Preparation method of highly oriented graphene aerogel and graphene composite interface material
By using porous PU film stretching and heat treatment technology in graphene aerogels, combined with the impregnation and curing method of silicone reaction solution, the problem of low longitudinal thermal conductivity of graphene composite interface materials was solved, and graphene with high thermal conductivity was prepared Composite interface material, suitable for high-performance applications in the field of thermal management.
Patent Information
- Application Number
- CN202211566587.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-12-07
AI Technical Summary
The existing graphene composite interface materials have low longitudinal thermal conductivity, which limits their application in the field of thermal management, and traditional directional cryogenic methods are complex and difficult to produce on a large scale.
By impregnating the porous PU film in the GO slurry and stretching, then rolling and heat treatment, forming a highly oriented graphene aerogel, vacuum impregnating and curing combined with the silicone reaction solution, high longitudinal heat conduction graphite was prepared by preparing Ethylene composite interface material.
The preparation of high-oriented graphene aerogel was achieved, which significantly improved the longitudinal thermal conductivity to reach ≥70W/mK, and showed good cooling effect and industrial application performance in thermal management applications.
Smart Images

Figure CN116161649B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of graphene materials, and more specifically, relates to a method for preparing a directional three-dimensional graphene aerogel, a graphene composite interface material with high longitudinal thermal conductivity and a method for preparing the same. Background Art
[0002] Graphene aerogels are widely used for their ultra-light, porous, high-strength, high-elasticity, strong adsorption, thermal and electrical conductivity, etc., such as in adsorption, sensing, catalysis, capacitors, batteries, thermal management and electromagnetic shielding. Phase change materials, polymers, etc. are used to replace the air in the pores of graphene aerogels by vacuum impregnation. After the composite material is cured, it can be used as a thermal interface material. The general graphene composite interface material is generally lower than 10W / mK, and cannot fully exert the extremely high intrinsic thermal conductivity of graphene (5300W / mK). How to fully reflect this microscopic intrinsic thermal conductivity in the macroscopic structure is a direction worth studying. The highly oriented alignment connection of graphene sheets is conducive to improving the thermal conductivity of the material in this direction. For example, the graphene film obtained by a series of heat treatment and calendering processes of graphene oxide film formed by horizontal arrangement and stacking of nanosheets can reach a thermal conductivity of more than 1500W / mK in the plane, which is 2~3 orders of magnitude higher than the longitudinal thermal conductivity. The industry has achieved great success and breakthroughs in improving the lateral thermal conductivity of graphene-related thermal application products, but there is still a lot of room for improvement in longitudinal thermal conductivity. The internal structure of graphene aerogel obtained by solvent foaming and subsequent heat treatment of graphene oxide membrane is fully cross-linked, with low density and high porosity, but the internal graphene sheets do not have consistent orientation, resulting in low longitudinal thermal conductivity. The commonly used directional freezing method in the industry can adjust the orientation of graphene sheets to prepare vertically arranged graphene aerogels, but the method is complicated and the drying conditions are high, which limits the possibility of large-scale production. The composite material constructed by the graphene aerogel skeleton provides a continuous heat flow path through the material. Compared with the composite interface material prepared by commonly using graphene powder as a thermal conductive filler, the former generally has a higher thermal conductivity. Therefore, graphene aerogel has also been a hot spot in the research direction of interface thermal management materials in recent years. Developing a simple method for preparing highly oriented graphene aerogel with high longitudinal thermal conductivity, and further using the graphene aerogel to prepare composite interface materials with high longitudinal thermal conductivity, is of great significance to many thermal management fields with high heat dissipation requirements. Summary of the invention
[0003] On the one hand, a method for preparing a highly oriented graphene aerogel is provided, and the specific method is as follows:
[0004] The porous PU membrane is completely immersed in the GO slurry, and the porous PU membrane is kept in a stretched state, and is wound onto a block substrate for winding and drying. The block substrate is then removed, and the PU membrane is removed and graphitized to obtain a highly oriented graphene aerogel hollow structure sample. The highly oriented graphene aerogel hollow structure sample is cut into four sides to obtain at least four blocks of highly oriented graphene aerogels.
[0005] Preferably, the solid content of the GO slurry is 1.5%-3%, and the viscosity is 18000-30000 cP. The solid content and viscosity within this range make the GO slurry have a certain fluidity, which is conducive to the diffusion of the GO slurry into the porous PU film; too low solid content and viscosity make it difficult to form a film, which is not conducive to the large-area adhesion of GO nanosheets on the inner and outer surfaces of the pores of the PU film, and it is not easy to form a continuous and complete graphene three-dimensional structure after the subsequent heat treatment to remove the porous PU film; too high solid content and viscosity have poor fluidity, which is not conducive to the diffusion of GO slurry into the porous PU film or is easy to agglomerate on the surface of the porous PU film.
