An extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material and a preparation method thereof

By introducing Ni, Gd, Y, Zn, and Cu elements into magnesium-based hydrogen storage materials, and using semi-continuous casting and extrusion processes, the problems of easy oxidation and slow kinetic performance of magnesium-based hydrogen storage materials have been solved, and the High hydrogen storage capacity and rapid hydrogen absorption and release kinetics reduce costs and improve quality uniformity.

CN116103552BInactive Publication Date: 2024-10-29CENT SOUTH UNIV +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211091074.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-07
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Magnesium-based hydrogen storage materials have problems such as easy oxidation, difficulty in activation, slow kinetic properties, high hydrogen release temperature, high cost, and poor uniformity of performance and quality in large-scale preparation, which limits their industrial application.

Method used

The extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material is used. By introducing specific amounts of Ni, Gd, Y, Zn and Cu elements, combined with semi-continuous casting, homogenization treatment and extrusion process, the alloy composition and Preparation process to form materials with excellent hydrogen storage capacity and rapid hydrogen absorption and release kinetic properties.

Benefits of technology

It achieves the high hydrogen storage capacity and rapid hydrogen absorption and release kinetic properties of the magnesium-based hydrogen storage material, reduces the preparation cost, improves the uniformity of performance and quality, and has a simple process and high economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116103552B_ABST
    Figure CN116103552B_ABST
Patent Text Reader

Abstract

An extruded Mg‑Ni‑Gd magnesium-based hydrogen storage functional material comprises the following components in mass percentage: 4-6% Ni, 4-6% Gd, 0.45-1.2% Cu, 0.6-1.2% Y, 0.5-0.8% Zn and the remainder Mg. The present invention also provides a method for preparing an extruded Mg‑Ni‑Gd magnesium-based hydrogen storage functional material, comprising the following steps: (1) smelting and casting the alloy raw materials in sequence to obtain an alloy ingot; (2) post-treating the alloy ingot to obtain a Mg‑Ni‑Gd magnesium-based hydrogen storage functional material; the post-treatment comprises a homogenization treatment and an extrusion treatment in sequence. The extruded Mg‑Ni‑Gd magnesium-based hydrogen storage functional material of the present invention can not only maintain a high hydrogen storage capacity of magnesium-based hydrogen storage, but also has an excellent hydrogen absorption and desorption rate index, with low cost and high economic benefit.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of alloy functional materials, and in particular relates to an extruded magnesium-based hydrogen storage functional material and a preparation method thereof. Background Art

[0002] In recent years, with the depletion of fossil fuels and the serious pollution they cause to the environment, it is urgent to find a renewable energy source that can replace fossil fuels. As a clean secondary energy source, hydrogen is not only abundant in reserves, green and pollution-free, but also a high calorific value fuel, and has received widespread attention.

[0003] So far, the extraction technology of hydrogen has been relatively mature. How to store hydrogen efficiently, at low cost and safely has become an important key link in the development of hydrogen energy. Magnesium-based hydrogen storage functional materials stand out among many hydrogen storage functional materials with their excellent hydrogen storage capacity, low cost, light weight and good reversibility, and are considered to be one of the hydrogen storage functional materials with broad prospects.

[0004] However, magnesium-based hydrogen storage materials still have bottlenecks such as easy oxidation, difficulty in activation, slow kinetic performance, high hydrogen desorption temperature, high cost, and difficulty in mass production of hydrogen storage alloys with uniform performance and quality, which to a certain extent limit their actual industrial application. In order to improve the comprehensive hydrogen storage performance of magnesium-based hydrogen storage materials, the main method at present is alloying. By alloying, transition metal elements (Cu, Ni, etc.) or rare earth elements (Gd, Y, La, etc.) are added to regulate the microstructure of the alloy, thereby changing its hydrogen absorption and desorption mechanism to achieve the purpose of improving its hydrogen storage performance. At present, hydrogen storage materials represented by Mg-Ni-based alloys have been developed. In the Mg-Ni system, the presence of Mg2Ni greatly improves its hydrogen storage absorption and desorption kinetics, providing an important idea for the development of magnesium-based hydrogen storage functional materials. Based on Mg-Ni-based alloys, hydrogen storage materials such as Mg-Ni-RE have also been developed. The introduction of rare earth elements can increase the hydrogen desorption rate of magnesium-based hydrogen storage materials, thereby further improving the hydrogen storage performance of magnesium-based hydrogen storage functional materials.

