Preparation method of bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film

By uniformly dispersing and regularly orienting magnesium-aluminum layered double hydroxide nanosheets in the bagasse pulp regenerated cellulose film, the problem of insufficient barrier properties of the composite film is solved and a high-performance environmentally friendly packaging material is realized.

CN116120609BActive Publication Date: 2024-10-25GUANGXI UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310168378.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-27
Publication Date
2024-10-25
Estimated Expiration
2043-02-27

AI Technical Summary

Technical Problem

It is difficult to uniformly disperse and regularly orient the magnesium-aluminum layered double hydroxide nanosheets in the regenerated cellulose film with the existing technology, resulting in insufficient barrier properties of the composite film.

Method used

Through the magnesium-aluminum layered double hydroxide dispersion process, film preparation and hot-pressing treatment, the nanosheets are evenly dispersed in the bagasse pulp regenerated cellulose film and regularly oriented along the parallel direction of the film to prepare bagasse pulp regenerated cellulose/nano Layered double hydroxide composite transparent film.

Benefits of technology

The barrier properties of the regenerated cellulose film are improved, the tensile strength reaches 40.0-80.0MPa, the elongation at break is 2-8%, the water vapor transmission rate and oxygen transmission rate are within the appropriate range, and the light transmittance can reach 75.86% , suitable for environmentally friendly packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004096952320000121
    Figure BDA0004096952320000121
Patent Text Reader

Abstract

The invention discloses a preparation method of a bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film, wherein the composite transparent film is made of a bagasse pulp regenerated cellulose substrate doped with a magnesium aluminum layered double hydroxide nanosheet, and the preparation process includes three steps, firstly dispersing the magnesium aluminum layered double hydroxide nanosheet in a mixed solution of an ionic liquid and ethanol, then dissolving the bagasse pulp cellulose using an ionic liquid 1-allyl-3-methylimidazole chloride, finally uniformly mixing the magnesium aluminum layered double hydroxide nanosheet dispersion with the bagasse pulp cellulose solution, washing and drying in a coagulation bath to form a film, and finally preparing the composite transparent film by heating and pressurizing a flat vulcanizing agent. Through this process, the layered double hydroxide nanosheets are uniformly dispersed in the regenerated cellulose film and are regularly oriented in a direction parallel to the film, resulting in a smaller gas permeable area and a longer gas permeation path, which helps to improve the barrier performance of the regenerated cellulose film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of degradable high-barrier transparent packaging materials, and in particular relates to a method for preparing a bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film. Background Art

[0002] The use of non-biodegradable and non-renewable materials in packaging applications has raised concerns about environmental pollution. Traditional methods of dealing with post-consumer plastic waste include incineration and landfill, which pose a threat to our health and the environment. Research has been conducted to develop alternative petroleum-based packaging materials to reduce their adverse effects, among which biopolymer-based materials have been widely studied. Due to their biodegradability, they can minimize the generation of packaging waste, thereby solving the waste disposal problem to a certain extent.

[0003] Cellulose from natural resources is considered to be the most abundant and renewable polymer material and a key source of sustainable materials on an industrial scale. Guangxi is rich in sugarcane resources, which can provide strong raw material support for the development of the functional cellulose industry using bagasse as raw materials. Regenerated cellulose materials can be directly prepared from cellulose through physical dissolution, molding and regeneration processes, and have attracted attention due to their advantages such as easy manufacturing, biocompatibility, biodegradability, and chemical stability. In recent years, research on the high-value utilization of cellulose has emerged in an endless stream. Improving the high barrier properties of regenerated cellulose films can greatly broaden their applications in various fields.