[0006] Preferably, a PET film is attached to the contact surface between the block substrate and the porous PU film. Specifically, prepare a square substrate of a certain specification, stick double-sided tape on the four sides of the square substrate that need to be wrapped with the porous PU film, tear off the protective film on the other side of the double-sided tape, take a PET film of a suitable size and wrap it around the four sides of the block with double-sided tape. The square substrate plays the role of winding and shaping, and the PET film prevents GO from directly contacting with blocks of different materials and affecting the removal of the material after drying. The oily surface of the PET film is easy to separate from the dried GO. The square substrate can be any hard material that can withstand a temperature of 80°C, such as wood blocks, aluminum blocks, stainless steel blocks, etc.
[0007] Preferably, the stretching length of the porous PU film is 2-3.5 times of the initial length, and the porous PU film has stretching resilience and self-adhesion. On the one hand, the stretching and impregnation of the porous PU film makes the film thinner, thereby reducing the diffusion distance of the GO slurry, so that it is fully wetted. On the other hand, it makes the inside of the PU film have a consistent orientation, and the nanosheets in the graphene aerogel form a similar directional arrangement, thereby improving the thermal conductivity of the graphene aerogel material in this direction. If the PU film is not stretched, the GO slurry has a large diffusion distance and no directional arrangement is formed, which will result in the final thermal conductivity of the graphene aerogel being low. If the stretching length of the PU film is too large, the pore structure of the graphene aerogel will be narrower and denser, hindering the subsequent filling of the composite material. At the same time, since the porous PU film has self-adhesion, it can be directly rolled up with a square substrate after being fully impregnated with GO slurry in a stretched state. After rolling up, the self-adhesion will not loosen, and there is no need to fix it with a rope or other external objects.
[0008] Preferably, the drying treatment temperature is ≤80°C. The drying temperature is limited to no higher than 80°C because GO retains most of the oxygen-containing functional groups below 80°C and is easy to self-assemble into a film.
[0009] Preferably, the PU film removal treatment is preferably performed by vacuum heat treatment at 800-1000°C. Specifically, the dried sample is placed in a carbonization furnace, heated from room temperature to 160-200°C at a heating rate of 0.5-1.5°C / min, kept warm for 1-3 hours, and heated from 160-200°C to 800-1000°C at a heating rate of 1-5°C / min, kept warm for 1-3 hours, in a vacuum environment, wherein the PU is completely removed after treatment at 800-1000°C.
[0010] Preferably, the graphitization treatment temperature is 2800-3000° C. Specifically, the sample after vacuum heat treatment is placed in a graphitization furnace, and the temperature is increased from room temperature to 2800-3000° C., the heating rate is 5-10° C. / min, and the temperature is kept for 2-5 hours in a vacuum environment. After the graphitization is completed, the sample is cooled and taken out to obtain a highly oriented graphene aerogel hollow structure sample.
[0011] The graphitized sample is cut into at least four complete modules on four sides, thus obtaining a block of highly oriented graphene aerogel. It should be noted that the intersection of the sample faces before cutting will produce a certain micro-curve when winding. In order to obtain highly oriented graphene aerogel in the same direction, some areas near the curved surface need to be cut off.
[0012] The highly oriented graphene aerogel prepared by the above method has loose pores and high thermal conductivity due to its directional arrangement in the same direction.
[0013] On the other hand, a method for preparing a graphene composite interface material with high longitudinal thermal conductivity is provided, and the specific method is as follows:
[0014] The highly oriented graphene aerogel prepared by the above method is vacuum impregnated into the organosilicon reaction solution for 20-30 minutes, taken out and hung at 120-180°C for 20-30 minutes until solidified, and then cut to a specified thickness along a direction perpendicular to the stretching direction of the porous PU film to obtain a graphene composite interface material with high longitudinal thermal conductivity.
[0015] Preferably, the organic silicon reaction solution comprises a base material, a crosslinking agent, a catalyst and an inhibitor, wherein the amount of the catalyst is 1% of the base material, the amount of the inhibitor is 1 / 1000 of the base material, and the molar ratio of the base material to the crosslinking agent is 0.8-1:1-1.2. The reaction molar ratio of the base material to the crosslinking agent is controlled at about 1:1 to ensure that the reaction and curing are carried out at a suitable time and temperature.
