A kind of adsorbent for purifying alcohol VOCs and preparation method thereof

By loading metal oxides on the zeolite molecular sieve and optimizing the silicon-aluminum ratio and pore size structure, the problems of poor adsorption properties and humidity of existing alcohol VOCs adsorbents are solved, and efficient and stable alcohol VOCs purification effect is achieved.

CN116173896BActive Publication Date: 2024-12-03ZHONGKE HUIZHI (DONGGUAN) EQUIP TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202111419187.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-11-26
Publication Date
2024-12-03
Estimated Expiration
2041-11-26

AI Technical Summary

Technical Problem

The existing alcohol VOCs adsorbents have poor adsorption properties on alcohol VOCs and perform poorly under humidity conditions, making it difficult to meet the purification needs of industrial emissions.

Method used

By loading metal oxides on the zeolite molecular sieve, the silicon-aluminum ratio and pore size structure of the zeolite are optimized, and combined with program heating and calcining technology, an adsorbent with high adsorption performance and stability is prepared.

Benefits of technology

It significantly improves the adsorption efficiency and selectivity of alcohol VOCs, ensuring that efficient purification performance is maintained under different humidity conditions and is low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116173896B_ABST
    Figure CN116173896B_ABST
Patent Text Reader

Abstract

The present invention provides an adsorbent for purifying alcohol VOCs, comprising: a zeolite with a silicon-aluminum ratio of not less than 3, and a metal oxide loaded on the zeolite; the loading amount of the metal oxide is 1-15wt% of the zeolite. The adsorbent of the present invention has the advantages of good hydrophobicity, good adsorption performance, high purification efficiency, good stability, low cost, etc.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of alcohol VOCs purification, and in particular to an adsorbent for purifying alcohol VOCs and a preparation method thereof. Background Art

[0002] VOCs (Volatile Organic Compounds) usually refer to various organic compounds with a boiling point of 50°C to 260°C under normal pressure. Alcohol VOCs are a class of organic compounds whose functional group is hydroxyl (-OH), and one or more hydrogens in hydrocarbon molecules are replaced by hydroxyl groups. In the production process of chemical industries such as printing, pulping, and pharmaceuticals, a large amount of alcohol VOCs, such as methanol, ethanol, isopropanol, and butanol, will be volatilized and emitted due to unorganized emissions and leakage. Most alcohol VOCs are flammable and explosive, and have certain toxicity, which will harm the environment and human health, but at the same time, as an important chemical material, they also have certain recycling value, so they need to be purified.

[0003] Among VOCs purification technologies, adsorption has the advantages of simple process, strong operability, low energy consumption, safety and environmental protection, and is currently the most widely used VOCs purification method. The key to adsorption technology is the selection of adsorption materials. Currently, commonly used adsorbents include activated carbon, activated alumina and silica gel. Although these adsorbents have universal adsorption and good adsorption for most VOCs, they have relatively poor adsorption for common alcohol VOCs. In order to further improve the adsorption capacity and efficiency of adsorbents for alcohol VOCs used in industrial emissions, new adsorbents must be developed.

[0004] Regarding the adsorption materials for alcohol VOCs, there are literature reports on "a new type of organic waste gas adsorption material and its preparation method" (patent number 201310501262.1), which uses olive kernels as raw materials to prepare a new type of organic waste gas adsorption material, which is more sensitive to the adsorption of alcohol organic waste gas. This patent uses olive kernels for pretreatment such as nucleic acid washing and impurity removal, activation, water washing and steam activation, and then adds a modifier to modify the functional groups of the adsorption material. Finally, after drying, a special material for adsorbing organic waste gas is obtained. The preparation process is cumbersome and complicated. Moreover, in actual industrial exhaust gas, water vapor and VOCs coexist, the hydrophobicity of activated carbon is poor, and humidity will inhibit the adsorbent's adsorption capacity for alcohol VOCs. This patent does not consider the adsorption capacity for alcohol VOCs under humidity conditions.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first purpose of the present invention is to provide an adsorbent for purifying alcohol VOCs. The adsorbent is prepared by loading metal oxides on zeolite molecular sieves so that the adsorbent has more active adsorption points and improves the adsorption performance. When the adsorbent is used for the purification of industrial alcohol VOCs, it has the advantages of good hydrophobicity, good adsorption performance, high purification efficiency, good stability and low cost.