[0005] So far, magnesium-based hydrogen storage materials still have shortcomings such as stable thermodynamic properties and slow kinetic properties. Therefore, it is urgent to develop a new type of magnesium-based hydrogen storage functional material with excellent hydrogen storage capacity and fast hydrogen absorption and desorption kinetics. At the same time, the new magnesium-based hydrogen storage functional material must also meet the characteristics of low cost, high economic benefits, and uniform performance quality. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology, and to provide an extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material having excellent hydrogen storage capacity and fast hydrogen absorption and desorption kinetics, low preparation cost, and uniform performance and quality, and a preparation method thereof. In order to solve the above technical problems, the technical solution proposed by the present invention is:

[0007] An extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material comprises the following components in mass percentage: 4-6% Ni, 4-6% Gd, 0.45-1.2% Cu, 0.6-1.2% Y, 0.5-0.8% Zn and the balance Mg.

[0008] The above-mentioned extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material preferably includes the following components in mass percentage: Ni 4.3-5.7%, Gd 4.3-5.7%, Cu 0.5-1.1%, Y 0.6-1.1%, Zn 0.53-0.77% and the balance Mg.

[0009] The above-mentioned extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material preferably includes the following components in mass percentage: Ni 4.6-5.4%, Gd 4.6-5.4%, Cu 0.53-1%, Y 0.66-1%, Zn 0.56-0.74% and the balance Mg.

[0010] In the present invention, the main component of the extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material is still magnesium. By introducing a specific amount of modified elements Ni, Gd, Y, Zn, and Cu elements, it is beneficial to improve the hydrogen absorption and desorption kinetics of the magnesium matrix. The amount of the modified elements Ni, Gd, Y, Zn, and Cu elements needs to be precisely controlled to balance the hydrogen storage capacity and the hydrogen absorption and desorption kinetics. In addition, the ratio of each component will also affect the effect of the subsequent preparation process. Through the optimization design of the components, combined with the matching improvement of the preparation process, it is beneficial to the comprehensive performance of the magnesium-based hydrogen storage functional material.

[0011] As a general technical concept, the present invention also provides a method for preparing the above-mentioned extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material, comprising the following steps:

[0012] (1) melting and casting the alloy raw materials in sequence to obtain an alloy ingot; specifically: firstly melting pure Mg, raising the temperature to 740-760°C, adding the intermediate alloy in sequence, introducing SF2 / CO2 (1:99) protective gas during the melting process, and when the temperature drops to 700-720°C, semi-continuous casting is performed to obtain an ingot of Φ325×5000 mm;

[0013] (2) The alloy ingot obtained in step (1) is post-processed to obtain an extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material; the post-processing includes homogenization and extrusion. Specifically, the heat treatment furnace is heated to 200°C and then the cast alloy is placed in it, and the heat preservation treatment is carried out at different temperatures. After the heat preservation time is reached, the alloy is placed in the air to cool; then the semi-continuous ingot is processed into a cast rod with a specification of Φ296×780mm, and the cast rod is placed in an industrial frequency furnace for heating and heat preservation, and the extrusion ratio and extrusion speed are controlled for extrusion treatment.

[0014] In the above preparation method, preferably, the casting temperature in step (1) is 720-760°C. The casting temperature will affect the quality of the final casting. If the melt temperature is too high, defects such as looseness, shrinkage, and central thermal cracks will occur. The higher the casting temperature, the larger the liquid phase area in the melt, which will create conditions that are more conducive to the growth of crystal nuclei, and the primary Mg phase will be coarse; if the casting temperature is too low, some elements in the alloy will be enriched, reducing the fluidity of the melt and causing casting defects.

