A solid waste recycling vegetation concrete cementitious material
By using cementitious materials composed of low-alkalinity sulfoaluminate cement and modified phosphogypsum, the problems of high pH value, low seed germination rate and high maintenance cost of vegetation concrete have been solved, realizing low-carbon and environmentally friendly high-strength vegetation concrete, which is suitable for slope protection.
Patent Information
- Application Number
- CN202310062925.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-17
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2043-01-17
AI Technical Summary
The existing vegetation concrete cementitious materials have too high a pH value, resulting in low seed germination rate, low early strength, high maintenance costs, high carbon emissions, and are not environmentally friendly.
The cementitious material, composed of low-alkalinity sulfoaluminate cement, modified phosphogypsum, volcanic ash, perlite tailings, polyacrylamide, potassium sulfate, and ammonium sulfate, is used to neutralize the alkaline substances generated by the hydration reaction through sulfate activation and the hydration reaction of low-alkalinity sulfoaluminate cement, combined with the action of humic acid and water-absorbing resin. This provides organic nutrients and trace elements, enhancing the strength and water retention performance of the vegetation concrete.
It lowers the pH value of vegetation concrete, increases seed germination rate, reduces maintenance costs, enhances the early strength and later performance of vegetation concrete, reduces carbon emissions, and is environmentally friendly.
Smart Images

Figure CN116120030B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and more specifically to a solid waste recycling vegetation concrete cementitious material. Background Art
[0002] Vegetation concrete technology is one of the most widely used technologies. It is based on geotechnical engineering and botany theory. It uses foreign soil mixed with a certain amount of mixed materials. The wire mesh is first reinforced with anchor rods on the slope surface, and then the mixed materials containing planting soil, plant seeds, water retaining agents, etc. are sprayed onto the slope surface using a spraying machine to form a soil complex with a thickness of 10-20cm and certain porosity. Seeds can take root, germinate, and grow in the complex. Such a complex has a certain strength and can prevent rainwater erosion and erosion. After a period of time, when the plants grow up, the purpose of restoring the vegetation of the slope, improving the landscape, and protecting the environment is achieved through the protective effect of vegetation. It is a vegetation restoration technology that integrates multiple disciplines such as geotechnical engineering, botany, soil science, and environmental ecology.
[0003] At present, vegetated concrete products have been widely used, but most of them are still in the research and development test stage. Vegetated concrete requires the use of special cementitious materials; it also needs to provide plants with the necessary space, nutrients and water for growth; it also needs to be durable enough and operable for vegetation replanting.
[0004] In the prior art, ordinary silicate cement is used as a cementitious material in the preparation of vegetation concrete. During the hydration process of ordinary silicate cement, strong alkaline hydration products such as calcium hydroxide will be produced, forming a strong alkaline environment, which is not conducive to the early germination of plants and the long-term growth in the later period, resulting in the situation that the plants do not germinate or the growth rate is low in the next year. In order to solve the above-mentioned technical problems, the most commonly used methods are alkali-reducing admixture technology and mineral admixture technology. Invention patent CN110317008B discloses a vegetation concrete and its preparation method and application. The vegetation concrete of the invention has weak alkalinity during the hydration process, excellent fertility and water retention properties, provides an excellent growth environment for plants, and utilizes solid waste at the same time. However, the invention adds an alkaline stimulator in the process of reducing alkali, and the alkalinity of the prepared vegetation concrete is still very high. It is not suitable for the growth of most seeds; the patent does not take into account the serious shrinkage of the alkali-activated system, which is easy to fall off, and the plant fiber is not suitable for the dry spraying process and cannot play a toughening role; the use of cellulose ether will also increase the compaction of the soil and reduce the overall performance of the vegetation concrete; in addition, the solid waste fly ash involved is currently in short supply as a resource.
[0005] Invention patent CN108323380B discloses a construction method for greening slope protection in saline-alkali land for planting radix strychnifoliae. The invention reduces the alkali return phenomenon when pouring greening slope protection in saline-alkali land, and solves the problem of single vegetation and low survival rate in saline-alkali land slope protection. However, the invention adds a large amount of alkali-reducing materials, which is costly and has a limited scope of application.