[0007] The second purpose of the present invention is to provide a method for preparing the above-mentioned adsorbent. The preparation method loads metal oxides on zeolite through specific steps, and its loading amount can be controlled to reach 1 to 15 wt%. The metal oxides are more evenly distributed on the zeolite by fully grinding after drying and performing programmed temperature rising calcination, thereby generating more active adsorption points. At the same time, the presence of the metal oxides also enhances the adsorption force on alcohol VOCs, thereby improving the selective adsorption effect on alcohol VOCs.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] The present invention provides an adsorbent for purifying alcohol VOCs, comprising: a zeolite having a silicon-aluminum ratio of not less than 3, and a metal oxide supported on the zeolite;

[0010] The loading amount of the metal oxide is 1 to 15 wt % of the zeolite.

[0011] Zeolite molecular sieve is a synthetic crystalline silicate with highly ordered molecular size, adjustable pores, rich skeleton structure, and good regeneration performance, excellent thermal stability and non-flammability. It is considered to have good application prospects in the adsorption field. In the existing technology, VOCs adsorption has the following problems:

[0012] 1. Traditional VOCs adsorbents can achieve the purpose of reducing water adsorption through hydrophobic modification. Generally, the hydrophobic modification of zeolite molecular sieves is achieved by increasing the silicon-aluminum ratio, but at the expense of reducing the specific surface area of ​​the zeolite molecular sieve. The adsorption capacity of zeolite molecular sieves is closely related to their specific surface area, which seriously restricts the application of zeolite adsorbents in the field of VOCs adsorption.

[0013] 2. Metals and metal oxides have been widely used in catalysis and adsorption. However, at high temperatures, metal and metal oxide particles will aggregate, reducing the specific surface area, which hinders their application prospects as adsorbents.

[0014] In order to solve the above technical problems, the present invention provides an adsorbent for purifying alcohol VOCs. The adsorbent loads metal oxides on zeolite molecular sieves, utilizes the porous structure of zeolite to disperse nanoparticles and reduce their agglomeration, and can also serve as active adsorption points to produce weak chemical adsorption with oxygen-containing functional groups of alcohol VOCs, effectively improving the selective adsorption capacity of specific gases, thereby ensuring its adsorption effect on alcohol VOCs.

[0015] The reason why metal oxides are loaded instead of metal ions is that metal oxides can serve as active adsorption points, thereby improving the adsorption effect.

[0016] Preferably, the type of the zeolite is one or more of FAU type, MFI type, MOR type, BEA* type, CHA type and STT type.

[0017] Preferably, the zeolite is a mixture of FAU zeolite and MFI zeolite.

[0018] Preferably, the mass ratio of the FAU zeolite to the MFI zeolite is (0.5-2):1;

[0019] Preferably, the mass ratio of the FAU zeolite to the MFI zeolite is 1:1.

[0020] The reason for choosing a mixture of two zeolites for adsorption is to utilize the synergistic effect of the different pore sizes of the two zeolite molecular sieves to load dual active sites in order to achieve a better adsorption effect.

[0021] Preferably, when the zeolite is FAU type, the silicon-aluminum ratio is 3 to 15; when the zeolite is MFI type, the silicon-aluminum ratio is 5 to 600; when the zeolite is CHA type, the silicon-aluminum ratio is 5 to 20; when the zeolite is MOR type, the silicon-aluminum ratio is 5 to 40; when the zeolite is BEA* type, the silicon-aluminum ratio is not less than 25; when the zeolite is STT type, the silicon-aluminum ratio is not less than 10.

[0022] Preferably, the silicon-to-aluminum ratio of the zeolite is 4 to 15; preferably, the silicon-to-aluminum ratio of the zeolite is 5.3.

[0023] Preferably, the metal oxide is an oxide of one or more of Cu, Fe, Zn, Co, Ni, Mn, Na, K, Ca, Ba, Ce and La, and the metal oxide is loaded on the zeolite in the form of a metal soluble salt.

[0024] Preferably, the metal oxides are of two types.

[0025] Preferably, the metal oxides are cobalt oxide and manganese oxide; wherein the molar ratio of CoO to MnO is (1-5):1.

[0026] Preferably, the molar ratio of CoO to MnO is 2:1.