[0004] Adding nanofillers to the film matrix can effectively improve the barrier properties of the composite film. Magnesium aluminum layered double hydroxide (Mg / Al-LDH) is a type of inorganic material with a lamellar structure, which is composed of metal layers and interlayer anions and water molecules in an orderly manner. It has been approved by regulators as a drug and food contact material. Due to its nano-size and high aspect ratio, it is often blended with polymers to prepare multifunctional composite materials. However, current methods pay less attention to the dispersion and arrangement of nanomaterials in polymers, so a practical preparation process is needed to solve the above problems. Summary of the invention

[0005] In order to solve the two problems of uniform dispersion process and regular orientation of magnesium-aluminum layered double hydroxide nanosheets in regenerated cellulose film, the present invention provides a method for preparing a composite transparent film of bagasse pulp regenerated cellulose / nano layered double hydroxide, so as to improve the barrier performance of the regenerated cellulose film. While achieving the established goals, the method pursues simple process, energy saving and efficiency improvement, in order to provide certain technical support for the high-value utilization of cellulose.

[0006] To achieve the above object, the present invention proposes the following technical solutions:

[0007] A method for preparing a bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film, wherein the nanosheets are uniformly dispersed in the bagasse pulp regenerated cellulose film and are regularly oriented in a direction parallel to the film through a magnesium aluminum layered double hydroxide dispersion process, film preparation and hot pressing treatment, thereby preparing the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film.

[0008] Furthermore, the preparation method specifically comprises the following steps:

[0009] 1) Preparation of magnesium aluminum layered double hydroxide nanosheet dispersion

[0010] Dispersing magnesium aluminum layered double hydroxide in a solvent, mixing the obtained magnesium aluminum layered double hydroxide dispersion with ionic liquid 1-allyl-3-methylimidazolium chloride, performing ultrasonic treatment and mechanical stirring alternately, heating and removing ethanol after mixing, and obtaining a magnesium aluminum layered double hydroxide nanosheet dispersion;

[0011] 2) Preparation of bagasse pulp cellulose solution

[0012] The bagasse pulp board raw material is ball-milled, and the obtained bagasse pulp cellulose powder is mixed with the ionic liquid 1-allyl-3-methylimidazolium chloride, stirred evenly and then sealed, left to swell at room temperature, and then stirred and dissolved under stage heating;

[0013] 3) Preparation of bagasse pulp regenerated cellulose / nano-layered double hydroxide composite transparent film

[0014] The magnesium aluminum layered double hydroxide nanosheet dispersion is added to the bagasse pulp cellulose solution, heated and stirred, centrifuged, and then coated on a glass plate with a scraper. After cooling to room temperature, the glass plate containing the solution is placed in a coagulation bath to form a hydrogel, placed in flowing water to remove the ionic liquid, eluted, dried, and finally heated and pressurized in a flat vulcanizer.

[0015] Furthermore, in step 1), the magnesium aluminum layered double hydroxide has a lateral dimension of 400 nm and a thickness of 30 nm; the mass fraction of the magnesium aluminum layered double hydroxide in the ionic liquid 1-allyl-3-methylimidazolium chloride is 2-15%; and the solvent is ethanol.

[0016] Furthermore, in step 1), the ultrasonic treatment parameters are: ultrasonic power is 100-200 W, and the time is 20 min; the mechanical stirring parameters are: temperature is 25-50° C., and the time is 40 min; and the number of alternations is 3-6 times.

[0017] Furthermore, in step 2), the particle size of the bagasse pulp cellulose powder is 60 μm; the mass fraction of the bagasse pulp cellulose powder in the ionic liquid 1-allyl-3-methylimidazolium chloride is 1-15%; the swelling time is 1-2 hours; the stage heating specifically refers to: the heating temperature of the first stage is 45-65°C, the time is 1-3 hours, the heating temperature of the second stage is 70-100°C, the time is 1-3 hours, and the total dissolution time is 3-8 hours.

[0018] Furthermore, in step 3), the mass fraction of magnesium aluminum layered double hydroxide in the magnesium aluminum layered double hydroxide nanosheet dispersion to fiber in bagasse pulp cellulose solution is 1-50%; the heating and stirring temperature is 60-80° C., and the time is 0.5-2 h.