[0006] Therefore, providing a solid waste recycling vegetation concrete cementitious material with low natural alkalinity, utilization of solid waste, environmental friendliness, low subsequent maintenance cost, and good slope protection effect has become an urgent problem to be solved by technical personnel in this field. Summary of the invention
[0007] In order to overcome the defects and deficiencies in the above-mentioned prior art, the present invention provides a solid waste recycling vegetation concrete cementitious material. The purpose of the present invention is to solve the problems of excessively high pH value, low seed germination rate, low initial strength, high maintenance cost, and high carbon emissions in the prior art vegetation concrete cementitious material. The cementitious material provided by the present invention has low carbon emissions, low native pH value, small amount of buffer, simple maintenance conditions, and saved maintenance costs; it has a high seed germination rate, good slope protection effect, can carbonize and absorb carbon dioxide, and is environmentally friendly.
[0008] In order to solve the above problems existing in the prior art, the present invention is implemented through the following technical solutions.
[0009] The present invention provides a solid waste recycling vegetation concrete cementitious material, the concrete cementitious material comprises the following raw materials in parts by mass:
[0010] Sulphoaluminate cement 15-25 parts;
[0011] 30-40 parts of modified phosphogypsum;
[0012] 15-25 parts of volcanic ash;
[0013] Perlite tailings 20-30 parts;
[0014] Polyacrylamide 0.5-1 part;
[0015] Potassium sulfate 0.5-1 part;
[0016] 0.5-1 part of ammonium sulfate;
[0017] Among them, sulphoaluminate cement is low-alkalinity sulphoaluminate cement with a specific surface area of 450 m 2 / kg -550m 2 / kg, cement slurry with a ash-water ratio of 1:10, and a pH value of no more than 10.3 in 1h;
[0018] The modified phosphogypsum is prepared by washing and drying 40-60 parts of phosphogypsum until the moisture content is less than 0.5%, and then adding 1-3 parts of water-absorbing resin and 2-5 parts of humic acid and grinding until the specific surface area is greater than 650 m 2 / kg prepared.
[0019] Further preferably, the phosphogypsum is a solid waste generated in a wet phosphoric acid process, and F- is less than 1%.
[0020] Further preferably, the water-absorbing resin has a water absorption ratio greater than 350.
[0021] Further preferably, the humic acid is humic acid raw powder, and the humic acid content in the humic acid raw powder is 30%-80%.
[0022] Further preferably, the volcanic ash has a specific surface area greater than 500 m 2 / kg.
[0023] Further preferably, the perlite tailings are solid waste from the industrial production of perlite, and have a particle size of 0.045 mm-0.075 mm.
[0024] Further preferably, the potassium sulfate, ammonium sulfate and polyacrylamide are all of industrial grade.
[0025] More preferably, the polyacrylamide is anionic polyacrylamide.
[0026] Compared with the prior art, the beneficial technical effects brought by the present invention are as follows:
[0027] 1. In the cementitious material of the vegetation concrete of the present invention, low-alkalinity sulphoaluminate cement is selected and used in a small amount. Sulfate activation and low-alkalinity sulphoaluminate cement provide strength together. The pH value of the hydration product is low. Since humic acid and volcanic ash and other substances are weakly acidic, the pH value inside the vegetation concrete is more suitable for plant growth. In addition, the low-alkalinity sulphoaluminate cement has high early strength, can prevent early sliding and provide early anti-scouring ability.