[0016] Preferably, the base material is vinyl silicone oil, the crosslinking agent is hydrogenated silicone oil, the catalyst is a platinum catalyst, and the inhibitor is acetylene cycloethanol, wherein the viscosity of the vinyl silicone oil is 200-400 mPa·s, the vinyl content is 0.12-0.63 wt%, and the hydrogen content of the hydrogenated silicone oil is 0.11-1.61 wt%. The viscosity of the vinyl silicone oil is 200-400 mPa·s, which can make the organosilicon reaction solution better filled into the three-dimensional structure of graphene. If the viscosity is too high, it is not conducive to the diffusion of the organosilicon solution into the graphene aerogel structure.
[0017] On the other hand, a graphene composite interface material with high longitudinal thermal conductivity prepared by the above method is provided. The graphene composite interface material has a longitudinal thermal conductivity of ≥70W / mK, no slag when cut, good surface viscosity and elasticity, and can be adhered to the surface of a release film and hung upside down in the air for 48 hours without falling off. After 100 cycles of 50% compression ratio testing, the rebound rate is close to 100%.
[0018] The highly oriented graphene aerogel prepared by this method has a highly consistent orientation, which greatly enhances its longitudinal thermal conductivity as the skeleton of the composite interface material. The organic silicon composite interface material prepared by this method will definitely have a good cooling effect on some serious heat-generating components such as chips with high integration and power density in thermal management applications. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 This is a physical picture of the porous PU film adsorbing GO slurry wrapped around the stainless steel block in Example 1;
[0020] Figure 2 This is a sample image of a highly oriented graphene aerogel hollow structure obtained in Example 1;
[0021] Figure 3 This is a physical comparison diagram of the porous PU film used in Example 1 before and after stretching;
[0022] Figure 4 This is the SEM image of the porous PU film in its unstretched natural state;
[0023] Figure 5 This is the SEM image of the porous PU film under stretching;
[0024] Figure 6 This is a cross-sectional SEM image of a three-dimensional graphene aerogel prepared in the unstretched state of the porous PU film in Comparative Example 1;
[0025] Figure 7 This is a cross-sectional SEM image of the highly oriented graphene aerogel prepared under the stretched state of the porous PU film in Example 2;
[0026] Figure 8This is a SEM image of a graphene composite interface material with high longitudinal thermal conductivity prepared under the stretched state of the porous PU film in Example 2;
[0027] Fig. 9 This is a test force-time curve of the high longitudinal thermal conductivity graphene composite interface material prepared in Example 2 after 100 cycles at 50% compression. DETAILED DESCRIPTION
[0028] The following detailed description of exemplary embodiments of the present invention refers to the accompanying drawings, which form a part of the description, in which exemplary embodiments of the present invention are shown as examples, wherein the features of the present invention are identified by reference numerals. The following more detailed description of the embodiments of the present invention is not intended to limit the scope of the claimed invention, but is merely for illustration and does not limit the description of the features and characteristics of the present invention, in order to propose the best way to perform the present invention, and is sufficient to enable those skilled in the art to implement the present invention. However, it should be understood that various modifications and variations may be made without departing from the scope of the present invention as defined by the appended claims. The detailed description and the accompanying drawings should be considered only as illustrative, not restrictive, and if there are any such modifications and variations, they will all fall within the scope of the present invention described herein. In addition, the background technology is intended to illustrate the current status and significance of the research and development of the present technology, and is not intended to limit the present invention or the application field of the present application and the present invention.
[0029] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs; the terms used in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention; the term "and / or" used herein includes any and all combinations of one or more related listed items.
[0030] If the specific conditions are not specified in the examples, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If the manufacturers of the reagents or instruments are not specified, they are all conventional products that can be purchased commercially.
[0031] In order to make the technical problems, technical solutions and advantages to be solved by the present invention more clear, a detailed description will be given below with reference to the accompanying drawings and specific embodiments.
[0032] Example 1
[0033] This embodiment is a specific method for preparing highly oriented graphene aerogel:
[0034] (1) Prepare a long stainless steel block (about 5 cm × 1.5 cm × 1.5 cm), stick a layer of double-sided tape on the four 5 cm × 1.5 cm surfaces of the stainless steel block, tear off the protective film on the other side of the double-sided tape, take a 4 cm wide PET film and wrap it around the four sides of the stainless steel block with double-sided tape. The stainless steel block is used as a winding PU film and can be reused.
[0035] (2) Use the Hummers method to prepare 200 g of GO slurry with a solid content of 2.5% and a viscosity of 25000 cP.
