A kind of dealcoholization type organosilicon sealant and preparation method thereof

By using α,ω-dihydroxypolydimethylsiloxane and a coupling agent for condensation reaction in the dealcoholized silicone sealant, combined with fillers, plasticizers and catalysts, the problem of reduced storage stability of the sealant is solved. , achieving high stability and improved moisture and heat resistance, avoiding an increase in process steps and performance degradation.

CN116144315BActive Publication Date: 2024-10-18HUBEI XINGRUI SILICON MATERIAL CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202211584794.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-11
Publication Date
2024-10-18
Estimated Expiration
2042-12-11

AI Technical Summary

Technical Problem

During the storage process, the curing performance of dealcoholized silicone sealant decreases due to the reaction between trace amounts of moisture and free alcohols and polysiloxane. The existing technology adds process steps or uses stabilizers with limited effects, resulting in a decrease in performance. It is necessary to seek to avoid increasing the Methods to improve the stability of process steps.

Method used

Using a combination of α,ω-dihydroxypolydimethylsiloxane, fillers, plasticizers, cross-linking agents, coupling agents, catalysts and stabilizers, the coupling agent and α,ω-dihydroxypolydimethylsiloxane are The siloxane undergoes a condensation reaction, reducing the silanol content and improving the storage stability of the sealant.

Benefits of technology

Through the condensation reaction, the reaction between free alcohol and polysiloxane is reduced, which effectively improves the storage stability of the sealant, reaching a stability of more than 12 months, improving the heat-humidity resistance bonding performance, without adding process steps and reducing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116144315B_ABST
    Figure CN116144315B_ABST
Patent Text Reader

Abstract

The present application relates to the technical field of adhesives, and in particular to a dealcoholized silicone sealant and a preparation method thereof. The silicone sealant provided in the present application is prepared using α, ω-dihydroxy polydimethylsiloxane, a filler, a plasticizer, a crosslinking agent, a coupling agent, a catalyst and a stabilizer; wherein the coupling agent has a plurality of alkoxy groups that undergo condensation reactions with the hydroxyl groups of α, ω-dihydroxy polydimethylsiloxane. The raw material combination of the dealcoholized silicone sealant provided in the present application does not require modification of α, ω-dihydroxy polydimethylsiloxane to achieve the improvement of the storage stability of the sealant, and the storage stability can reach more than 12 months.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of adhesives, and in particular to a dealcoholized organic silicon sealant and a preparation method thereof. Background Art

[0002] Dealcoholized silicone sealants have the advantages of being non-corrosive to the bonding substrate and having no irritating odor, and are widely used in the photovoltaic and electrical and electronic industries. During the storage of dealcoholized silicone sealants, the trace moisture and free alcohol contained in them react with polysiloxane in the presence of an organic metal catalyst to undergo chain scission and equilibrium reactions to form short-chain (CH3O)(CH3)2SiO 1 / 2 The products such as end groups make its curing performance and physical properties gradually decline or even disappear as the storage time increases. In the prior art, the following two methods are mainly used to improve the storage stability of dealcoholized silicone sealants: 1. Alkoxy end-capping modification of the base polymer α,ω-dihydroxy polydimethylsiloxane; 2. Adding a hydroxyl scavenger as a stabilizer, generally using nitrogen silane, molecular sieve, calcium chloride, etc. Although the first method can better solve the storage stability problem, it requires additional process steps, resulting in increased costs; the second method has limited effect and will cause a decline in other properties.

[0003] Based on the above analysis, it is very important to provide a raw material combination that can improve the storage stability of dealcoholized silicone sealant without adding process steps. Summary of the invention

[0004] The embodiment of the present application provides a dealcoholized silicone sealant to solve the problem in the related art of improving the storage stability of silicone sealants by adding process steps.

[0005] In a first aspect, the present application provides a dealcoholized silicone sealant prepared using α, ω-dihydroxypolydimethylsiloxane, a filler, a plasticizer, a cross-linking agent, a coupling agent, a catalyst and a stabilizer; wherein the coupling agent has an alkoxy group that undergoes a condensation reaction with the hydroxyl group of the α, ω-dihydroxypolydimethylsiloxane.