[0028] 2. Humic acid is added to the phosphogypsum in the cementitious material of the vegetation concrete of the present invention as an antistatic agent and to prevent the ground phosphogypsum from agglomerating. The humic acid is weakly acidic and can neutralize the alkali produced by the hydration reaction and provide organic nutrients for the growth of vegetation. The addition of high-performance water-absorbing resin to the phosphogypsum can also effectively dry the phosphogypsum to prevent agglomeration, thereby ensuring the dispersibility of the phosphogypsum. The water-absorbing resin can also play a role in retaining water in the vegetation concrete, thereby reducing the cost of water spraying and curing. The modified phosphogypsum has a large specific surface area, is not easy to agglomerate, and dissolves quickly in the solution. It can well dissolve calcium sulfate and react with low-alkalinity sulfoaluminate cement to form calcium sulfate. The reaction is as follows:
[0029] 3CaO•3Al2O3•CaSO4+2CaSO4+38H2O→3CaO•Al2O3•3CaSO4•32H2O+2 (Al2O3•3H2O)
[0030] 2CaO•SiO2+nH2O→CS-H+Ca(OH)2
[0031] Al2O3•3H2O+3Ca(OH)2+3CaSO4+26H2O→3CaO•Al2O3•3CaSO4•32H2O
[0032] In addition, the rapidly decomposed sulfate, phosphoric acid and calcium hydroxide generated by the hydration reaction of low-alkalinity sulfoaluminum cement and the calcium hydroxide generated by the reaction of low-alkalinity sulfoaluminate cement and calcium sulfate also act as activators to activate volcanic ash and perlite tailings to further improve the strength of vegetation concrete.
[0033] 3. The volcanic ash in the cementitious material of the vegetation concrete of the present invention has good activity. While undergoing alkali excitation reaction, it can also provide the vegetation concrete with trace elements such as iron, aluminum, copper, zinc, magnesium, and calcium, thereby safeguarding the later growth of vegetation.
[0034] 4. The perlite tailings in the cementitious material of the vegetation concrete of the present invention, as a solid waste, has caused serious environmental pollution and ecological damage. When applied to the vegetation concrete, it can not only participate in the alkali excitation reaction and provide strength, but its internal porous structure can also effectively adsorb harmful substances such as F- and heavy metal ions together with the activated carbon component in humic acid. In addition, the presence of internal pores also increases the overall porosity of the vegetation concrete, enhances water retention and provides sufficient space for rooting, further improving the comprehensive performance of the vegetation concrete.
[0035] 5. The polyacrylamide added to the cementitious material of the vegetation concrete of the present invention can effectively regulate and improve the soil aggregate structure, eliminate soil compaction, enhance soil permeability, improve soil buffering performance, alleviate the secondary salinization of soil caused by herbicides and excessive fertilization, and the harm of continuous cropping to crops; promote the growth and development of beneficial microorganisms in the soil and improve fertilizer utilization. At the same time, polyacrylamide has a good flocculation effect and strengthens the adsorption of harmful substances in each component.
[0036] 6. The hydration products generated by the alkali-induced reaction of the vegetation concrete in the prior art will shrink greatly in the later stage, causing the vegetation concrete to crack and fall off. However, the expansion of the hydration products of the low-alkalinity sulphoaluminate cement and the water absorption expansion of the perlite tailings in the present invention can effectively compensate for the shrinkage and enhance the later performance of the vegetation concrete.
[0037] 7. The potassium sulfate and ammonium sulfate in the vegetation concrete cementitious material of the present invention can not only serve as early strength agents to enhance the early strength performance of the vegetation concrete, but also are good potassium fertilizers and nitrogen fertilizers. Combined with the nutrients in volcanic ash, modified phosphogypsum, and humic acid, no additional topdressing is required in the later stage, thereby reducing the cost of fertilization. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 This is a product diagram of modified phosphogypsum in the vegetation concrete of the present invention;
[0039] Figure 2 This is a product picture of unmodified phosphogypsum;
[0040] Figure 3 This is the planting effect of vegetation concrete with perlite tailings added;
[0041] Figure 4 This is a picture of the planting effect of vegetation concrete without adding perlite tailings;
[0042] Figure 5 This is the planting effect diagram with sufficient amount of perlite tailings and water-absorbing resin added;
[0043] Figure 6 This is the planting effect diagram when insufficient amounts of perlite tailings and water-absorbing resin are added;
[0044] Figure 7 This is a diagram of the soil structure after adding polyacrylamide;
[0045] Figure 8 This is a diagram of the soil structure without the addition of polyacrylamide. DETAILED DESCRIPTION
[0046] The following will be combined with the drawings of the present invention specification to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0047] This embodiment discloses a solid waste recycling vegetation concrete cementitious material, which is composed of sulphoaluminate cement, modified phosphogypsum, volcanic ash, perlite tailings, polyacrylamide, potassium sulfate and ammonium sulfate. The sulphoaluminate cement is low-alkalinity sulphoaluminate cement with a specific surface area of 450 m 2 / kg -550m 2 / kg, cement slurry with an ash-water ratio of 1:10, and a 1h pH value of no more than 10.3; modified phosphogypsum is prepared by washing and drying phosphogypsum to a moisture content of less than 0.5%, and then adding water-absorbing resin and humic acid to grind the specific surface area to more than 650 m2 / kg prepared.
