A method for preparing methyl methacrylate by oxidation
By using a composite catalytic material of all-silica molecular sieves and metal elements dispersed in the molecular sieve crystals, the problems of low catalyst conversion rate and high by-products in the production of methyl methacrylate are solved, and efficient and environmentally friendly methyl methacrylate is achieved. Production.
Patent Information
- Application Number
- CN202111424561.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-11-26
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-11-26
AI Technical Summary
The existing production process of methyl methacrylate has problems such as low catalyst conversion rate, large number of by-products, and poor selectivity. Moreover, the traditional method is complicated, equipment consumption is high, and environmental pollution is serious.
A composite catalytic material of all-silica molecular sieve and metal elements dispersed in the molecular sieve crystal is used as a catalyst to improve the conversion rate of methacrolein and the selectivity of methyl methacrylate through oxidative esterification reaction under oxygen conditions.
The high conversion rate of methacrolein and the high selectivity of methyl methacrylate are achieved under milder conditions, simplifying the process, reducing energy consumption and investment costs, and reducing corrosion and side reactions of acidic substances on equipment. .
Smart Images

Figure CN116174013B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of organic chemical industry, and in particular, to a method for preparing methyl methacrylate by oxidation. Background Art
[0002] MMA can be used as a monomer for homopolymerization or copolymerization. The homopolymer PMMA is a colorless and transparent plastic that is easy to process and color. It can be processed into thin plates, extruded sheets, rods, tubes and powders. It is widely used in the construction, sanitary ware, advertising decoration, home appliances, instrumentation and other industries. After molding, it has durability and good insulation properties. Copolymers can be used in coatings, spray paints, adhesives, lubricants, artificial marble, PVC processing aids and PVC impact modifiers, textile and paper processing, leather surface treatment, etc. Other uses include casting biological specimens and making dentures, and can react with other alcohols to make other types of acrylates.
[0003] The synthesis method of MMA was previously mainly based on the acetone cyanohydrin method (ACH method), and the industrial application technology is mature and reliable. However, it has disadvantages such as the highly toxic raw material hydrocyanic acid, difficult to handle reaction by-products, poor atom economy and environmental restrictions. It has gradually been replaced by environmentally friendly processes, among which the C4 synthesis process is the main one. The C4 synthesis process is mainly divided into the following four process routes: isobutylene (IB) / tert-butyl alcohol (TBA) three-step oxidation method, IB / TBA two-step oxidation method, IB / TBA direct esterification method and isobutane oxidation method; among them, Japan Catalyst Chemical Co., Ltd. and Mitsubishi Rayon Co., Ltd. respectively adopted the IB / TBA three-step oxidation method to realize the industrialization of isobutylene oxidation in 1982. The process is complicated and has a long process, requires many production equipment, and has a low overall yield; Asahi Kasei Corporation has been studying the IB / TBA two-step oxidation method to synthesize MMA since 1995. The IB / TBA direct esterification method is also a process developed and industrialized by Asahi Kasei Corporation in 1984. Although this process does not use highly toxic chemicals such as hydrocyanic acid, it produces a large amount of by-product ammonium bisulfate, which needs to solve a series of problems such as waste acid treatment, environmental pollution and equipment corrosion, and the MMA yield is not as high as the direct oxidation method. Therefore, Asahi Kasei Corporation transformed it into an IB / TBA direct oxidation two-step device in 1999. Rohm and Haas Company of the United States uses heteropolyacid catalysts to catalyze the direct oxidation and dehydrogenation of isobutane to produce MAA, and then esterifies MAA to produce MMA, which is the isobutane oxidation method. This process requires large investment, and the production cost of the product isobutene is high, and the production of MMA is not competitive.
[0004] The two-step direct oxidation method of IB / TBA integrates the last two steps of the three-step method into one step, that is, IB / TBA is first directly oxidized to MAL, and then MAL, MeOH and O2 are oxidized and esterified in the presence of a catalyst to obtain the product methyl methacrylate. The two-step method is a very promising environmentally friendly process route. Compared with the three-step oxidation method of IB / TBA, the two-step method greatly simplifies the process flow, has higher atomic economy, lower energy consumption, lower investment cost and operating cost, and does not generate the intermediate product methacrylic acid, which reduces the corrosion of acidic substances to equipment and the polymerization side reaction of methacrylic acid. The raw material methanol can be recycled, which is currently the most competitive production method.
[0005] Palladium metal is the main active component in the catalyst for the direct oxidative esterification reaction of MAL, MeOH and O2 to produce MMA, but the result of single metal catalysis is low conversion rate, many by-products and poor selectivity (US3772381). Subsequent patents have made improvements to this, such as the Pd-Pb system catalysts proposed in JP-B-57-35856, JP-A-57-50545 and JP-A-61-243044, the Pd-Pb-Bi system proposed in CN1485133A, CN103721744A, CN101332427A, the Pd-Te system proposed in JP-A-61-243044, the Pd-Tl-Hg system proposed in JP-B-57-35860, the Pd-alkaline earth-Zn-Cd system proposed in JP-B-57-19090, etc. However, the improvement methods disclosed in these patents are limited to adding many other metal components to improve this defect, and the catalyst preparation process is cumbersome and has poor reproducibility. Summary of the invention
[0006] The object of the present disclosure is to provide a method for preparing methyl methacrylate by oxidation, which uses a composite catalytic material including an all-silicon molecular sieve and metal elements dispersed in the molecular sieve crystals as a catalyst, so that a high conversion rate of methacrolein and a high selectivity of methyl methacrylate can be obtained in the reaction of methacrolein to produce methyl methacrylate under relatively mild conditions.