[0006] In some embodiments, the weight proportions of the raw materials are: 100 parts of α, ω-dihydroxypolydimethylsiloxane, 60-150 parts of filler, 5-40 parts of plasticizer, 2-15 parts of crosslinking agent, 0.5-8 parts of coupling agent, 1-10 parts of catalyst, and 0.1-5 parts of stabilizer.

[0007] In some embodiments, the structural formula of α,ω-dihydroxy polydimethylsiloxane is:

[0008]

[0009] Wherein, n is a positive integer which makes the kinematic viscosity of α,ω-dihydroxypolydimethylsiloxane 1000-200000 mPa·S at 25°C; and R is methyl, phenyl or vinyl.

[0010] In some preferred embodiments, R is methyl.

[0011] In some preferred embodiments, the kinematic viscosity of α,ω-dihydroxypolydimethylsiloxane at 25° C. is 5000-80000 mPa·S.

[0012] In some embodiments, the coupling agent includes an α-coupling agent trimer, and the structural formula of the α-coupling agent trimer is:

[0013]

[0014] In the formula, R1, R2, and R3 are independently C1-C4 alkyl groups, and R1, R2, and R3 can be the same group or different groups. The functional group of the α-coupling agent trimer is only one carbon atom away from the silicon atom and is very close to each other, so the electronic effect on the functional group is more easily transferred to the silicon atom, making the alkoxy group directly connected to the silicon atom extremely active, and easily undergoing condensation reaction with the silanol to remove the alcohol, so that the silanol content in the system is reduced, and the storage stability of the sealant is improved; in addition, because the molecular structure contains a special nitrogen-containing heterocyclic structure, it can improve the sealant's resistance to moisture and heat adhesion to various substrates such as aluminum, copper, polycarbonate, PPO, and ABS.

[0015] In some preferred embodiments, R1, R2, and R3 are each independently methyl or ethyl.

[0016] In some embodiments, the coupling agent further comprises a mixture of one or more of aminopropyltrimethoxysilane, aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-methacryloyloxypropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, isocyanatepropyltrimethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, N,N-diethyl-3-aminopropyltrimethoxysilane, bis-[3-(methoxysilyl)-propyl]-amine and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

[0017] In some preferred embodiments, the coupling agent includes aminopropyltriethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane or corresponding hydrolyzed copolymers.

[0018] In some embodiments, the mass amount of the α-coupling agent trimer accounts for 20%-80% of the total mass of the coupling agent.

[0019] In some embodiments, the plasticizer includes hydroxyl-terminated polybutadiene and polydimethylsiloxane, and the kinematic viscosity of polydimethylsiloxane at 25°C is 100-1000mPa·S. The viscosity of hydroxyl-terminated polybutadiene is 100-1000mPa·S, and the molecule of polybutadiene is a directional stereostructure. The outer periphery of the molecular structure is terminated by active hydroxyl groups, which can form chemical bonds with α, ω-dihydroxy polydimethylsiloxane to improve the mechanical properties of the sealant; polybutadiene itself has a low moisture permeability, so after complete curing, it can effectively improve the high temperature and high humidity resistance of the sealant.

[0020] In some embodiments, the mixing mass ratio of the hydroxyl-terminated polybutadiene and polydimethylsiloxane is 1:5-5:1.

[0021] In some embodiments, the filler is a mixture of one or more of nano calcium carbonate, silicon powder, fumed silica, light calcium carbonate and heavy calcium carbonate; the nano calcium carbonate is active nano calcium carbonate surface treated with stearic acid, and has an average particle size of 50-100 nm.

[0022] In some embodiments, the crosslinking agent is a mixture of one or more of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, isopropyltrimethoxysilane, isopropyltriethoxysilane, phenyltrimethoxyphenyltriethoxysilane, methyl orthosilicate, and ethyl orthosilicate.

[0023] In some embodiments, the catalyst is a mixture of one or more of n-butyl titanate, tetraisobutyl titanate, n-propyl titanate, tetraisopropyl titanate, tert-butyl titanate and a titanium complex of ethyl acetoacetate.