[0015] In the above preparation method, preferably, the homogenization step in step (2) is as follows: control the initial temperature to 200°C, control the time from 200°C to 250°C to 0.5-1h, then keep it at 250°C for 5-6h, then control the time from 250°C to 460°C to 1.5-2h, finally keep it at 460°C for 18-22h, and finally air cool. Homogenization treatment is to make the elements in the alloy diffuse in the solid state to eliminate the phenomenon of intragranular segregation and improve the performance of the casting. Our research shows that after the cast alloy is homogenized, the LPSO phase will change. In the original LPSO phase, it mainly exists in the eutectic region. The LPSO phase is mainly 14H-LPSO, and there is also a small amount of 18R-LPSO. After homogenization, there is a large amount of 14H-LPSO on the magnesium matrix, that is, the intergranular LPSO phase has transformed into the intragranular LPSO phase. At the same time, 18R-LPSO disappears and becomes 14H-LPSO. 14H-LPSO is more beneficial to improving the hydrogen storage performance than 18R-LPSO. The homogenization temperature corresponds to the homogenization time. High temperature and long time can easily cause coarse grains. Low homogenization temperature and short time will make the elements diffuse insufficiently and the intragranular segregation cannot be eliminated. The above-mentioned programmed homogenization process steps are conducive to the synergistic effect with the subsequent extrusion treatment to improve the hydrogen storage capacity and hydrogen absorption and desorption kinetics of the product.

[0016] In the above preparation method, preferably, the temperature of the extrusion treatment in step (2) is 380-440°C, the extrusion speed is 0.3-3 mm / s, and the extrusion ratio is 6-22. The extrusion temperature will affect the properties of the alloy, and the extrusion ratio will also affect the degree of extrusion of the alloy. Controlling the above extrusion process parameters is conducive to improving the hydrogen storage capacity and hydrogen absorption and desorption kinetics of the product.

[0017] In the above preparation method, preferably, the alloy raw materials include pure Mg ingots, pure Zn ingots, Mg-30% Gd master alloys, Mg-30% Ni master alloys, Mg-25% Cu master alloys and Mg-30% Y master alloys.

[0018] For magnesium-based hydrogen storage alloys, pure magnesium has the highest hydrogen absorption and desorption capacity, but its hydrogen absorption and desorption rate and hydrogen absorption and desorption temperature requirements are very strict, so it is necessary to reasonably design the composition and optimize its hydrogen absorption and desorption conditions under the premise of sacrificing its hydrogen absorption and desorption capacity. The original intention of the composition optimization of the present invention is to retain its hydrogen absorption and desorption capacity as much as possible while improving other performances. The present invention introduces a small amount of Ni, Gd, Y, Zn, and Cu elements on the basis of Mg. Ni and Gd are added mainly to generate Mg2Ni and GdH2 and other phases to accelerate its hydrogen absorption and desorption rate and reduce the hydrogen absorption and desorption temperature. Y, Cu, and Zn are introduced to introduce LPSO phase. LPSO phase can be decomposed into nano catalytic phase in situ under the action of hydrogen, acting as a catalyst. The synergistic effect of each phase is conducive to improving the hydrogen storage capacity and hydrogen absorption and desorption kinetics of the product. Based on the above-mentioned component design, and through the regulation of the preparation process, the low-cost extrusion process is used to significantly improve the hydrogen storage performance. The final alloy phase composition of the present invention is Mg, Mg2Ni and LSPO phase, of which Mg accounts for the majority, LSPO and Mg2Ni account for a smaller proportion, and the regulated phases Mg2Ni and LSPO phases will not affect the hydrogen storage of the main magnesium, and its hydrogen absorption and desorption capacity is retained to the maximum extent. Overall, the present invention optimizes the composition, based on the specific components, and then adopts a specific preparation process, using a specific homogenization treatment and extrusion process to cooperate and modify, which is used to regulate the phase composition of the final product, the alloy components and the preparation process cooperate with each other, and the advantages complement each other, and the final extruded Mg-Ni-Gd series magnesium-based hydrogen storage functional material has excellent hydrogen storage capacity and hydrogen absorption and desorption kinetics.