[0036] (3) After the porous PU film is impregnated with GO slurry in a stretched state, it is rolled up with the PET surface of a stainless steel block in the center. The specific operation is to take a 3 cm wide porous PU film, wet one end with GO slurry, and tightly wrap it around the square PET surface for two weeks, then press and fix it. Subsequently, the PU film is stretched to 2.5 times the original length, soaked in GO slurry, and rolled up to a thickness of 1 cm.
[0037] (4) The stainless steel block wrapped with the PU-GO membrane obtained after step (3) was placed in a forced air drying oven and baked at 80°C for 3 hours to dry. After drying, the sample was basically separated from the PET. The stainless steel block at the central axis was slightly loosened and removed to obtain a hollow structure sample composed of a directional graphene oxide membrane and PU.
[0038] (5) Heat treatment to pre-reduce GO and remove the PU template. Specifically, the dried sample was placed in a tube furnace, heated from room temperature to 180°C at a heating rate of 1°C / min, kept warm for 3 h, and then heated from 180°C to 800°C at a heating rate of 5°C / min, kept warm for 1 h, and heated in a vacuum environment. After the heat treatment was completed, the sample was taken out after cooling to obtain a three-dimensional reduced graphene oxide hollow structure sample.
[0039] (6) Graphitizing the heat-treated sample. Specifically, the heat-treated sample is placed in a graphitization furnace, heated from room temperature to 3000°C at a heating rate of 5°C / min, kept warm for 4 hours, and heated in a vacuum environment. After the graphitization treatment is completed, the sample is cooled and taken out to obtain a highly oriented graphene aerogel hollow structure sample.
[0040] (7) The graphitized sample is cut into four complete graphene blocks along four sides to obtain four blocks of highly oriented graphene aerogels.
[0041] Example 2
[0042] This embodiment is a specific method for preparing a graphene composite interface material with high longitudinal thermal conductivity:
[0043] (1) Prepare 300g of organosilicon reaction solution. Specifically, vinyl silicone oil with a viscosity of 300mPa·s, platinum catalyst, and acetylene cycloethanol are added to a rubber tank in a certain proportion, the amount of platinum catalyst is 1% of the vinyl silicone oil, and the amount of acetylene cycloethanol is 1 / 1000 of the vinyl silicone oil. The rubber tank containing the organosilicon reaction solution is placed in a double planetary vacuum mixer and rotated at high speed to make the components blended evenly. After the equipment stops, take out the rubber tank, add cross-linking agent hydrogenated silicone oil, and place the mixer again to rotate at high speed for mixing. The stirring parameters for both times are 3000r / min, the mixing time is 5min, and the vacuum is synchronized. The molar ratio of vinyl silicone oil to hydrogenated silicone oil is 1:1.
[0044] (2) The block-shaped highly oriented graphene aerogel obtained in Example 1 is completely immersed in the silicone solution system in the glue tank, and a simple limiting tool is used to prevent the aerogel from floating on the liquid surface. The glue tank is placed in a vacuum drying oven. After vacuum impregnation at room temperature for 25 minutes, the aerogel filled with silicone is taken out and hung in an oven and heated at 120°C to allow the silicone to cross-link and react for 30 minutes to solidify. After solidification, the finished product is cut into a thickness of 1.5 mm using a laser cutting device perpendicular to the stretching direction of the porous PU film to obtain a square sheet of graphene composite interface material with high longitudinal thermal conductivity.
[0045] Embodiment 3-9
[0046] This group of embodiments is a specific method for preparing a graphene composite interface material with high longitudinal thermal conductivity. The difference from Example 2 is that variables are made in GO solid content, GO viscosity, PU film stretching multiple, vinyl silicone oil viscosity, vinyl content, base material vinyl silicone oil and cross-linking agent hydrogen silicone oil molar ratio, and graphene aerogel vacuum impregnation time, and the others remain unchanged. Compared with Example 2, the variables of each group of embodiments are as follows:
[0047]
[0048] The graphene composite interface materials with high longitudinal thermal conductivity prepared in each embodiment were tested, and the results shown in the following table were obtained:
[0049]
[0050] From the above data results, it can be seen that the high longitudinal thermal conductivity graphene composite interface material prepared by the method described in this application has a longitudinal thermal conductivity ≥70W / mK, which is much higher than the graphene composite interface material prepared by the traditional method (generally around 40W / mK), and its viscosity test and compression rebound test can meet the requirements of industrial applications.