[0048] The proportion of modified materials in the modified phosphogypsum of each embodiment is shown in Table 1 below:
[0049] Table 1 is the raw material list of phosphogypsum modified materials
[0050]
[0051] Wherein, phosphogypsum is solid waste generated in the wet phosphoric acid process, and F- is less than 1%. The water-absorbing resin is a water-absorbing resin with a water absorption rate greater than 350. The humic acid is humic acid raw powder, and the humic acid content in the humic acid raw powder is between 30% and 80%.
[0052] The raw material table of 1kg of the vegetation concrete cementitious material prepared by using the modified phosphogypsum in Table 1 above is shown in Table 2 below:
[0053] Table 2 is the raw material ratio table of each embodiment of vegetation concrete cementitious material per 1kg
[0054]
[0055] Among them, sulphoaluminate cement is low-alkalinity sulphoaluminate cement with a specific surface area of 450 m 2 / kg -550m 2 / kg, cement slurry with an ash-water ratio of 1:10, and a pH value of no more than 10.3 in 1h; the specific surface area of the volcanic ash is greater than 500 m 2 / kg; the perlite tailings are solid waste from the industrial production of perlite, with a particle size between 0.045mm and 0.075mm; the potassium sulfate, ammonium sulfate and polyacrylamide are all industrial grade; the polyacrylamide is anionic polyacrylamide.
[0056] The special cementitious materials for vegetation concrete prepared in Examples 1 to 5 in Table 2 above are prepared into vegetation concrete according to the mix ratio shown in Table 3 below, and then the 3d bulk density and porosity are tested by the ring knife method, the 3d pH value is tested by the potentiometric method, the unconfined compressive strength is tested by GB / T50123 "Standard for Geotechnical Test Methods", and the hydrolyzed nitrogen, available phosphorus and available potassium are tested by the cracking-diffusion method, the molybdenum antimony colorimetric method and the flame photometry. The test results are shown in Table 4 below.
[0057] Table 3 shows the mix ratio of vegetation concrete
[0058]
[0059] Table 4 shows the test results of the vegetation concrete prepared by the cementitious materials in each embodiment.
[0060]
[0061] The prepared vegetation concrete meets the requirements of NB / T35082-2016 "Technical Specifications for Ecological Restoration of Vegetation Concrete on Steep Slopes of Hydropower Projects".
[0062] In order to further demonstrate the benefits of the present invention, this embodiment also designs a plurality of comparative examples, and the proportions of the vegetation concrete cementitious materials of the plurality of comparative examples are shown in Table 5 below:
[0063] Table 5 shows the raw material ratio of the cementitious materials of vegetation concrete in the comparative example
[0064]
[0065] The cementitious materials in the comparative examples in Table 5 were configured according to the mix ratio in Table 3 to obtain the test data of vegetation concrete as shown in Table 6 below:
[0066] Table 6 shows the test results of vegetation concrete prepared by various comparative cementitious materials
[0067] Porosity / % <![CDATA[Bulk density (g / cm 3 )]]> PH Unconfined compressive strength MPa Hydrolyzed nitrogen (mg / kg) Available phosphorus (mg / kg) Available potassium (mg / kg) Comparative Example 1 21 2.2 9.4 0.68 53 2 102 Comparative Example 2 31 1.5 7.4 0.38 195 31 579 Comparative Example 3 22 2.2 6.7 0.46 364 87 338 Comparative Example 4 24 1.9 6.7 0.58 304 72 337
[0068] Comparative Example 1 illustrates that the combination of low-alkalinity sulfur aluminum and modified phosphogypsum can effectively reduce the pH of vegetation concrete, and perlite can not only be used as an excitation material, but also effectively increase the porosity; Comparative Example 2 illustrates that humic acid and water-absorbing resin in modified phosphogypsum are indispensable, and can effectively reduce the pH of vegetation concrete and increase the dissolution rate of phosphogypsum, increase effective phosphorus and improve strength; Comparative Example 3, combined with Comparative Example 1, further illustrates the role of perlite in increasing porosity; Comparative Example 4 illustrates the role of polyacrylamide in increasing porosity.