[0019] In addition, compared with the induction melting method, the semi-continuous casting ingots used in the present invention can be produced using existing metal processing and casting facilities, with a short preparation technology process and a high yield rate. At the same time, the semi-continuous casting ingots obtained can be directly processed into powder chips in large quantities and put into practical use. Compared with other technical means, on the basis of obtaining the finished alloy material, it is necessary to carry out traditional time-consuming and high-cost methods such as high-energy ball milling. The present invention has higher economic benefits, low preparation and processing costs, short activation time, and no expensive and time-consuming processing process such as ball milling. At the same time, on the basis of the semi-continuous casting state, the present invention uses extrusion and other means to continue to optimize the performance of hydrogen storage functional materials. Compared with the cast alloy, the hydrogen storage capacity of the extruded alloy has a qualitative leap, and the hydrogen absorption and desorption rate is also improved.

[0020] Compared with the prior art, the advantages of the present invention are:

[0021] 1. The present invention designs the Mg-Ni-Gd-Y-Zn-Cu system by rationally designing the types of alloy elements and optimizing the alloy composition. The cast magnesium-based hydrogen storage alloy ingot is first obtained by semi-continuous casting, and then the extruded Mg-Ni-Gd system hydrogen storage functional material is obtained by homogenization treatment and mechanical plastic deformation on the basis of the semi-continuous ingot. The extruded Mg-Ni-Gd system magnesium-based hydrogen storage functional material designed by the present invention can not only maintain the high hydrogen storage capacity of magnesium-based hydrogen storage, but also has excellent hydrogen absorption and desorption rate indicators, low cost and high economic benefits.

[0022] 2. The advantages of the extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material designed by the present invention in regulating hydrogen storage performance are specifically reflected in the following aspects: (1) The presence of the Mg2Ni phase can accelerate the hydrogen absorption rate of the magnesium-based hydrogen storage functional material and reduce the hydrogen absorption temperature; (2) During the hydrogen absorption process, LPSO can serve as a hydrogen diffusion channel to accelerate the hydrogen absorption and desorption process, and on the other hand, LPSO can be decomposed in situ to form nano-sized particles, which can act as a catalyst in the hydrogen absorption and desorption process to improve the hydrogen absorption and desorption kinetics, especially greatly accelerating its desorption rate; (3) The grain size of the alloy can be refined by extrusion molding. At the same time, severe plastic deformation can introduce a large number of crystal defects such as dislocations, which will play an important role in the hydrogen storage performance of the alloy.

[0023] 3. The practical application advantages of the extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material designed by the present invention are specifically reflected in the following aspects: (1) it can be produced using existing metal processing and casting facilities, with a short preparation process and a high yield rate; (2) there is no need to use traditional time-consuming and high-cost methods such as high-energy ball milling to reprocess magnesium powder chips. The magnesium-based hydrogen storage functional material of the present invention has low cost and high economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 This is the X-ray diffraction pattern of the cast magnesium-based hydrogen storage functional material obtained in step (1) of Example 1.

[0026] Figure 2The following are scanning electron microscope images of the cast magnesium-based hydrogen storage functional material obtained in step (1) of Example 1; wherein (a) is a low-magnification scanning electron microscope image of the cast magnesium-based hydrogen storage functional material, and (b) is a high-magnification scanning electron microscope image of the eutectic region.

[0027] Figure 3 This is a high-magnification scanning electron microscope image of the eutectic region of the cast magnesium-based hydrogen storage functional material obtained in step (1) of Example 1 after deep etching.

[0028] Figure 4 The figures are scanning electron microscope images of the cast magnesium-based hydrogen storage functional material powder obtained in step (2) of Example 1 before and after hydrogenation; wherein (a) is a low-magnification scanning electron microscope image before hydrogenation, (b) is a high-magnification scanning electron microscope image before hydrogenation, (c) is a low-magnification scanning electron microscope image after hydrogenation, and (d) is a high-magnification scanning electron microscope image after hydrogenation.

[0029] Figure 5 This is the X-ray diffraction pattern of the magnesium-based hydrogen storage functional material after hydrogenation in step (2) of Example 1.