[0027] Preferably, the zeolite is of FAU type and MFI type, the silicon-aluminum ratio of the zeolite is 5.3, the loading amount of the metal oxide is 15wt%, and the metal oxide is cobalt oxide and manganese oxide; wherein the molar ratio of CoO to MnO is 2:1.

[0028] Preferably, the metal soluble salt is at least one of nitrate, acetate or chloride.

[0029] The adsorbent for purifying alcohol VOCs of the present invention achieves a good adsorption effect by loading metal oxides on zeolite and optimizing parameters such as zeolite type, silicon-aluminum ratio, loaded metal oxide type, loading amount and ratio.

[0030] On the one hand, by limiting the type of zeolite and the silicon-aluminum ratio, its capture of specific adsorbates can be improved. Selecting zeolites with pore sizes that match their kinetic diameters can reduce the effects of molecular diffusion and Knudsen diffusion effects, increase the adsorption rate in the pores, strengthen the effective adsorption of adsorbate molecules in the pores, and increase the adsorption capacity of the adsorbent. The molecular kinetic diameter of alcohol VOCs is in the range of 0.36 to 0.5 nm, and different types of zeolites have different pore sizes. By metal-modifying the zeolite molecular sieve to adjust the pore size, the pore size is matched with the molecular kinetic diameter of alcohol VOCs, thereby effectively improving the adsorption capacity;

[0031] On the other hand, alcohol VOCs are polar molecules, and their polarity is stronger than other types of VOCs, so a highly polar adsorbent, namely zeolite molecular sieve, is used. The adsorption of zeolite molecular sieve and alcohol VOCs belongs to physical adsorption. Under certain humidity conditions, water molecules with stronger polarity will replace the already adsorbed organic matter. Alcohol VOCs contain oxygen-containing functional groups, hydroxyl groups, which can combine with metal oxides loaded on zeolite to produce certain weak chemical adsorption, so metal oxides have a positive effect on improving the ability of zeolite molecular sieve to adsorb alcohol VOCs.

[0032] The present invention also provides a method for preparing the above-mentioned adsorbent, comprising the following steps:

[0033] Obtaining a predetermined mass of zeolite raw powder, dissolving at least one metal salt in deionized water according to a theoretical loading amount to form a metal salt solution;

[0034] Dropping the metal salt solution into the zeolite raw powder and stirring the mixture until it becomes a paste-like non-Newtonian fluid, wherein the amount of the metal salt solution added is determined according to the saturation amount of the zeolite raw powder;

[0035] The mixture is dried, and then ground so that the metal oxide can be uniformly loaded on the zeolite;

[0036] The ground zeolite is calcined at a high temperature to obtain a zeolite adsorbent loaded with metal oxides.

[0037] Preferably, the method for determining the saturation amount of the zeolite raw powder is as follows:

[0038] Take a certain amount of zeolite powder, add metal salt solution and stir until the mixture becomes a non-Newtonian fluid. Calculate the saturation amount of zeolite powder according to the amount of metal salt solution added. Specifically, saturation amount (mL / g) = amount of solution / mass of zeolite powder

[0039] The reason for obtaining the saturated amount of zeolite raw powder is to ensure the quantitative addition of the metal salt solution. If too much is added, the mixture will be too dilute and unable to form a non-Newtonian fluid. Not only will it be difficult to dry later, but it will also affect the loading amount of the metal oxide, which is not conducive to the adsorption effect of the adsorbent prepared later.

[0040] Preferably, before the mixture is dried, the mixture is twisted into a uniform cake shape so that a water film is formed on the surface of the mixture to facilitate rapid drying.

[0041] Preferably, the drying method is any one of rapid flash drying and microwave drying.

[0042] Preferably, the drying method is microwave drying, the microwave power is 600-900W, and the time is 30-240s.

[0043] Preferably, the grinding time is 5 to 20 minutes.

[0044] Preferably, the temperature-raising calcination process is: heating to 100-200° C. at a heating rate of 5-20° C. / min, maintaining for 0.5-2 h, heating to 300-550° C., and maintaining for 3-5 h.