[0069] like Figure 1 and Figure 2 As shown, Figure 1 This is a cementitious material product obtained by modifying phosphogypsum with water-absorbing resin and humic acid. Figure 2 This is a product diagram of cementitious materials made from unmodified phosphogypsum. Figure 1 and Figure 2 It can be clearly seen that the use of modified phosphogypsum is conducive to the dispersion of cementitious materials, while the cementitious materials prepared by ordinary unmodified phosphogypsum are clumping and difficult to decompose. Figure 3 and Figure 4 The variable comparison chart of pearl tailings is added, among which, Figure 3 This is the planting effect diagram of vegetation concrete with perlite tailings added. Figure 4 This is the planting effect of vegetation concrete without adding perlite tailings. Figure 3 and Figure 4It can be seen that if perlite is not added to the cementitious material of the present application, the cementitious material is prone to shrinkage and cracking. Figure 5 The planting effect diagram of adding sufficient amount of perlite tailings and water-absorbing resin. Figure 6 This is the planting effect diagram when insufficient amounts of perlite tailings and water-absorbing resin are added. Figure 5 and Figure 6 It can be seen that when the amount of perlite tailings and water-absorbing resin added is insufficient, it will cause insufficient water retention and easily dry out the plants. Figure 7 This is the soil structure diagram after adding polyacrylamide. Figure 8 This is the soil structure diagram without adding polyacrylamide. Figure 7 and Figure 8 It can be seen that without adding polyacrylamide, the soil becomes compacted and is not suitable for plant growth.
[0070] From the above, it can be seen that in the present invention, low-alkalinity sulphoaluminate cement is selected and used in a small amount. Sulfate activation and low-alkalinity sulphoaluminate cement provide strength together. The pH value of the hydration product is low. Since substances such as humic acid and volcanic ash are weakly acidic, the pH value inside the vegetation concrete is more suitable for plant growth. In addition, low-alkalinity sulphoaluminate cement has high early strength, can prevent early sliding and provide early anti-scouring ability. Phosphogypsum, adding humic acid as antistatic and preventing the ground phosphogypsum from agglomerating, and humic acid is weakly acidic, which can neutralize the alkali produced by the hydration reaction and provide organic nutrients for vegetation growth; adding high-performance water-absorbing resin to phosphogypsum can also effectively dry the phosphogypsum to prevent agglomeration, ensure the dispersion performance of phosphogypsum, and the water-absorbing resin can play a role in water retention in vegetation concrete, reducing the cost of water spraying maintenance; the modified phosphogypsum has a large specific surface area, is not easy to agglomerate, dissolves quickly in the solution, and can well dissolve calcium sulfate to react with low-alkalinity sulfoaluminate cement to form calcium sulfate. The reaction is as follows:
[0071] 3CaO•3Al2O3•CaSO4+2CaSO4+38H2O→3CaO•Al2O3•3CaSO4•32H2O+2 (Al2O3•3H2O)
[0072] 2CaO•SiO2+nH2O→CS-H+Ca(OH)2
[0073] Al2O3•3H2O+3Ca(OH)2+3CaSO4+26H2O→3CaO•Al2O3•3CaSO4•32H2O
[0074] In addition, the rapidly decomposed sulfate, phosphoric acid and calcium hydroxide generated by the hydration reaction of low-alkalinity sulphoaluminate cement and calcium hydroxide generated by the reaction of low-alkalinity sulphoaluminate cement and calcium sulfate also act as activators to activate volcanic ash and perlite tailings to further improve the strength of vegetation concrete. Volcanic ash has good activity. While undergoing alkali activation reaction, it can also provide trace elements such as iron, aluminum, copper, zinc, magnesium, and calcium to vegetation concrete, safeguarding the growth of vegetation in the later stage.