[0019] Furthermore, in step 3), the centrifugal speed is 3000-7000rpm, the centrifugal time is 1-10min; the scraper thickness is 500-3000μm; the coating speed is 1-5mm / s; the drying temperature is 50-80℃; the heating and pressurizing treatment parameters are: temperature 80-120℃, pressure 4-10MPa, time 1-10h.

[0020] Furthermore, in step 3), the scraper and the glass plate need to be preheated before coating, and the preheating temperature is 60° C.; and the acid solution is a 0.05 mol / L tartaric acid solution.

[0021] The present invention also provides a bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film prepared by the preparation method.

[0022] The invention also provides an application of the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film in packaging materials.

[0023] The composite film prepared by the present invention has the following characteristics:

[0024] 1) The base material of the composite film is bagasse pulp regenerated cellulose, which has the advantages of being non-toxic, environmentally friendly, and biodegradable under natural conditions. It has high transparency, excellent mechanical properties and film-forming properties. The addition of nanosheets improves the barrier properties of the film and is effectively used in environmentally friendly packaging materials.

[0025] 2) Under the preparation process conditions of the present invention, the prepared bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film has a tensile strength of 40.0-80.0 MPa, an elongation at break of about 2-8%, and a water vapor permeability of 300-650 g·m -2 ·24h -1 , the oxygen permeability of the membrane is 8.0-30.0cm 3 ·m-2 ·24h -1 , the light transmittance can reach 75.86%.

[0026] 3) Using layered double hydroxide nanosheets with a high aspect ratio as filler, this process allows them to be evenly dispersed in the regenerated cellulose film and regularly oriented along the parallel direction of the film. The highly oriented layered double hydroxide can produce a smaller gas permeable area and a longer gas permeation path, which helps to improve the barrier properties of the regenerated cellulose film. DETAILED DESCRIPTION

[0027] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0028] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0029] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0030] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0031] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0032] The "room temperature" mentioned in the present invention is 25±2°C unless otherwise specified.

[0033] The raw material magnesium aluminum layered double hydroxide used in the present invention was purchased from Aladdin Mall. The bagasse pulp board raw material was purchased from a pulping company in Guangxi. The raw material ionic liquid 1-allyl-3-methylimidazolium chloride was purchased from Aladdin Mall.

[0034] A method for preparing a bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film, wherein the nanosheets are uniformly dispersed in the bagasse pulp regenerated cellulose film and are regularly oriented in a direction parallel to the film through a magnesium aluminum layered double hydroxide dispersion process, film preparation and hot pressing treatment, thereby preparing the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film.

[0035] In some preferred embodiments, the preparation method specifically comprises the following steps:

[0036] 1) Preparation of magnesium aluminum layered double hydroxide nanosheet dispersion

[0037] The magnesium aluminum layered double hydroxide is dispersed in a solvent, and the obtained magnesium aluminum layered double hydroxide dispersion is mixed with the ionic liquid 1-allyl-3-methylimidazolium chloride, and ultrasonic treatment and mechanical stirring are performed alternately. After the mixture is evenly mixed, the mixture is placed in a vacuum oven to remove ethanol, and then taken out and placed in a sample bottle for use;

[0038] 2) Preparation of bagasse pulp cellulose solution

[0039] The bagasse pulp board raw material is subjected to ball milling treatment, and the obtained bagasse pulp cellulose powder is mixed with the ionic liquid 1-allyl-3-methylimidazolium chloride and put into a conical flask, stirred evenly with a glass rod, and then the bottle cap is covered and sealed, and the mixture is left to swell at room temperature, and then the conical flask is placed in an oil bath pot and dissolved by magnetic stirring in stages according to the heating temperature;

[0040] 3) Preparation of bagasse pulp regenerated cellulose / nano-layered double hydroxide composite transparent film