[0045] The preparation method of the present invention supports metal oxides on zeolite through specific steps, and can control the loading amount to 1 to 15 wt%. The metal oxides are more evenly distributed on the zeolite by fully grinding after drying and performing programmed temperature rising calcination, thereby generating more active adsorption points, thereby improving the adsorption effect on alcohol VOCs.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] The adsorbent for purifying alcohol VOCs of the present invention loads metal oxides on zeolite molecular sieves, utilizes the porous structure of zeolite to disperse metal oxide nanoparticles and reduce their agglomeration, and can also serve as active adsorption points to effectively improve the selective adsorption capacity of specific gases, thereby ensuring its adsorption effect on alcohol VOCs. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0049] Figure 1 This is the adsorption breakthrough curve of the alcohol adsorbent provided in Example 1 of the present invention;

[0050] Figure 2 This is the adsorption breakthrough curve of the alcohol adsorbent provided in Example 7 of the present invention;

[0051] Figure 3 This is the adsorption breakthrough curve of the alcohol adsorbent provided in Example 9 of the present invention. DETAILED DESCRIPTION

[0052] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0053] Example 1

[0054] Weigh 10 g of H-FAU molecular sieve with a silicon-aluminum ratio of 5.3 into a beaker, and weigh 1.6 g of copper nitrate according to the theoretical loading of 5 wt%, and add 8.9 mL of deionized water to dissolve. Use a pipette to mix the prepared Cu(NO 3 ) 2 ·3H 2O metal salt solution. Use a pipette to add the prepared solution to the original powder one by one, and stir continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the paste-like mixture in a petri dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10 minutes, then increase the temperature to 200℃ in a muffle furnace at 10℃ / min, maintain it for 0.5h, and continue to increase it to 550℃ at 10℃ / min, and maintain it for 4h. The zeolite molecular sieve adsorbent loaded with copper oxide CuO can be obtained.

[0055] Example 2

[0056] Weigh 10g of H-MFI molecular sieve with a silicon-aluminum ratio of 55 into a beaker, and weigh 1.135g of copper chloride according to the theoretical loading of 5wt% and dissolve it in 8.2ml of deionized water. Use a pipette to mix the prepared CuCl 2 ·2H 2 O solution is added to the original powder gradually, and stirred continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, the mixture is placed in a petri dish, twisted into a uniform cake with a spoon, placed in a microwave heater, and flashed at a fixed power of 600W for 240s until it is completely dry. After taking it out, grind the mixture for 5 minutes, then increase the temperature to 160℃ at 5℃ / min in a muffle furnace, keep it for 1h, and then increase it to 400℃ and keep it for 4h. The zeolite molecular sieve adsorbent loaded with copper oxide CuO can be obtained.

[0057] Example 3

[0058] Weigh 10 g of CHA molecular sieve with a silicon-aluminum ratio of 10 into a beaker, and weigh 2.39 g of lanthanum nitrate according to the theoretical loading of 5 wt% and dissolve it in 9 ml of deionized water. 3 ) 3 6H 2 O metal solution is added to the original powder gradually, and stirred continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, the mixture is placed in a petri dish, twisted into a uniform cake with a spoon, placed in a microwave heater, and flashed at a fixed power of 700W for 150s until it is completely dry. After taking it out, grind the mixture for 10 minutes, then increase the temperature to 200℃ in a muffle furnace at 20℃ / min, maintain for 2h, and continue to increase the temperature to 300℃ at 20℃ / min, and maintain for 5h. The loaded lanthanum oxide La can be obtained. 2 O 3 Zeolite molecular sieve adsorbent.

[0059] Example 4

[0060] Weigh 10 g of MOR molecular sieve with a silicon-aluminum ratio of 15 into a beaker, and weigh 1.43 g of zinc acetate according to the theoretical loading of 5 wt% and dissolve it in 8.9 ml of deionized water. Use a pipette to mix the prepared Zn(CH 3 COO 2 ·2H 2 O metal solution is added to the original powder gradually, and stirred continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, the mixture is placed in a petri dish, twisted into a uniform cake with a spoon, placed in a microwave heater, and flashed at a fixed power of 800W for 200s until it is completely dry. After taking it out, grind the mixture for 10 minutes, then increase the temperature to 160℃ at 5℃ / min in a muffle furnace, keep it for 1h, and then increase it to 550℃ and keep it for 4h. The zeolite molecular sieve adsorbent loaded with zinc oxide ZnO can be obtained.