[0075] Perlite tailings, as a solid waste, has caused serious environmental pollution and ecological damage. When applied to vegetation concrete, it can not only participate in the alkali excitation reaction and provide strength, but its internal porous structure can also effectively adsorb harmful substances such as F- and heavy metal ions together with the activated carbon component in humic acid. In addition, the presence of internal pores also improves the overall porosity of vegetation concrete, enhances water retention and provides sufficient space for rooting, further improving the comprehensive performance of vegetation concrete. Polyacrylamide can effectively regulate and improve soil aggregate structure, eliminate soil compaction, enhance soil permeability, improve soil buffering performance, alleviate the harm of soil secondary salinization caused by herbicides and excessive fertilization and continuous cropping to crops; promote the growth and development of beneficial microorganisms in the soil and improve fertilizer utilization. At the same time, polyacrylamide has a good flocculation effect and strengthens the adsorption of harmful substances in each component. The expansion of the hydration product of the low-alkalinity sulphoaluminate cement of the present invention and the water absorption and expansion of the perlite tailings can effectively compensate for the shrinkage and enhance the later performance of vegetation concrete. The potassium sulfate and ammonium sulfate in the vegetation concrete cementitious material of the present invention can not only serve as early strength agents to enhance the early strength performance of the vegetation concrete, but also are good potassium fertilizers and nitrogen fertilizers. Combined with the nutrients in volcanic ash, modified phosphogypsum, and humic acid, no additional topdressing is required in the later stage, thereby reducing the fertilization cost.
Claims
1. A solid waste recycling vegetation concrete cementitious material, characterized in that: The vegetation concrete cementitious material comprises the following raw materials in parts by mass: Sulphoaluminate cement 15-25 parts; 30-40 parts of modified phosphogypsum; 15-25 parts of volcanic ash; Perlite tailings 20-30 parts; Polyacrylamide 0.5-1 part; 0.5-1 part of potassium sulfate; 0.5-1 part of ammonium sulfate; Among them, sulphoaluminate cement is low-alkalinity sulphoaluminate cement with a specific surface area of 450 m 2 / kg -550m 2 / kg, cement slurry with a ash-water ratio of 1:10, and a pH value of no more than 10.3 in 1h; The modified phosphogypsum is prepared by washing and drying 40-60 parts of phosphogypsum until the moisture content is less than 0.5%, and then adding 1-3 parts of water-absorbing resin and 2-5 parts of humic acid and grinding until the specific surface area is greater than 650 m 2 / kg prepared.
2. The solid waste recycling vegetation concrete cementitious material according to claim 1, characterized in that: The phosphogypsum is a solid waste generated in the wet phosphoric acid process. - Less than 1%.
3. The solid waste recycling vegetation concrete cementitious material according to claim 1, characterized in that: The water-absorbing resin has a water absorption ratio greater than 350.
4. The solid waste recycling vegetation concrete cementitious material according to claim 1, characterized in that: The humic acid is humic acid raw powder, and the humic acid content in the humic acid raw powder is 30%-80%.
5. The solid waste recycling vegetation concrete cementitious material according to any one of claims 1 to 4, characterized in that: The specific surface area of the volcanic ash is greater than 500 m 2 / kg.
6. A solid waste recycling vegetation concrete cementitious material as claimed in any one of claims 1 to 4, characterized in that: The perlite tailings are solid waste from the industrial production of perlite, and have a particle size of 0.045 mm to 0.075 mm.
7. A solid waste recycling vegetation concrete cementitious material according to any one of claims 1 to 4, characterized in that: The potassium sulfate, ammonium sulfate and polyacrylamide are all of industrial grade.
8. The solid waste recycling vegetation concrete cementitious material according to any one of claims 1 to 4, characterized in that: The polyacrylamide is anionic polyacrylamide.
Citation Information
Cited By
Ecological concrete based on phosphogypsum-sulphoaluminate cement synergistic alkali reduction and preparation method thereof
CN120441269A