[0041] A magnesium aluminum layered double hydroxide nanosheet dispersion is added to a bagasse pulp cellulose solution, heated and stirred until the mixture is uniformly mixed, the mixed solution is centrifuged using a centrifuge to remove bubbles and impurities, and then coated on a glass plate using a scraper through an automatic coating machine, and the scraper and the glass plate are preheated at 60°C before coating; after cooling to room temperature, the glass plate containing the solution is placed in a de-tartaric acid solution to construct a coagulation bath, and after a hydrogel is formed, it is placed in running water to remove all ionic liquids, and the washed cellulose gel film is dried in a blast drying oven to obtain a regenerated cellulose film, which is then heated and pressurized in a flat vulcanizer, and the treated composite transparent film is placed in a 23°C, 50% RH climate box for storage for later use.

[0042] In some preferred embodiments, in step 1), the average lateral size of the magnesium-aluminum layered double hydroxide is 400 nm, and the average thickness is 30 nm; the mass fraction of the magnesium-aluminum layered double hydroxide in the ionic liquid 1-allyl-3-methylimidazolium chloride is 2-15%, preferably 5%, 8%, 10%; the solvent is anhydrous ethanol, and the ratio of ethanol to magnesium-aluminum layered double hydroxide is 3 mL:2 g.

[0043] In some preferred embodiments, in step 1), the ultrasonic treatment parameters are: ultrasonic power is 100-200 W, preferably 100 W, 150 W, 200 W, and the time is 20 min; the mechanical stirring parameters are: temperature is 25-50°C, preferably 25°C, 40°C, 50°C, and the time is 40 min; the number of alternations is 3-6 times, preferably 3 times, 4 times, and 6 times.

[0044] In some preferred embodiments, in step 2), the average particle size of the bagasse pulp cellulose powder is 60 μm; the mass fraction of the bagasse pulp cellulose powder to the ionic liquid 1-allyl-3-methylimidazolium chloride is 1-15%, preferably 5%, 7%, 10%.

[0045] In some preferred embodiments, in step 2), the swelling time is 1-2h, preferably 1h, 1.5h, 2h; the stage heating specifically refers to: the heating temperature in the first stage is 45-65°C, preferably 45°C, 50°C, 55°C, and the time is 1-3h, preferably 1h, 2h, 3h; the heating temperature in the second stage is 70-100°C, preferably 85°C, 90°C, 95°C, and the time is 1-3h, preferably 1h, 2h, 3h, and the dissolution time is 3-8h.

[0046] In some preferred embodiments, in step 3), the mass fraction of magnesium aluminum layered double hydroxide in the magnesium aluminum layered double hydroxide nanosheet dispersion to the fiber in the bagasse pulp cellulose solution is 1-50%, preferably 5%, 10%, 20%; the heating and stirring temperature is 60-80°C, preferably 65°C, 70°C, 80°C, and the time is 0.5-2h, preferably 30min, 50min, 70min.

[0047] In some preferred embodiments, in step 3), the centrifugal speed is 3000-7000rpm, preferably 3000rpm, 5000rpm, 7000rpm, the centrifugal time is 1-10min, preferably 5min, 6min, 7min; the scraper thickness is 500-3000μm, preferably 1000μm, 1500μm, 2000μm; the coating speed is 1-5mm / s, preferably 1mm / s, 2mm / s, 3mm / s; the drying temperature is 50-80℃, preferably 55℃, 60℃, 65℃; the heating and pressurization treatment parameters are: temperature 80-120℃, preferably 80℃, 90℃, 100℃; pressure 4-10MPa, preferably 6MPa, 8MPa, 9MPa; time 1-10h, preferably 3h, 5h, 6h.

[0048] In some preferred embodiments, in step 3), the scraper and the glass plate need to be preheated before coating, and the preheating temperature is 60° C.; and the acid solution is a 0.05 mol / L tartaric acid solution.

[0049] The present invention also provides a bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film prepared by the preparation method.

[0050] The invention also provides an application of the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film in packaging materials.