[0061] Example 5

[0062] Weigh 10 g of BEA* molecular sieve with a silicon-aluminum ratio of 30 into a beaker, and weigh 2.06 g of cobalt nitrate according to the theoretical loading of 5 wt% and dissolve it in 10 ml of deionized water. Use a pipette to mix the prepared Co(NO 3 ) 2 6H 2 O metal salt solution is added to the original powder gradually, and stirred continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, the mixture is placed in a petri dish, twisted into a uniform cake with a spoon, placed in a microwave heater, and flashed at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10 minutes, then increase it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, increase it to 550℃, and keep it for 4h. The zeolite molecular sieve adsorbent loaded with cobalt oxide CoO can be obtained.

[0063] Example 6

[0064] Weigh 10 g of STT molecular sieve with a silicon-aluminum ratio of 15 into a beaker, and weigh 1.8 g of manganese acetate according to the theoretical loading of 5 wt% and dissolve it in 7 ml of deionized water. Use a pipette to mix the prepared (CH 3 COO 2 Mn·4H 2 O metal salt solution is added to the original powder gradually, and stirred continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, the mixture is placed in a petri dish, twisted into a uniform cake with a spoon, placed in a microwave heater, and flashed at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10 minutes, then increase it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, increase it to 550℃, and keep it for 4h. The zeolite molecular sieve adsorbent loaded with manganese oxide can be obtained.

[0065] Example 7

[0066] Weigh 5g of H-FAU molecular sieve with a silicon-aluminum ratio of 5.3 and 5g of MFI molecular sieve into a beaker, and weigh 4.12g of cobalt nitrate according to the theoretical loading of 10wt%, and weigh 1.8g of manganese acetate according to the theoretical loading of 5wt% and dissolve them in 10.2ml of deionized water. Use a pipette to add the prepared metal mixed salt solution to the original powder one by one, and stir continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0067] Example 8

[0068] The specific operating conditions are the same as those in Example 7, except that the silicon-to-aluminum ratio of the zeolite in this example is 4.

[0069] Example 9

[0070] The specific operating conditions are the same as those in Example 7, except that the silicon-to-aluminum ratio of the zeolite in this example is 15.

[0071] Example 10

[0072] Weigh 5g of CHA molecular sieve and 5g of MOR molecular sieve with a silicon-aluminum ratio of 5.3 and put them into a beaker. At the same time, weigh 4.12g of cobalt nitrate according to the theoretical loading of 10wt%, and weigh 1.8g of manganese acetate according to the theoretical loading of 5wt% and dissolve them in 10.6ml of deionized water. Use a pipette to add the prepared solution to the original powder one by one, and stir continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0073] Embodiment 11

[0074] Weigh 5g of H-FAU molecular sieve and 5g of H-MFI molecular sieve with a silicon-aluminum ratio of 5.3 and put them into a beaker. At the same time, weigh 6.18g of cobalt nitrate according to the theoretical loading of 15wt% and dissolve it in 7.4ml of deionized water. Use a pipette to add the prepared metal salt solution to the original powder one by one, and stir it continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ at 10℃ / min in a muffle furnace, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide.

[0075] Example 12

[0076] Weigh 5g of H-FAU molecular sieve and 5g of H-MFI molecular sieve with a silicon-aluminum ratio of 5.3 and put them into a beaker. At the same time, weigh 5.4g of manganese acetate according to the theoretical loading of 15wt% and dissolve it in 7.4ml of deionized water. Use a pipette to add the prepared solution to the original powder one by one, and stir it continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ at 10℃ / min in a muffle furnace, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with manganese oxide.

[0077] Embodiment 13

[0078] Weigh 10g of H-FAU molecular sieve with a silicon-aluminum ratio of 5.3 and put it into a beaker. At the same time, weigh 4.12g of cobalt nitrate according to the theoretical loading of 10wt%, and weigh 1.8g of manganese acetate according to the theoretical loading of 5wt% and dissolve them in 9.1ml of deionized water. Use a pipette to add the prepared metal mixed solution to the original powder one by one, and stir it continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0079] Embodiment 14