[0030] Figure 6 The following are scanning electron microscope images of the extruded magnesium-based hydrogen storage functional material obtained in step (2) of Example 2; wherein (a) is a low-magnification scanning electron microscope image of the extruded magnesium-based hydrogen storage functional material, and (b) is a high-magnification scanning electron microscope image of the extruded magnesium-based hydrogen storage functional material.

[0031] Figure 7 These are thermodynamic analysis diagrams of the cast magnesium-based hydrogen storage functional material after hydrogenation in Example 3; wherein (a) is a DSC diagram of the hydrogenated sample at a heating rate of 10° / min, and (b) is a TGA diagram of the hydrogenated sample.

[0032] Figure 8 This is a graph showing the results of hydrogen absorption performance testing of the extruded Mg-Ni-Gd hydrogen storage functional material powder obtained from Example 4 at four temperatures of 360°C, 330°C, 300°C, and 250°C under a hydrogen pressure of 2MPa.

[0033] Fig. 9 The hydrogenated extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material powder obtained in Example 5 was subjected to hydrogen desorption performance tests at three temperatures: 360°C, 330°C, and 300°C under vacuum.

[0034] Fig.10 This is a graph showing the results of hydrogen absorption performance testing of the semi-continuously cast Mg-Ni-Gd hydrogen storage functional material powder obtained from Example 6 at four temperatures of 360°C, 330°C, 300°C, and 250°C under a hydrogen pressure of 2MPa.

[0035] Fig.11The hydrogenated semi-continuously cast Mg-Ni-Gd magnesium-based hydrogen storage functional material powder obtained in Example 7 was subjected to hydrogen desorption performance tests at three temperatures: 360°C, 330°C, and 300°C under vacuum. DETAILED DESCRIPTION

[0036] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the present invention, but the protection scope of the present invention is not limited to the following specific embodiments.

[0037] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0038] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0039] Embodiment 1:

[0040] The Mg-Ni-Gd magnesium-based hydrogen storage functional material provided in this embodiment is composed of the following components in mass percentage: Ni 5.12%, Gd 4.87%, Cu 0.53%, Y 0.76%, Zn 0.6% and the balance Mg. The preparation method thereof includes the following steps:

[0041] (1) The alloy raw materials are sequentially melted and cast to obtain alloy ingots. Specifically: a crucible with a volume of 2000 kg is used for melting, and the raw materials used are pure Mg (Mg ≥ 99.9%), Mg-30% Gd, Mg-30% Ni, Mg-25% Cu, Mg-30% Y and pure Zn. Pure Mg is first melted, and when the temperature is raised to 760°C, intermediate alloys are added in sequence. SF6 / CO2 (1:99) protective gas is introduced during the melting process, and when the temperature drops to 700°C, semi-continuous casting is performed to obtain an ingot of Φ325×5000 mm.

[0042] (2) The ingot obtained in step (1) is subjected to a pulverization treatment. First, magnesium shavings are removed from the ingot using a diamond file, and then finer shavings are screened through a 100-mesh sieve and hydrogenated at 380° C. and 3 MPa.

[0043] The cast alloy obtained in step (1) of Example 1 was characterized by X-ray diffraction to characterize the original structure of the alloy. The characterization results are as follows: Figure 1 Then the microstructure of the cast alloy was observed by scanning electron microscope. The results are shown in Figures 2-3 As shown. Among them, Figure 2 (a) is a low-magnification scanning image of the cast alloy obtained in Example 1, Figure 2 (b) is a high-magnification scanning electron microscope image of the as-cast eutectic region obtained in Example 1; Figure 3 This is a high-magnification scanning electron microscope image of the eutectic area after deep corrosion of the cast alloy.