[0051] The invention provides a method for preparing a composite transparent film of bagasse pulp regenerated cellulose / nano layered double hydroxide. The composite transparent film is made of bagasse pulp regenerated cellulose substrate doped with magnesium aluminum layered double hydroxide nanosheets. The preparation process includes three steps. First, the magnesium aluminum layered double hydroxide nanosheets are dispersed in a mixed solution of ionic liquid and ethanol. Then, the bagasse pulp cellulose is dissolved by using ionic liquid 1-allyl-3-methylimidazolium chloride. Finally, the magnesium aluminum layered double hydroxide nanosheet dispersion is uniformly mixed with the bagasse pulp cellulose solution. The film is washed and dried in a coagulation bath. Finally, the composite transparent film is prepared by heating and pressurizing with a flat vulcanizing agent. Through this process, the layered double hydroxide nanosheets are uniformly dispersed in the regenerated cellulose film and are regularly oriented in the parallel direction of the film, resulting in a smaller gas permeable area and a longer gas permeation path, which is helpful to improve the barrier performance of the regenerated cellulose film.

[0052] The technical solution of the present invention is further illustrated by the following examples.

[0053] The bagasse pulp board in the embodiment of the present invention is commercially available.

[0054] Example 1

[0055] 1) 2.0 g of magnesium aluminum layered double hydroxide (average lateral size of 400 nm, average thickness of 30 nm) and 3 mL of anhydrous ethanol (concentration of 99.7%) were mixed together, and after stirring evenly, 40.0 g of ionic liquid 1-allyl-3-methylimidazolium chloride was added, and mechanical stirring was first performed at 40° C. for 40 min, followed by ultrasonic treatment at 100 W for 20 min, and the two treatments were performed alternately for 4 times. After mixing evenly, the mixture was placed in a vacuum oven for 24 h to remove ethanol, thereby obtaining a magnesium aluminum layered double hydroxide nanosheet dispersion, which was stored for later use.

[0056] 2) Tear the bagasse pulp into small pieces, take 20.0g of the pieces and put them into a multifunctional pulverizer for mechanical pulverization for 2min, then put 20.0g of flocculent fibers into a 250mL zirconia ball milling jar and use a planetary ball mill to perform ball milling at a speed of 300rpm for 10h. After the ball milling, take out the bagasse pulp fiber powder (average particle size of 60μm) and place it in a 60℃ forced air drying oven for drying for 24h and store it for future use.

[0057] Take 2.0g of ball-milled bagasse pulp fiber powder and 40.0g of ionic liquid 1-allyl-3-methylimidazolium chloride and add them to a 150mL conical flask. Stir evenly with a glass rod and seal the bottle cap. Let it swell at room temperature for 1h. Then put the conical flask into a 50℃ oil bath and heat with magnetic stirring to dissolve for 2h. Then raise the temperature of the oil bath to 90℃ and continue stirring and dissolving for 2h to obtain a bagasse pulp cellulose solution.

[0058] 3) Add 2.0g of magnesium aluminum layered double hydroxide nanosheet dispersion to 42.0g of bagasse pulp cellulose solution, stir and mix at 70°C for 30min, then use a centrifuge to remove bubbles and impurities from the mixed solution, the centrifuge speed is set to 5000rpm, and the time is 5min. Then, the automatic coating machine is used to coat the glass plate at a speed of 1mm / s, the scraper thickness is set to 1500μm, and the scraper and glass plate are preheated at 60°C before coating. After cooling to room temperature, the glass plate containing the solution is placed in a 0.05mol / L tartaric acid solution to construct a coagulation bath, and after forming a hydrogel, it is placed in running water for 24h to remove the ionic liquid. The washed cellulose gel film was dried in a 55°C forced air drying oven for 30 min to obtain a regenerated cellulose film, which was then pressure treated in a flat vulcanizer at 90°C and 8 MPa for 5 h. The treated bagasse pulp regenerated cellulose / nano-layered double hydroxide composite transparent film was stored in a 23°C, 50% RH climate chamber.