[0080] Weigh 10g of MFI molecular sieve with a silicon-aluminum ratio of 5.3 and put it into a beaker. At the same time, weigh 4.12g of cobalt nitrate according to the theoretical loading of 10wt%, and weigh 1.8g of manganese acetate according to the theoretical loading of 5wt% and dissolve them in 9ml of deionized water. Use a pipette to add the prepared metal mixed solution to the original powder one by one, and stir it continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0081] Embodiment 15

[0082] Weigh 5g of H-FAU molecular sieve and 5g of H-MFI molecular sieve with a silicon-aluminum ratio of 5.3 and put them into a beaker. At the same time, weigh 2.06g of cobalt nitrate according to the theoretical loading of 5wt%, weigh 1.8g of manganese acetate according to the theoretical loading of 5wt%, and weigh 2.7g of ferric nitrate according to the theoretical loading of 5wt% and dissolve them in 9.1ml of deionized water. Use a pipette to add the prepared metal mixed solution to the original powder one by one, and stir continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ at 10℃ / min in a muffle furnace, keep it for 0.5h, raise it to 550℃, and keep it for 4h. A zeolite molecular sieve adsorbent loaded with cobalt oxide, manganese oxide and iron oxide can be obtained.

[0083] Example 16

[0084] Weigh 5g of H-FAU molecular sieve and 5g of H-MFI molecular sieve with a silicon-aluminum ratio of 5.3 and put them into a beaker. At the same time, weigh 2.47g of cobalt nitrate according to the theoretical loading of 6wt%, and weigh 1.08g of manganese acetate according to the theoretical loading of 3wt% and dissolve them in 7.4ml of deionized water. Use a pipette to add the prepared mixed solution to the original powder one by one, and stir continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0085] Embodiment 17

[0086] Weigh 5g of H-FAU molecular sieve and 5g of H-MFI molecular sieve with a silicon-aluminum ratio of 5.3 and put them into a beaker. At the same time, weigh 4.12g of cobalt nitrate according to the theoretical loading of 10wt%, and weigh 1.8g of manganese acetate according to the theoretical loading of 5wt% and dissolve them in 7.5ml of deionized water. Use a pipette to add the prepared solution to the original powder one by one, and stir continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then quickly raise it to 200℃ in a muffle furnace and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0087] Embodiment 18

[0088] Weigh 5g of H-FAU molecular sieve and 5g of H-MFI molecular sieve with a silicon-aluminum ratio of 5.3 and put them into a beaker. At the same time, weigh 2.06g of cobalt nitrate according to the theoretical loading of 5wt%, and weigh 1.8g of manganese acetate according to the theoretical loading of 5wt% and dissolve them in 7.4ml of deionized water. Use a pipette to add the prepared solution to the original powder one by one, and stir continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0089] Embodiment 19

[0090] Weigh 5g of H-FAU molecular sieve and 5g of H-MFI molecular sieve with a silicon-aluminum ratio of 5.3 and put them into a beaker. At the same time, weigh 4.12g of cobalt nitrate according to the theoretical loading of 10wt%, and weigh 0.72g of manganese acetate according to the theoretical loading of 2wt% and dissolve them in 7.4ml of deionized water. . Use a pipette to add the prepared solution to the original powder one by one, and stir it continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ at 10℃ / min in a muffle furnace, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0091] Embodiment 20

[0092] Weigh 8g of H-FAU molecular sieve with a silicon-aluminum ratio of 5.3 and 2g of H-MFI molecular sieve into a beaker, weigh 4.12g of cobalt nitrate according to the theoretical loading of 10wt%, and weigh 1.8g of manganese acetate according to the theoretical loading of 5wt% and dissolve them in 8.1ml of deionized water. Use a pipette to add the prepared mixed solution to the original powder one by one, and stir continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0093] Comparative Example 1

[0094] Weigh 5g of H-FAU molecular sieve and 5g of H-MFI molecular sieve with a silicon-aluminum ratio of 5.3 and put them into a beaker. At the same time, weigh 4.12g of cobalt nitrate according to the theoretical loading of 10wt%, and weigh 5.4g of manganese acetate according to the theoretical loading of 15wt% and dissolve them in 7.4ml of deionized water. Use a pipette to add the prepared solution to the original powder one by one, and stir continuously with a glass rod until the mixture becomes a paste-like non-Newtonian fluid. Then, place the mixture in a culture dish, twist it into a uniform cake with a spoon, put it into a microwave heater, and flash it at a fixed power of 900W for 90s until it is completely dry. After taking it out, grind the mixture for 10min, then raise it to 200℃ in a muffle furnace at 10℃ / min, keep it for 0.5h, raise it to 550℃, and keep it for 4h. You can get a zeolite molecular sieve adsorbent loaded with cobalt oxide and manganese oxide.

