerization kettle, adding a portion of the redox agent 1 dropwise at a temperature of 20-40° C. in the kettle, and controlling the adding time to be 5-20 min. After the adding is completed, continuing to add the remaining redox agent 2 dropwise, and the adding time is 10-40 min; cooling and filtering to obtain the modified polyurethane emulsion; The emulsifier is an anionic nonionic emulsifier with a molecular weight lower than 10,000.

2. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 1, characterized in that: In step 1), the amounts of raw materials used are, by mass, respectively: Polymer polyol a 90-120 parts, Polyisocyanate b 60-80 parts, Hydrophilic chain extender c 10-20 parts, Non-hydrophilic alcohol chain extender d 0.1-3 parts, Nonionic hydrophilic compound e 0.1-3 parts, Acrylate monomer f 10-45 parts, In step 2), the amount of the acrylic acid ester monomer f is 100-200 parts by weight; the amount of the neutralizing agent is 5-15 parts by weight; In step 3), the amount of the emulsifier is 5-15 parts by weight; the amount of the polyamine is 2-5 parts by weight; In step 4), the amount of acrylic acid ester monomer f is 40-70 parts by weight; the amount of emulsifier is 3-10 parts by weight; In step 5), the amount of the redox agent 1 is 0.08-0.30 parts by mass; the amount of the redox agent 2 is 0.65-0.85 parts by mass.

3. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 2, characterized in that: In step 1), the amounts of raw materials used are, by mass, respectively: Polymer polyol a 100-110 parts, Polyisocyanate b 65-75 parts, Hydrophilic chain extender c 11-15 parts, Non-hydrophilic alcohol chain extender d 2-3 parts, Nonionic hydrophilic compound e 1-2 parts, Acrylate monomer f 20-30 parts, In step 2), the amount of the acrylic acid ester monomer f is 150-170 parts by weight; the amount of the neutralizing agent is 8-10 parts by weight; In step 3), the amount of emulsifier used is 8-10 parts by weight; The amount of polyamine used is 2-4 parts by mass; In step 4), the amount of acrylic acid ester monomer f is 50-60 parts by weight; the amount of emulsifier is 3-5 parts by weight; In step 5), the amount of the redox agent 1 is 0.10-0.20 parts by mass; the amount of the redox agent 2 is 0.65-0.75 parts by mass.

4. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 2, characterized in that: The polymer polyol a is a polyester polyol and / or a polyether polyol having a functionality of 2-4 and a weight average molecular weight of 500-4000.

5. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 4, characterized in that: The polymer polyol a is one or more of polytetramethylene glycol, polycarbonate diol, polycaprolactone diol, polypropylene glycol, polybutylene adipate diol, polyneopentyl adipate diol, polyhexanediol adipate diol and polypropylene glycol.

6. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 4, characterized in that: The polymer polyol a is one or more of polyether polyol DL2000, polyether polyol DL3000 and polyether polyol DL4000.

7. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 4, characterized in that: The polyisocyanate b is an aliphatic diisocyanate and / or an aromatic diisocyanate.

8. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 7, characterized in that: The polyisocyanate b is one or more of toluene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate, cyclohexane dimethylene diisocyanate, and 4,4'-dicyclohexylmethane diisocyanate.

9. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 4, characterized in that: The hydrophilic chain extender c is one or more of carboxyl diol, sulfonate diamine and polyoxyethylene diol.

10. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 9, characterized in that: The hydrophilic chain extender c is carboxyl diol.

11. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 9, characterized in that: The hydrophilic chain extender c is dimethylol propionic acid and / or dimethylol butyric acid.

12. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 4, characterized in that: The non-hydrophilic alcohol chain extender d is an aliphatic diol and / or an aliphatic triol having a molecular weight lower than 500.

13. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 12, characterized in that: The non-hydrophilic alcohol chain extender d is one or more of 1,2-propylene glycol, 1,4-butanediol, 1,5-pentanediol, neopentyl glycol, diethylene glycol, and trimethylolpropane.

14. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 4, characterized in that: The nonionic hydrophilic compound e is a polyethoxy ether containing a hydroxyl group or an amino group.

15. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 14, characterized in that: The nonionic hydrophilic compound e is a monofunctional polyoxyethylene ether with a weight average molecular weight of 200-3000 and an ethylene oxide number of 4-200.

16. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 14, characterized in that: The nonionic hydrophilic compound e is a monomethyl polyoxyethylene ether having a weight average molecular weight of 500-3000 and an ethylene oxide number of 12-75.

17. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 14, characterized in that: The nonionic hydrophilic compound e is polyethylene glycol monomethyl ether.

18. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to any one of claims 1 to 17, characterized in that: The acrylic acid ester monomer f is one or more of hydroxyethyl acrylate, 2-ethylhexyl acrylate, methyl methacrylate, butyl methacrylate, phenyl methacrylate, ethyl acrylate, and butyl acrylate.

19. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 18, characterized in that: In step 1), the acrylic acid ester monomer f contains at least 30 wt % of hydroxyethyl acrylate.

20. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 18, characterized in that: The neutralizing agent is one or more of triethylamine, triethanolamine, tripropylamine, ammonia water, sodium hydroxide, potassium hydroxide, and dimethylethanolamine.

21. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 4, characterized in that: The emulsifier is one or more of ethoxylated alkyl sulfate sodium salt, isomeric tridecyl alcohol sulfate sodium salt, and rhamnolipid.

22. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 21, characterized in that: The emulsifier is rhamnolipid.

23. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 21, characterized in that: The polyamine is one or more of ethylenediamine, hexamethylenediamine, 4,4-dicyclohexylmethanediamine, isophoronediamine and diethylenetriamine.

24. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 4, characterized in that: The redox agent 1 and the redox agent 2 are independently selected from at least one of tert-butyl hydroperoxide, tert-amyl hydroperoxide, sodium bisulfite, sodium dithionite and isoascorbic acid.

25. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 24, characterized in that: The redox agent 1 and the redox agent 2 are independently selected from tert-butyl hydroperoxide and / or isoascorbic acid.

26. The method for preparing the modified polyurethane emulsion with high acrylic acid content according to any one of claims 1 to 17, characterized in that: Step 2) The mid-end NCO prepolymer is cooled to 60-70°C before adding the acrylic monomer f.

27. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 26, characterized in that: In step 3), the dropwise addition time of the emulsifier solution is controlled within 10-30 min; the reaction temperature after adding the polyamine is 25-40° C., and the reaction time is 5-20 min.

28. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 26, characterized in that: In step 4), the high-speed shearing condition is: stirring at 1500-3000 rpm for 5-10 min.

29. The method for preparing the modified polyurethane emulsion with high acrylic acid content according to any one of claims 1 to 17, characterized in that: The modified polyurethane emulsion has a solid content of not less than 40%, a pH value of 6-10, and a particle size of 50-150 nm.

30. The method for preparing a modified polyurethane emulsion with a high acrylic acid content according to claim 29, characterized in that: The solid content of the modified polyurethane emulsion is 40-42wt%.

31. Use of a modified polyurethane emulsion with a high acrylic acid content prepared by the method according to any one of claims 1 to 30 in the field of solid wood furniture coating.

Citation Information

Patent Citations

  • Preparation method for water-borne acrylic acid modified polyurethane emulsion with high carboxylic acid content through one step

    CN105315415A