[0059] Example 2

[0060] 1) 4.0 g of magnesium aluminum layered double hydroxide (average lateral size of 400 nm, average thickness of 30 nm) and 6 mL of anhydrous ethanol (concentration of 99.7%) were mixed together, and after stirring evenly, 50.0 g of ionic liquid 1-allyl-3-methylimidazolium chloride was added, and mechanical stirring was first performed at 25° C. for 40 min, followed by ultrasonic treatment at 150 W for 20 min, and the two treatments were alternately performed 6 times. After mixing evenly, the mixture was placed in a vacuum oven for 24 h to remove ethanol, thereby obtaining a magnesium aluminum layered double hydroxide nanosheet dispersion, which was stored for later use.

[0061] 2) Tear the bagasse pulp into small pieces, take 20.0g of the pieces and put them into a multifunctional pulverizer for mechanical pulverization for 2min, then put 20.0g of flocculent fibers into a 250mL zirconia ball milling jar and use a planetary ball mill to perform ball milling at a speed of 300rpm for 10h. After the ball milling, take out the bagasse pulp fiber powder (average particle size of 60μm) and place it in a 60℃ forced air drying oven for drying for 24h for storage.

[0062] Take 2.5g of ball-milled bagasse pulp fiber powder and 35.0g of ionic liquid 1-allyl-3-methylimidazolium chloride and add them to a 150mL conical flask. Stir evenly with a glass rod and seal the bottle cap. Let it swell at room temperature for 1.5h. Then put the conical flask into a 55℃ oil bath and heat with magnetic stirring to dissolve for 1h. Then raise the temperature of the oil bath to 95℃ and continue stirring and dissolving for 2h to obtain a bagasse pulp cellulose solution.

[0063] 3) Add 3.8g of magnesium aluminum layered double hydroxide nanosheet dispersion to 37.5g of bagasse pulp cellulose solution, stir and mix at 65°C for 50min, then use a centrifuge to remove bubbles and impurities from the mixed solution, the centrifuge speed is set to 3000rpm, and the time is 7min. Then, the automatic coating machine is used to coat the glass plate at a speed of 2mm / s, the scraper thickness is set to 2000μm, and the scraper and glass plate are preheated at 60°C before coating. After cooling to room temperature, the glass plate containing the solution is placed in a 0.05mol / L tartaric acid solution to construct a coagulation bath, and after forming a hydrogel, it is placed in running water for 24h to remove the ionic liquid. The washed cellulose gel film was dried in a 60°C forced air drying oven for 30 min to obtain a regenerated cellulose film, which was then pressure treated in a flat vulcanizer at 80°C and 9 MPa for 6 h. The treated bagasse pulp regenerated cellulose / nano-layered double hydroxide composite transparent film was stored in a 23°C, 50% RH climate chamber.

[0064] Example 3

[0065] 1) 10.0 g of magnesium aluminum layered double hydroxide (average lateral size of 400 nm, average thickness of 30 nm) and 15 mL of anhydrous ethanol (concentration of 99.7%) were mixed together, and after being stirred evenly, 100.0 g of ionic liquid 1-allyl-3-methylimidazolium chloride was added, and mechanical stirring was first performed at 50° C. for 40 min, followed by ultrasonic treatment at 200 W for 20 min, and the two treatments were performed alternately for 3 times. After being mixed evenly, the mixture was placed in a vacuum oven for 24 h to remove ethanol, thereby obtaining a magnesium aluminum layered double hydroxide nanosheet dispersion, which was stored for later use.

[0066] 2) Tear the bagasse pulp into small pieces, take 20.0g of the pieces and put them into a multifunctional pulverizer for mechanical pulverization for 2min, then put 20.0g of flocculent fibers into a 250mL zirconia ball milling jar and use a planetary ball mill to perform ball milling at a speed of 300rpm for 10h. After the ball milling, take out the bagasse pulp fiber powder (average particle size of 60μm) and place it in a 60℃ forced air drying oven for drying for 24h for storage.