[0095] Experimental Example 1

[0096] The adsorbents of Examples 1-20 and Comparative Example 1 were used to conduct adsorption and penetration experiments on isopropanol VOCs, and the adsorption performance of the adsorbents was evaluated by the penetration time and the penetration adsorption amount. Figure 1-3 .

[0097] Experimental conditions: the adsorbent particle size is 60-40 mesh, the adsorption column is a quartz tube with an outer diameter of 6 mm and an inner diameter of 4 mm, the adsorbent is loaded with 25 mg, the total gas flow rate is 50 mL / min, the initial concentration of organic matter is 80 ppm, and the adsorption temperature is 30 °C.

[0098] During the entire adsorption process, the inlet concentration is constant. When the outlet concentration reaches 10% of the inlet concentration, the adsorbent is considered to have penetrated. The breakthrough adsorption amount is calculated based on the breakthrough curve as follows:

[0099]

[0100]

[0101] M is the molar mass of the adsorbate, in g / mol; F is the feed gas flow rate, in mL / min;

[0102] C 0 is the initial concentration of the adsorbate, in mg / m 3 ; C is the concentration of adsorbate in the tail gas at time t, in mg / m 3

[0103] m is the adsorbent loading amount, in g; t 0 is the adsorption starting time, in min;

[0104] t s is the starting breakthrough time, min; q is the breakthrough adsorption amount of the adsorbent, in mg / g;

[0105] is the initial concentration signal value of the chromatographic detector, in mv; is the baseline signal value of the chromatographic detector, in mv; is the concentration signal value of the chromatographic detector at time t, in mV.

[0106] Table 1 Experimental results

[0107]

[0108]

[0109] It can be seen from Table 1 that the adsorbent of the present invention has a good adsorption effect on VOCs of isopropanol, and the adsorption effect of Example 7 is the best.

[0110] Comparing Example 7 with Example 8 and Example 9, it can be seen that when the silicon-aluminum ratio increases or decreases, it will have an adverse effect on the adsorption performance of the adsorbent. This is because an increase or decrease in the silicon-aluminum ratio will affect the polarity of the zeolite molecular sieve. Only when the silicon-aluminum ratio is 5.3 can the optimal polarity matching effect with alcohol VOCs be achieved.

[0111] Comparing Example 7 with Example 10, Example 13 and Example 14, it can be seen that the adsorption effect of Example 10 is not as good as that of Example 7, indicating that the mixed adsorption effect of H-FAU and MFI is stronger than the combination of other zeolites; the adsorption effect of Example 7 is worse than that of Example 13 and Example 14, because the two zeolite molecular sieves can provide a reasonably matched pore structure and gradiently distributed acidity, which can achieve a synergistic effect between the two zeolite molecular sieves and achieve a better adsorption effect.

[0112] Comparing Example 7 with Example 11, Example 12 and Example 15, it can be seen that the adsorption effect of Example 7 is better than that of Example 11, Example 12 and Example 15. This is because loading two oxides can play a synergistic role, and the effect is better than the case of loading only one metal oxide. Loading three metal oxides will affect the strength of the adsorbent due to the competition between the loadings, which will have an adverse effect on the adsorption effect.

[0113] Comparing Example 7 with Example 16 and Comparative Example 1, it can be found that the adsorption effect of Example 7 is better than that of Example 16 and Comparative Example 1, which indicates that when the loading amount is too high, it will also have an adverse effect on the adsorption effect of the adsorbent. The best adsorption effect can only be achieved when the total loading amount is 15wt%.

[0114] Comparing Example 7 with Example 17, it can be seen that the adsorption effect of Example 17 is much lower than that of Example 7. This is because Example 7 adopts a programmed temperature rising calcination method. This specific temperature rising method can make the metal oxide more evenly distributed on the zeolite, produce more active adsorption points, and thus improve the adsorption effect on alcohol VOCs.