[0044] Depend on Figure 1 It can be seen that the cast alloy of this embodiment consists of Mg, Mg2Ni and LPSO phases. Figure 2 (a) shows that the as-cast alloy structure consists of magnesium matrix + eutectic. Figure 2 (b) is the specific composition of the eutectic part, the white part is Mg2Ni, and the gray part is LPSO phase; Figure 2 It can be seen that the LPSO phase of the cast alloy mainly exists on the eutectic, the LPSO type is mainly 14H-LPSO, there is a small amount of 18R-LPSO at the edge of the eutectic, and there is no LPSO phase on the magnesium matrix. Figure 3 It can be seen that the cast alloy consists of lamellar eutectic and Mg matrix.

[0045] Hydrogen absorption experiment: The magnesium powder obtained in step (2) was hydrogenated at 3MPa and 380°C to obtain a hydrogenated sample. The microstructures of the original cast powder and the hydrogenated sample powder were observed using a scanning electron microscope. The results are as follows: Figure 4 Then the hydrogenated sample was characterized by laboratory XRD diffraction, and the characterization results are shown in Figure 5 shown.

[0046] according to Figure 4 It can be seen that the Mg-Ni-Gd magnesium alloy powder prepared in Example 1 showed jagged edges and flat edges before hydrogenation, and the powder size was relatively large; after hydrogen absorption, the powder became smaller and denser, agglomerated, and cracks appeared. Figure 5 The XRD diffraction pattern shows that the hydrogenated phase is composed of Mg, MgH2, Mg2Ni, Mg2NiH4, GdH3, GdH2 and MgO. Figure 4 and Figure 5 The presence of cracks and nano-sized rare earth hydrides effectively improves the hydrogen absorption and desorption kinetics of the alloy.

[0047] Embodiment 2:

[0048] The semi-continuous ingot obtained in step (1) of Example 1 was subjected to homogenization heat treatment: the initial temperature was controlled to be 200°C, the time for heating from 200°C to 250°C was controlled to be 0.5 h, then the temperature was kept at 250°C for 5 h, then the time for heating from 250°C to 460°C was controlled to be 1.5 h, and finally the temperature was kept at 460°C for 20 h. Finally, the alloy was cooled in air after air cooling for the holding time.

[0049] The homogenized semi-continuous cast rod was extruded with an extrusion ratio of about 9, a mold heating temperature of 395°C, a holding time of 15 minutes, and an extrusion speed of 0.3 mm / s.

[0050] The microstructure of the extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material obtained in Example 2 was observed using a scanning electron microscope. Figure 6 shown.

[0051] according to Figure 6 It can be seen that during the extrusion process, the grains are refined, typical extrusion streamlines appear, and the eutectic structure is crushed. The refinement of grains and the change of eutectic structure will have an important impact on improving the hydrogen storage performance of the alloy.

[0052] Embodiment 3:

[0053] The magnesium-based hydrogen storage functional material powder obtained in step (2) of Example 1 was placed in a hydrogenation furnace, and the temperature was set to 400° C., the pressure was 4 MPa, and the insulation time was 4 h to allow it to be completely hydrogenated.

[0054] Thermodynamic properties / hydrogen desorption capacity analysis of the fully hydrogenated alloy was performed using DSC / TGA. The results are as follows: Figure 7 As shown. Among them, Figure 7 (a) is the DSC graph of the hydrogenated sample with a heating rate of 10° / min. Figure 7 (b) is the TGA graph of the hydrogenated sample.

[0055] according to Figure 7 (a) It can be seen that the dehydrogenation process of the cast Mg-Ni-Gd hydrogen storage functional material is divided into two stages: the first stage starts at 231°C, corresponding to the allotropic transformation of Mg2NiH4, the dehydrogenation of GdH3 to GdH2 and the dehydrogenation of Mg2NiH4 to Mg2Ni; the second stage starts at 390°C, corresponding to the dehydrogenation process of MgH2. TGA results show that the amount of hydrogen released by this alloy in the second stage (dehydrogenation process) reaches 6.4%, which has excellent hydrogen storage capacity.