[0067] Take 5.0g of ball-milled bagasse pulp fiber powder and 50g of ionic liquid 1-allyl-3-methylimidazolium chloride and add them to a 250mL conical flask. Stir evenly with a glass rod and seal the bottle cap. Let it swell at room temperature for 2h. Then put the conical flask into a 45℃ oil bath and heat with magnetic stirring to dissolve for 3h. Then raise the temperature of the oil bath to 85℃ and continue stirring and dissolving for 3h to obtain a bagasse pulp cellulose solution.

[0068] 3) 11.0g of magnesium aluminum layered double hydroxide nanosheet dispersion was added to 55g of bagasse pulp cellulose solution, stirred and mixed at 80°C for 70min, and then the mixed solution was centrifuged to remove bubbles and impurities, the centrifuge speed was set to 7000rpm, and the time was 6min. Then the automatic coating machine was used to coat the glass plate at a speed of 3mm / s, the scraper thickness was set to 1000μm, and the scraper and glass plate were preheated at 60°C before coating. After cooling to room temperature, the glass plate containing the solution was placed in a 0.05mol / L tartaric acid solution to construct a coagulation bath, and after forming a hydrogel, it was placed in running water for 24h to remove the ionic liquid. The washed cellulose gel film was dried in a 65°C forced air drying oven for 30 min to obtain a regenerated cellulose film, which was then pressure treated in a flat vulcanizer at 100°C and 6 MPa for 3 h. The treated bagasse pulp regenerated cellulose / nano-layered double hydroxide composite transparent film was stored in a 23°C, 50% RH climate chamber.

[0069] Comparative Example 1

[0070] The same as Example 1, except that, in step 1), only mechanical stirring is performed during the preparation of the magnesium aluminum layered double hydroxide nanosheet dispersion, and no ultrasonic treatment is performed.

[0071] Comparative Example 2

[0072] Same as Example 1, except that no ethanol is added in step 1).

[0073] Comparative Example 3 (no swelling and no stage heating)

[0074] The same as Example 1, except that the preparation step of the bagasse pulp cellulose solution in step 2) is as follows: 2.0 g of ball-milled bagasse pulp fiber powder and 40.0 g of ionic liquid 1-allyl-3-methylimidazolium chloride are added to a 150 mL conical flask, stirred evenly with a glass rod, and then the bottle cap is covered and sealed, and then the conical flask is placed in a 90° C. oil bath pot and heated with magnetic stirring for dissolution for 5 hours to obtain a bagasse pulp cellulose solution.

[0075] Comparative Example 4

[0076] The same as Example 1, except that the regenerated cellulose film prepared in step 3) is not subjected to heating and pressurizing treatment in a flat vulcanizer.

[0077] Test Example 1

[0078] The performance of the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent films prepared in Examples 1-3 and Comparative Examples 1-4 of the present invention were tested according to ASTM D882-12, GB / T 1037-1988 and GB / T 19789-2005. The results are shown in Table 1.

[0079] Table 1 Performance test results of different composite membranes

[0080]

[0081] As can be seen from Table 1, the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film prepared by the present invention has a tensile strength of 40.0-80.0 MPa, an elongation at break of about 2-8%, and a water vapor permeability of 300-650 g·m -2 ·24h -1 , the oxygen permeability of the membrane is 8.0-30.0cm 3 ·m -2 ·24h -1 , the light transmittance can reach 75.86%.