[0115] Experimental Example 2

[0116] The adsorption penetration experiment of isopropanol VOCs under water vapor conditions was carried out using the embodiment with a higher adsorption amount in Experimental Example 1, and the adsorption performance of the adsorbent was evaluated by the penetration time and the penetration adsorption amount. Experimental conditions: the adsorbent particle size is 60-40 mesh, the adsorption column is a quartz tube with an outer diameter of 6mm and an inner diameter of 4mm, the adsorbent is loaded with 25mg, the total gas flow is 50mL / min, the relative humidity of the gas flow is RH=50%, the initial concentration of organic matter is 80ppm, and the adsorption temperature is 30°C.

[0117] Table 2 Experimental results

[0118]

[0119] It can be seen from Table 2 that the adsorbent of the present invention can still ensure a good adsorption effect on VOCs under water vapor conditions.

[0120] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.

Claims

1. An adsorbent for purifying alcohol VOCs, characterized in that: include: A zeolite having a silicon-aluminum ratio of 4 to 15, and a metal oxide supported on the zeolite; The loading amount of the metal oxide is 1-15wt% of the zeolite; The zeolite is a mixture of FAU zeolite and MFI zeolite; the mass ratio of the FAU zeolite to the MFI zeolite is (0.5-2):1; The metal oxide is an oxide of one or both of Co and Mn.

2. The adsorbent according to claim 1, characterized in that The mass ratio of the FAU zeolite to the MFI zeolite is 1:

1.

3. The adsorbent according to claim 1, characterized in that The silicon-to-aluminum ratio of the zeolite is 5.

3.

4. The adsorbent according to claim 1, characterized in that The metal oxides are cobalt oxide and manganese oxide; wherein the mass ratio of CoO to MnO is (1-5):

1.

5. The adsorbent according to claim 4, characterized in that The mass ratio of the CoO to the MnO is 2:

1.

6. The adsorbent according to claim 5, characterized in that The zeolite is of FAU type and MFI type, the silicon-aluminum ratio of the zeolite is 5.3, the loading amount of the metal oxide is 15wt%, and the metal oxide is cobalt oxide and manganese oxide; wherein the mass ratio of CoO to MnO is 2:

1.

7. A method for preparing the adsorbent according to any one of claims 1 to 6, characterized in that: The steps include: Obtaining a predetermined mass of zeolite raw powder, dissolving at least one metal salt in deionized water according to a theoretical loading amount to form a metal salt solution; Dropping the metal salt solution into the zeolite raw powder and stirring the mixture until it becomes a paste-like non-Newtonian fluid, wherein the amount of the metal salt solution added is determined according to the saturation amount of the zeolite raw powder; The mixture is dried, and then ground so that the metal oxide can be uniformly loaded on the zeolite; The ground mixture is calcined at a high temperature to obtain a zeolite adsorbent loaded with metal oxides.

8. The preparation method according to claim 7, characterized in that: The method for determining the saturation amount of the zeolite raw powder is as follows: A fixed amount of zeolite raw powder is taken, a metal salt solution is added dropwise and stirred until the mixture becomes a non-Newtonian fluid, and the saturated amount of zeolite raw powder is calculated based on the amount of the metal salt solution added dropwise.

9. The preparation method according to claim 7, characterized in that: Before the mixture is dried, the mixture is twisted into a uniform cake shape so that a water film is formed on the surface of the mixture to facilitate rapid drying.

10. The preparation method according to claim 7, characterized in that: The drying method is any one of rapid flash drying and microwave drying.

11. The preparation method according to claim 10, characterized in that: The drying method is microwave drying, the microwave power is 600-900W, and the time is 30-240s.

12. The preparation method according to claim 7, characterized in that: The grinding time is 5 to 20 minutes.

13. The preparation method according to claim 7, characterized in that: The temperature-raising calcination process is: raising the temperature to 100-200° C. at a heating rate of 5-20° C. / min, maintaining for 0.5-2 h, raising the temperature to 300-550° C., and maintaining for 3-5 h.

Citation Information

Patent Citations

  • A kind of organic waste gas adsorption material and preparation method thereof

    CN103537259B

  • Preparation of binderless MFI / FAU composite zeolite molecular sieve

    CN101348260A

  • Catalyst for catalytic ozonation of volatile organic compounds and preparation method thereof

    CN113145161A