[0024] In some embodiments, the stabilizer is a mixture of one or more of hexamethyldisilazane, hexamethylcyclotrisilylazane, isocyanatepropyltrimethoxysilane, divinyltetramethoxydisilazane, calcium chloride, magnesium chloride, zeolite, and molecular sieve.

[0025] In some preferred embodiments, the stabilizer is divinyltetramethoxydisilazane or hexamethyldisilazane.

[0026] In a second aspect, the present invention also provides a method for preparing the above-mentioned dealcoholization type silicone sealant, comprising the following steps:

[0027] α,ω-dihydroxy polydimethylsiloxane, a plasticizer and a filler are mixed, heated and vacuumized to obtain a mixed base material;

[0028] Add a crosslinking agent, a coupling agent, a catalyst and a stabilizer to the mixed base material in sequence, and evacuate the mixture to obtain a dealcoholized organic silicone sealant.

[0029] The beneficial effects brought about by the technical solution provided by the present application include: the alkoxy group contained in the coupling agent in the raw material combination of the dealcoholized silicone sealant provided by the present application can undergo a condensation reaction with the silanol group of α, ω-dihydroxypolydimethylsiloxane to remove the alcohol, thereby reducing the silanol content in the system, effectively avoiding the reaction between free alcohol and polysiloxane, and improving the storage stability of the sealant without modifying the α, ω-dihydroxypolydimethylsiloxane, and the storage stability can reach more than 12 months. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0031] Figure 1 A schematic flow chart of a method for preparing a dealcoholized silicone sealant provided in an embodiment of the present application. DETAILED DESCRIPTION

[0032] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.

[0033] The embodiment of the present application provides a dealcoholized silicone sealant, which can solve the problem of improving the storage stability of silicone sealants by adding process steps in the related art.

[0034] refer to Figure 1 The method for preparing the dealcoholized organosilicon sealant provided in the embodiment of the present application comprises the following steps:

[0035] Step S101, adding 100 parts of α, ω-dihydroxy polydimethylsiloxane, 5-40 parts of plasticizer and 60-150 parts of filler into a stirring kettle, stirring and dehydrating for 2-4 hours at a temperature of 120-150° C. and under vacuum conditions, cooling to obtain a mixed base material;

[0036] Step S102, adding 2-15 parts of a crosslinking agent, 0.5-8 parts of a coupling agent, 1-10 parts of a catalyst and 0.1-5 parts of a stabilizer to the mixed base material in order by weight, and evacuating the mixture to obtain a dealcoholized silicone sealant.

[0037] Among them, the structural formula of α, ω-dihydroxy polydimethylsiloxane is: In the formula, R is methyl, phenyl or vinyl.

[0038] The coupling agent composition includes an α-coupling agent trimer, and the structural formula of the α-coupling agent trimer is shown in formula (I):

[0039] Formula (I):

[0040] In the formula, R1, R2, and R3 are each independently a C1-C4 alkyl group, and R1, R2, and R3 may be the same group or different groups.

[0041] The α-coupling agent trimer is prepared by the following process: adding an α-halosilane coupling agent, cyanate and a nickel complex to a solvent, stirring them evenly to completely dissolve them, heating them to 100-140° C., reacting them for 3-5 hours, filtering the obtained solution, and distilling them under reduced pressure to obtain α-isocyanate methyl silane; adding α-isocyanate methyl silane to a reaction kettle, adding a catalyst in the presence of a solvent, and then reacting them at 50-80° C. for 3-5 hours, then adding benzoyl chloride, and continuing to react for 0.5-1 hour to obtain the α-coupling agent trimer; the solvent used in the preparation process is methyl isobutyl ketone, N,N-dimethylformamide or n-butyl acetate; the catalyst used is an organic phosphorus catalyst, an organic amine catalyst or an organic base catalyst; the cyanate used is potassium cyanate or sodium cyanate; the structural formula of the α-halosilane coupling agent is:

[0042] The coupling agent also includes a mixture of one or more of aminopropyltrimethoxysilane, aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, isocyanatepropyltrimethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, N,N-diethyl-3-aminopropyltrimethoxysilane, bis-[3-(methoxysilyl)-propyl]-amine and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

[0043] Plasticizers include hydroxy-terminated polybutadiene and polydimethylsiloxane.