[0082] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film, characterized in that: The following steps are involved: 1) Preparation of magnesium aluminum layered double hydroxide nanosheet dispersion The magnesium aluminum layered double hydroxide is dispersed in anhydrous ethanol, and the obtained magnesium aluminum layered double hydroxide dispersion is mixed with the ionic liquid 1-allyl-3-methylimidazolium chloride, and ultrasonic treatment and mechanical stirring are performed alternately. After mixing, the ethanol is removed by heating to obtain a magnesium aluminum layered double hydroxide nanosheet dispersion; 2) Preparation of bagasse pulp cellulose solution The bagasse pulp board raw material is ball-milled, and the obtained bagasse pulp cellulose powder is mixed with the ionic liquid 1-allyl-3-methylimidazolium chloride, stirred evenly and then sealed, left to swell at room temperature, and then stirred and dissolved under stage heating; 3) Preparation of bagasse pulp regenerated cellulose / nano-layered double hydroxide composite transparent film The magnesium aluminum layered double hydroxide nanosheet dispersion is added to the bagasse pulp cellulose solution, heated and stirred, centrifuged, and then coated on a glass plate with a scraper. After cooling to room temperature, the glass plate containing the solution is placed in an acid solution to form a coagulation bath. After the hydrogel is formed, it is placed in running water to remove all the ionic liquid, eluted, dried, and finally heated and pressurized in a flat vulcanizer; In step 2), the swelling time is 1-2 hours; the stage heating specifically refers to: the first stage heating temperature is 45-65°C, the time is 1-3 hours, the second stage heating temperature is 70-100°C, the time is 1-3 hours, and the total dissolution time is 3-8 hours.

2. The method for preparing the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film according to claim 1, characterized in that: In step 1), the magnesium aluminum layered double hydroxide has a lateral dimension of 400 nm and a thickness of 30 nm; the mass fraction of the magnesium aluminum layered double hydroxide in the ionic liquid 1-allyl-3-methylimidazolium chloride is 2-15%.

3. The method for preparing the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film according to claim 1, characterized in that: In step 1), the ultrasonic treatment parameters are: ultrasonic power is 100-200W, and the time is 20 minutes; the mechanical stirring parameters are: temperature is 25-50°C, and the time is 40 minutes; and the number of alternations is 3-6 times.

4. The method for preparing the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film according to claim 1, characterized in that: In step 2), the particle size of the bagasse pulp cellulose powder is 60 μm; the mass fraction of the bagasse pulp cellulose powder to the ionic liquid 1-allyl-3-methylimidazolium chloride is 1-15%.

5. The method for preparing the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film according to claim 1, characterized in that: In step 3), the mass fraction of magnesium aluminum layered double hydroxide in the magnesium aluminum layered double hydroxide nanosheet dispersion to fiber in bagasse pulp cellulose solution is 1-50%; the heating and stirring temperature is 60-80° C., and the time is 0.5-2 h.

6. The method for preparing the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film according to claim 1, characterized in that: In step 3), the centrifugal speed is 3000-7000rpm, the centrifugal time is 1-10min; the scraper thickness is 500-3000μm; the coating speed is 1-5mm / s; the drying temperature is 50-80℃; the heating and pressurizing treatment parameters are: temperature 80-120℃, pressure 4-10MPa, time 1-10h.

7. The method for preparing the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film according to claim 1, characterized in that: In step 3), the scraper and the glass plate need to be preheated before coating, and the preheating temperature is 60° C.; the acid solution is a 0.05 mol / L tartaric acid solution.

8. A bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film prepared by the preparation method according to any one of claims 1 to 7.

9. Use of the bagasse pulp regenerated cellulose / nano layered double hydroxide composite transparent film as claimed in claim 8 in packaging materials.

Citation Information

Patent Citations

  • Titanium containing cellulose / LDHs (Layered Double Hydroxides) nanocomposite as well as preparation method and application thereof

    CN102583621A

  • Nano-crystalline cellulose / layered double hydroxide composite membrane and preparation method

    CN105058913A

  • Bagasse-based nano antibacterial fresh-keeping film and preparation method thereof

    CN108384064A

  • Nano cellulose membrane with better photo-thermal stability

    CN111848996A