[0051] Comparative Examples 1-7
[0052] The difference between this group of comparative examples and Example 2 is that variables are made in GO solid content, GO viscosity, PU film stretching ratio, vinyl silicone oil viscosity, vinyl content, molar ratio of base vinyl silicone oil to cross-linking agent hydrogen silicone oil, and vacuum impregnation time of graphene aerogel, and the variable range is not within the optimal range provided in this application, and the others remain unchanged. Compared with Example 2, the variables of each group of comparative examples are as follows:
[0053]
[0054] The graphene composite interface materials with high longitudinal thermal conductivity prepared in each embodiment were tested, and the results shown in the following table were obtained:
[0055]
[0056] From the above data results, we can know that:
[0057] (1) GO slurry with high solid content and viscosity is not conducive to GO diffusion into the PU film due to high resistance and large diffusion distance. As shown in Comparative Example 3, it will lead to the failure to successfully prepare graphene composite interface materials;
[0058] (2) The three-dimensional graphene prepared under the stretched state of the porous PU film is highly oriented, and the corresponding composite material has a higher thermal conductivity, which is better than the three-dimensional graphene composite material prepared from the unstretched PU film;
[0059] (3) Graphene aerogel prepared under appropriate stretching is conducive to the diffusion of silicone inside it, while ensuring that the composite material has a high thermal conductivity. Although it is easier to fill and is conducive to improving elasticity when it is not stretched, the thermal conductivity is not high. Excessive stretching makes it more difficult to fill silicone, resulting in poor elasticity of the composite material.
[0060] (4) Highly oriented graphene aerogel is the main thermal conductive network in the composite material, while silicone is mainly used as an elastomer. The ratio of their components has little effect on the overall thermal conductivity of the material;
[0061] (5) The reaction molar ratio of the base material and the cross-linking agent needs to have a certain degree of cross-linking to ensure that it reacts and cures at an appropriate time and temperature. For example, in Comparative Example 6, due to too little cross-linking agent, the degree of cross-linking by hydrosilylation is low, resulting in the final sample failing to cure at 120°C for 30 min.
[0062] The above embodiments are preferred implementation schemes of the present invention. In addition, the present invention may also be implemented in other ways. Any obvious replacement without departing from the concept of the present invention is within the protection scope of the present invention.
Claims
1. A method for preparing a graphene composite interface material, characterized in that: The following steps are involved: Completely immerse a porous PU membrane in GO slurry, keep the porous PU membrane in a stretched state, wind it onto a block substrate for winding and drying, then remove the block substrate and perform PU membrane removal and graphitization to obtain a highly oriented graphene aerogel hollow structure sample, cut the highly oriented graphene aerogel hollow structure sample into four sides to obtain at least four blocks of highly oriented graphene aerogels, vacuum impregnate the highly oriented graphene aerogel into an organosilicon reaction solution for 25-30 minutes, take it out and hang it at 120-180° C. for 20-30 minutes until it solidifies, then cut it to a specified thickness along a direction perpendicular to the stretching direction of the porous PU film to obtain a graphene composite interface material; The GO slurry has a solid content of 1.5%-3% and a viscosity of 18000-30000 cP; The stretched length of the porous PU film is 2-3.5 times of the initial length, and the porous PU film has stretching resilience and self-adhesion; The organic silicon reaction solution comprises a base material, a crosslinking agent, a catalyst and an inhibitor, wherein the base material is vinyl silicone oil, wherein the viscosity of the vinyl silicone oil is 200-400 mPa·s, the vinyl content is 0.12-0.63 wt %, and the molar ratio of the base material to the crosslinking agent is 0.8-1:1-1.
2.
2. A method for preparing the graphene composite interface material according to claim 1, characterized in that: A PET film is attached to the contact surface between the block substrate and the porous PU film.
3. A method for preparing the graphene composite interface material according to claim 1, characterized in that: The PU film removal treatment is a vacuum heat treatment at 800-1000°C.
4. A method for preparing the graphene composite interface material according to claim 1, characterized in that: The drying treatment temperature is ≤80°C, and the graphitization treatment temperature is 2800-3000°C.
5. A method for preparing a graphene composite interface material according to any one of claims 1 to 4, characterized in that: The amount of the catalyst is 1% of the base material, and the amount of the inhibitor is 1 / 1000 of the base material.
6. A method for preparing the graphene composite interface material according to claim 5, characterized in that: The cross-linking agent is hydrogen-containing silicone oil, and the catalyst is a platinum catalyst.
7. A graphene composite interface material, characterized in that: The graphene composite interface material is prepared by the method according to any one of claims 1 to 6, and the longitudinal thermal conductivity of the graphene composite interface material is ≥70 W / mK.