[0044] The dealcoholized organosilicon sealant and its preparation method provided by the present application are described in detail below in combination with the embodiments and comparative examples.

[0045] Example 1

[0046] Embodiment 1 provides a method for preparing a dealcoholized organosilicon sealant, comprising the following steps:

[0047] (1) adding 100 parts by mass of α,ω-dihydroxy polydimethylsiloxane having a viscosity of 20000 mPa·S at 25° C., 100 parts of nano calcium carbonate, 15 parts of polydimethylsiloxane having a viscosity of 300 mPa·S at 25° C., 10 parts of hydroxyl-terminated liquid polybutadiene having a viscosity of 400 mPa·S at 25° C., and 10 parts of fumed silica into a vacuum kneader, dehydrating, blending and kneading for 3 hours at a temperature of 120° C. and a vacuum degree of 0.095 MPa, and cooling to obtain a mixed base material;

[0048] (2) At room temperature, 7 parts by mass of methyltrimethoxysilane, 3 parts by mass of vinyltrimethoxysilane, 1 part by mass of aminopropyltriethoxysilane, 2 parts by mass of γ-(2,3-epoxypropoxy)propyltrimethoxysilane and 5 parts by mass of titanium complex of ethyl acetoacetate are added into a high-speed disperser or planetary mixer containing the above mixed base material, stirred for 30 minutes under the conditions of vacuum degree of -0.095 to -0.1 MPa and rotation speed of 80 rpm, then evacuated, and then 4 parts by mass of α-coupling agent trimer and 0.5 parts by mass of hexamethyldisilazane are added in sequence, stirred for 10 minutes under the conditions of vacuum degree of -0.095 to -0.1 MPa and rotation speed of 80 rpm, then evacuated to obtain a one-component dealcoholization type silicone sealant.

[0049] In Example 1, the nano calcium carbonate used is active nano calcium carbonate treated with stearic acid, and the fumed silica used is fumed silica surface treated with hexamethyldisilazane, with a specific surface area of ​​160 m 2 / g.

[0050] In Example 1, the structural formula of the α-coupling agent trimer used is shown in Formula (I), wherein R1 is a methyl group, and R2 and R3 are ethyl groups.

[0051] Comparative Example 1

[0052] Comparative Example 1 provides a method for preparing a dealcoholized silicone sealant. The difference between the preparation method provided in Comparative Example 1 and Example 1 is that: in the process of preparing the silicone sealant in Comparative Example 1, no α-coupling agent trimer is added; the rest of the process is basically the same as Example 1.

[0053] Comparative Example 2

[0054] Comparative Example 2 provides a method for preparing a dealcoholized silicone sealant. The difference between the preparation method provided in Comparative Example 2 and Example 1 is that: in the process of preparing the silicone sealant in Comparative Example 2, hydroxyl-terminated liquid polybutadiene is not added; the rest of the process is basically the same as Example 1.

[0055] Example 2

[0056] Embodiment 2 provides a method for preparing a dealcoholized organosilicon sealant, comprising the following steps:

[0057] (1) adding 100 parts by mass of α,ω-dihydroxy polydimethylsiloxane having a viscosity of 50000 mPa·S at 25°C, 120 parts of nano calcium carbonate, 5 parts of polydimethylsiloxane having a viscosity of 200 mPa·S at 25°C, 10 parts of hydroxyl-terminated liquid polybutadiene having a viscosity of 400 mPa·S at 25°C, and 10 parts of fumed silica into a vacuum kneader, dehydrating, blending and kneading for 3 hours at a temperature of 130°C and a vacuum degree of 0.095 MPa, and cooling to obtain a mixed base material;