[0056] Embodiment 4:

[0057] The extruded Mg-Ni-Gd hydrogen storage functional material obtained in Example 2 was subjected to the powdering treatment as in step (2) of Example 1, and then the powder was placed in a Sievert-type device to test the hydrogen storage performance of the alloy. After activation, the alloy was tested for hydrogen absorption performance at four temperatures of 360°C, 330°C, 300°C, and 250°C under a hydrogen pressure of 2MPa. The results of the hydrogen absorption performance test are shown in FIG. Figure 8 The hydrogen absorption amount indicates the amount of hydrogen that can be absorbed within 1 hour at different temperatures, and the hydrogen absorption time indicates the time required to reach 85% of the hydrogen absorption amount at each temperature.

[0058] according to Figure 8 It can be seen that the hydrogen absorption amount of the extruded Mg-Ni-Gd hydrogen storage functional material at 2MPa, 360℃, 330℃, 300℃, and 250℃ for 1h is 4.7wt.%, 4.44wt.%, 4.28wt.%, and 3.64wt.%, respectively, and the hydrogen absorption time required to reach 85% of the hydrogen absorption amount is 126s, 710s, 1185s, and 600s, respectively. It can be found that the extruded Mg-Ni-Gd hydrogen storage functional material has excellent hydrogen storage capacity and fast hydrogen absorption kinetic rate.

[0059] Embodiment 5:

[0060] The hydrogenated extruded Mg-Ni-Gd hydrogen storage functional material obtained by hydrogenation at 360°C, 330°C and 300°C for 1h in Example 4 was tested for hydrogenation performance at the same temperature. The hydrogenation performance results are as follows: Fig. 9 The hydrogen release time indicates the time required for the hydrogen release amount to reach 85% of the hydrogen absorption amount in Example 4.

[0061] according to Fig. 9 It can be seen that the time required for the extruded Mg-Ni-Gd hydrogen storage functional material to release 85% of the hydrogen absorbed in Example 4 at 360°C, 330°C and 300°C is 56s, 101s and 290s respectively. It can be seen that the extruded Mg-Ni-Gd hydrogen storage functional material designed by the present invention has excellent hydrogen release rate performance indicators.

[0062] Embodiment 6:

[0063] The semi-continuously cast Mg-Ni-Gd hydrogen storage functional material obtained in step (2) of Example 1 was placed in a Sievert-type device to test the hydrogen storage performance of the alloy. After activation, the alloy was tested for hydrogen absorption performance at four temperatures of 360°C, 330°C, 300°C, and 250°C under a hydrogen pressure of 2MPa. The results of the hydrogen absorption performance test are shown in FIG. Fig.10 The hydrogen absorption amount indicates the amount of hydrogen that can be absorbed within 1 hour at different temperatures, and the hydrogen absorption time indicates the time required to reach 85% of the hydrogen absorption amount at each temperature.

[0064] according to Fig.10It can be seen that the semi-continuously cast Mg-Ni-Gd hydrogen storage functional material has a hydrogen absorption capacity of 3.35wt.%, 2.98wt.%, 3wt.%, 2.6wt.% and a hydrogen absorption time of 990s, 1170s, 1175s and 1560s respectively when hydrogenated for 1h at 2MPa, 360℃, 330℃, 300℃ and 250℃. The extruded Mg-Ni-Gd hydrogen storage functional material is also significantly better than the semi-continuously cast one in terms of hydrogen absorption capacity and hydrogen absorption rate performance indicators.

[0065] Embodiment 7:

[0066] The hydrogenated semi-continuously cast Mg-Ni-Gd hydrogen storage functional material obtained by hydrogenation at 360°C, 330°C and 300°C for 1h in Example 6 was tested for hydrogenation performance at the same temperature. The hydrogenation performance results are as follows: Fig.11 The hydrogen release time indicates the time required for the hydrogen release amount to reach 85% of the hydrogen absorption amount in Example 6.

[0067] according to Fig.11 It can be seen that the semi-continuously cast Mg-Ni-Gd hydrogen storage functional material requires 101s, 172s, and 364s for the hydrogen release amount to reach 85% of the hydrogen absorption amount in Example 6 at 360°C, 330°C, and 300°C, respectively. It can be seen that the extruded Mg-Ni-Gd hydrogen storage functional material is also significantly better than the semi-continuously cast one in terms of hydrogen release rate.