[0058] (2) At room temperature, 5 parts by mass of methyltrimethoxysilane, 3 parts by mass of vinyltriethoxysilane, 2 parts by mass of aminopropyltrimethoxysilane, 2 parts by mass of γ-(2,3-epoxypropoxy)propyltrimethoxysilane and 4 parts by mass of titanium complex of ethyl acetoacetate are added into a high-speed disperser or planetary mixer containing the above mixed base material, stirred for 30 minutes at a vacuum degree of -0.095 to -0.1 MPa and a rotation speed of 80 rpm, and then evacuated. Then, 2 parts by mass of α-coupling agent trimer and 3 parts by mass of hexamethylcyclotrisilylazane are added in sequence, stirred for 10 minutes at a vacuum degree of -0.095 to -0.1 MPa and a rotation speed of 80 rpm, and then evacuated to obtain a one-component dealcoholized silicone sealant.

[0059] In Example 2, the nano calcium carbonate used is active nano calcium carbonate treated with stearic acid, and the fumed silica used is fumed silica surface treated with hexamethyldisilazane, with a specific surface area of ​​160 m 2 / g.

[0060] In Example 2, the structural formula of the α-coupling agent trimer used is shown in Formula (I), wherein R1 is methyl, R2 is ethyl, and R3 is butyl.

[0061] Example 3

[0062] Embodiment 3 provides a method for preparing a dealcoholized organosilicon sealant, comprising the following steps:

[0063] (1) Add 100 parts by mass of α,ω-dihydroxy polydimethylsiloxane having a viscosity of 20000 mPa·S at 25°C, 80 parts of nano calcium carbonate, 15 parts of polydimethylsiloxane having a viscosity of 600 mPa·S at 25°C, 15 parts of hydroxyl-terminated liquid polybutadiene having a viscosity of 600 mPa·S at 25°C, and 10 parts of silicon powder into a vacuum kneader, dehydrate, blend and knead for 3 hours at a temperature of 140°C and a vacuum degree of 0.095 MPa, and cool to obtain a mixed base material;

[0064] (2) By mass, at room temperature, 4 parts of isopropyl triethoxysilane, 3 parts of isopropyl trimethoxysilane, 0.5 parts of aminopropyl triethoxysilane, 1 part of γ-mercaptopropyl trimethoxysilane, and 3 parts of n-butyl titanate were added into a high-speed disperser or planetary mixer containing the above mixed base material, and stirred for 30 minutes under the conditions of vacuum degree of -0.095 to -0.1 MPa and rotation speed of 80 rpm, and then evacuated, and then 1 part of α-coupling agent trimer and 1 part of divinyltetramethoxydisilazane were added in sequence, and stirred for 10 minutes under the conditions of vacuum degree of -0.095 to -0.1 MPa and rotation speed of 80 rpm, and then evacuated to obtain a one-component dealcoholized silicone sealant.

[0065] In Example 3, the nano calcium carbonate used is active nano calcium carbonate treated with stearic acid.

[0066] In Example 3, the structural formula of the α-coupling agent trimer used is shown in Formula (I), wherein R1 and R2 are ethyl groups, and R3 is butyl group.

[0067] Example 4

[0068] The only difference between Example 4 and Example 1 is that aminopropyltriethoxysilane and γ-(2,3-epoxypropoxy)propyltrimethoxysilane are not added during the preparation of the silicone sealant; the rest is basically the same as Example 1.

[0069] The performance of the silicone sealants prepared in Examples 1-4 and Comparative Examples 1-2 was tested. The results are shown in Table 1.

[0070] Table 1: Performance comparison of the silicone sealants prepared in Examples 1-4 and Comparative Examples 1-2

[0071]

[0072] Note: The thermal storage aging condition is 70℃×7d, and the double 85 environmental aging condition is: temperature 85±2℃, humidity 85±5%

[0073] From the results of Examples 1-4 and Comparative Examples 1-2, it can be seen that the thermal storage aging performance and double 85 environmental aging of the sealant prepared in Comparative Example 1 without adding the α-coupling agent trimer are significantly lower than those of the sealant prepared in Example 1; the mechanical properties of the sealant prepared in Comparative Example 2 without adding polybutadiene are significantly lower than those of the sealant prepared in Example 1.