[0068] Embodiment 8:

[0069] The extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material provided in this embodiment is composed of the following components in mass percentage: Ni 4.5%, Gd 4.2%, Cu 0.48%, Y 0.8%, Zn 0.7% and the balance Mg. The preparation method thereof includes the following steps:

[0070] (1) Same as Example 1;

[0071] (2) taking the semi-continuous ingot obtained in step (1) and subjecting it to homogenization heat treatment: keeping it at 220° C. for 0.5 h, then keeping it at 250° C. for 5 h, then keeping it at 400° C. for 1.5 h, and finally keeping it at 460° C. for 20 h, and finally air cooling the alloy after the holding time has elapsed, and then cooling it in air;

[0072] (3) The homogenized semi-continuous cast rod is extruded with an extrusion ratio of about 8, a mold heating temperature of 420°C, a holding time of 15 min, and an extrusion speed of 1 mm / s.

[0073] Embodiment 9:

[0074] The extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material provided in this embodiment is composed of the following components in mass percentage: Ni 5.8%, Gd 5.2%, Cu 0.68%, Y 0.72%, Zn 0.6% and the balance Mg. The preparation method thereof includes the following steps:

[0075] (1) Same as Example 1;

[0076] (2) taking the semi-continuous ingot obtained in step (1) and subjecting it to homogenization heat treatment: keeping it at 200° C. for 1 h, then keeping it at 250° C. for 6 h, then keeping it at 300° C. for 2 h, and finally keeping it at 460° C. for 19 h, and finally air cooling the alloy after the holding time has elapsed, and then cooling it in air;

[0077] (3) The homogenized semi-continuous cast rod is extruded with an extrusion ratio of about 10, a mold heating temperature of 380°C, a holding time of 15 min, and an extrusion speed of 0.5 mm / s.

Claims

1. A method for preparing an extruded Mg-Ni-Gd magnesium-based hydrogen storage functional material, characterized in that: The magnesium-based hydrogen storage functional material comprises the following components in mass percentage: Ni 4-6%, Gd 4-6%, Cu 0.45-1.2%, Y 0.6-1.2%, Zn 0.5-0.8% and the balance Mg; The preparation method comprises the following steps: (1) melting and casting the alloy raw materials in sequence to obtain an alloy ingot; (2) post-treating the alloy ingot obtained in step (1) to obtain a Mg-Ni-Gd magnesium-based hydrogen storage functional material; the post-treating comprises homogenization treatment and extrusion treatment in sequence; The homogenization process in step (2) is as follows: controlling the initial temperature to 200°C, controlling the time from 200°C to 250°C to 0.5-1h, then keeping the temperature at 250°C for 5-6h, then controlling the time from 250°C to 460°C to 1.5-2h, finally keeping the temperature at 460°C for 18-22h, and finally air cooling; The temperature of the extrusion treatment in step (2) is 380-440° C., the extrusion speed is 0.3-3 mm / s, and the extrusion ratio is 6-22.

2. The preparation method according to claim 1, characterized in that: The invention comprises the following components in mass percentage: Ni 4.3-5.7%, Gd 4.3-5.7%, Cu 0.5-1.1%, Y 0.63-1.1%, Zn 0.53-0.77% and the balance Mg.

3. The preparation method according to claim 2, characterized in that: The alloy comprises the following components in mass percentage: Ni 4.6~5.4%, Gd 4.6~5.4%, Cu 0.53~1%, Y 0.66~1%, Zn 0.56~0.74% and the balance Mg.

4. The preparation method according to claim 1, characterized in that: The casting temperature in step (1) is 720-760°C.

5. The preparation method according to any one of claims 1 to 4, characterized in that: The alloy raw materials include pure Mg ingots, pure Zn ingots, Mg~30%Gd master alloys, Mg~30%Ni master alloys, Mg~25%Cu master alloys and Mg~30%Y master alloys.

Citation Information

Patent Citations

  • Magnesium-based nano-composite hydrogen storage material with dispersively distributed catalytic phase and preparation method of material

    CN107345282A

  • LPSO-phase strengthened degradable high-temperature magnesium alloy and preparation method thereof

    CN111235450A