[0074] In the description of this specification, the description with reference to the terms "one embodiment / method", "some embodiments / methods", "example", "specific example" or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment / method or example are included in at least one embodiment / method or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment / method or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments / methods or examples. In addition, those skilled in the art may combine and combine the different embodiments / methods or examples described in this specification and the features of the different embodiments / methods or examples, unless they are contradictory.

[0075] It should be noted that, in the present application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply that there is any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that the process, method, article or equipment including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment. In the absence of more restrictions, the elements defined by the sentence "comprise one..." do not exclude the existence of other identical elements in the process, method, article or equipment including the elements. In the present application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically stipulated.

[0076] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.

Claims

1. A dealcoholized organosilicon sealant, characterized in that: It is prepared by using α, ω-dihydroxy polydimethylsiloxane, filler, plasticizer, crosslinking agent, coupling agent, catalyst and stabilizer. The preparation steps are as follows: S1. Mixing α, ω-dihydroxy polydimethylsiloxane, a plasticizer and a filler, heating and evacuating to obtain a mixed base material; S2. Adding a crosslinking agent, a coupling agent, a catalyst and a stabilizer to the mixed base material in sequence, evacuating to obtain a dealcoholized silicone sealant; The weight parts of the raw materials are: 100 parts of α, ω-dihydroxy polydimethylsiloxane, 60-150 parts of filler, 5-40 parts of plasticizer, 2-15 parts of crosslinking agent, 0.5-8 parts of coupling agent, 1-10 parts of catalyst, and 0.1-5 parts of stabilizer; The coupling agent has a plurality of alkoxy groups that undergo condensation reaction with the hydroxyl groups of α,ω-dihydroxy polydimethylsiloxane; the coupling agent includes an α-coupling agent trimer, and the structural formula of the α-coupling agent trimer is: , In the formula, R1, R2, and R3 are each independently a C1-C4 alkyl group; The mass amount of the α-coupling agent trimer accounts for 20%-80% of the total mass of the coupling agent; The plasticizer includes hydroxyl-terminated polybutadiene and polydimethylsiloxane; the viscosity of the hydroxyl-terminated polybutadiene is 100-1000 mPa·S.

2. The dealcoholized organosilicon sealant according to claim 1, characterized in that: The coupling agent also includes a mixture of one or more of aminopropyltrimethoxysilane, aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, isocyanatepropyltrimethoxysilane, γ-(2,3-epoxypropoxy)propyltrimethoxysilane, N,N-diethyl-3-aminopropyltrimethoxysilane and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.

3. The dealcoholized organosilicon sealant according to claim 1, characterized in that: The mass ratio of the hydroxyl-terminated polybutadiene to polydimethylsiloxane is 1:5-5:

1.

4. The dealcoholized organosilicon sealant according to claim 1, characterized in that: The filler is a mixture of one or more of nano calcium carbonate, silicon powder, fumed silica, light calcium carbonate and heavy calcium carbonate.

5. The dealcoholized organosilicon sealant according to claim 1, characterized in that: The crosslinking agent is a mixture of one or more of methyltrimethoxysilane, methyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, isopropyltrimethoxysilane, isopropyltriethoxysilane, phenyltriethoxysilane, methyl orthosilicate, and ethyl orthosilicate.

6. The method for preparing the dealcoholized organosilicon sealant according to any one of claims 1 to 5, characterized in that: The following steps are involved: α,ω-dihydroxy polydimethylsiloxane, a plasticizer and a filler are mixed, heated and vacuumized to obtain a mixed base material; Add a crosslinking agent, a coupling agent, a catalyst and a stabilizer to the mixed base material in sequence, and evacuate the mixture to obtain a dealcoholized organic silicone sealant.

Citation Information

Patent Citations

  • Heat-conducting single component dealcoholization type RTV sealant and preparation method thereof

    CN106833504A

  • Dealcoholized silicone rubber sealant

    CN106957631A

  • Silane-terminated liquid polybutadiene modified organic silicon sealant and preparation method thereof

    CN109722216A

  • Bi-component room temperature vulcanized silicone rubber composition for sensor and preparation method thereof

    CN112574712A