[0007] In order to achieve the above object, the present disclosure provides a method for preparing methyl methacrylate by oxidation, the method comprising the following steps:
[0008] Under oxygen conditions, methacrolein is contacted with a catalyst to carry out an oxidative esterification reaction;
[0009] The catalyst is a composite catalytic material, which includes metal nanoparticles and molecular sieve composite catalytic material. The composite catalytic material includes an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve. The metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0010] Optionally, the composite catalytic material has the following FT-IR characteristics:
[0011] The wave number in the FT-IR spectrum of the composite catalytic material is 960 cm -1 The peak intensity is recorded as I1, and the wave number is 800cm -1 The peak intensity is recorded as I2,
[0012] I0 defined by the following formula (1) is any value between 0.5 and 1.3;
[0013] I0=I1 / I2 Formula (1);
[0014] Preferably, the value of I0 is any value between 0.6 and 1.3.
[0015] Optionally, the method further comprises: mixing the methacrolein and methanol and contacting the mixture with the catalyst;
[0016] Optionally, the molar ratio of methacrolein to methanol is 1:(50-200), preferably 1:(60-100).
[0017] Optionally, the conditions of the oxidative esterification reaction include: reaction temperature of 40-100° C., preferably 50-100° C.; time of 1-48 h, preferably 1-24 h; oxygen pressure of 0.1-0.5 MPa, preferably 0.1-0.3 MPa;
[0018] Optionally, the weight ratio of the catalyst to the methacrolein is 1:(1-20); preferably 1:(1-10);
[0019] Optionally, the reactor for the oxidation reaction includes any one of a tank reactor, a fixed bed reactor, a moving bed reactor, a suspended bed reactor and a slurry bed reactor.
[0020] Optionally, the all-silicon molecular sieve in the composite catalytic material is at least one of MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MWW structure molecular sieve, two-dimensional hexagonal structure molecular sieve, MOR structure molecular sieve and TUN structure molecular sieve; preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve.
[0021] Optionally, in the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.18):1, preferably (0.001-0.15):1.
[0022] Optionally, the BET specific surface area of the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65mL / g, the micropore volume is 0.1-0.19mL / g, the mesopore volume is 0.2-0.48mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5-9nm.
[0023] Optionally, the catalyst is prepared by a preparation method comprising the following steps:
[0024] S1, mixing a template, a silicon source, water, a metal M precursor, a nitrogen-containing ligand and a silanization agent to obtain a reaction mixture;
[0025] S2. performing hydrothermal crystallization and calcination on the reaction mixture.
[0026] Optionally, in step S1, the molar ratio of silicon source: template: water: metal element M: silanization agent calculated as SiO2 is 1: (0.001~1): (5~100): (0.001~0.18): (0.025~0.4), preferably 1: (0.001~0.5): (5~50): (0.001~0.15): (0.025~0.3); the molar ratio of nitrogen-containing ligand to metal element M is (0.2~2):1.
[0027] Optionally, step S1 includes:
[0028] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;
[0029] b. adding a nitrogen-containing ligand to an aqueous solution of a metal M precursor, and mixing the mixture to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material;
[0030] c. Adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.
[0031] Optionally, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably selected from at least one of organic silicone grease, solid silica gel and white carbon black; further preferably organic silicone grease, the general formula of the organic silicone grease is the structure shown in the following formula (A):
[0032]
[0033] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms; further preferably, the R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl; further preferably, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0034] Optionally, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium bases, aliphatic amines and aliphatic alcohol amines; further preferably, the template is at least one selected from quaternary ammonium bases having a structure represented by the following formula (B):
[0035] R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms, preferably a straight-chain alkyl group having 1 to 4 carbon atoms and a branched-chain alkyl group having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from at least one of a methyl group, an ethyl group, a n-propyl group, an isopropyl group, a n-butyl group, a sec-butyl group, an isobutyl group and a tert-butyl group;
[0036] Further preferably, the molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0037] The molecular sieve of the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0038] The molecular sieve of the composite catalytic material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
[0039] Optionally, in step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;
[0040] Optionally, the conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.
[0041] Optionally, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;
[0042] The metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold;
[0043] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0044] Optionally, in step S1, the general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group, and the amine group are each independently 1 to 18, and the number of carbon atoms of the aromatic group is 6 to 18;
[0045] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0046] Optionally, in step S1, the nitrogen-containing ligand is an alkylamine compound containing only an amino group or an amine compound containing other coordination groups, and the other coordination groups include one or more of hydroxyl, carboxyl, carbonyl, and thiol;
[0047] Preferably, the nitrogen-containing ligand is one or more of an alkylamine compound containing only an amino group having a structure shown in the following formula (C), an alcoholamine compound having a structure shown in the following formula (D), and an aminocarboxylic acid compound having a structure shown in the following formula (E):
[0048] R9(NH2) n Formula (C);
[0049] wherein n is 1 or 2; when n is 1, R9 is an alkyl group having 1 to 6 carbon atoms, preferably a linear alkyl group having 1 to 6 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms, and more preferably one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, isopentyl, tert-pentyl and n-hexyl; when n is 2, R9 is an alkylene group having 1 to 6 carbon atoms, preferably a linear alkylene group having 1 to 6 carbon atoms and a branched alkylene group having 3 to 6 carbon atoms, and more preferably one of methylene, ethylene, n-propylene, n-butylene, n-pentylene and n-hexylene;
[0050] (HOR 10 ) m NH (3m) Formula (D);
[0051] Where R 10 is an alkylene group having 1 to 4 carbon atoms and a branched alkylene group having 3 to 4 carbon atoms, preferably one of methylene, ethylene, n-propylene and n-butylene; m is 1, 2 or 3. When m is greater than 1, multiple R 10 Same or different;
[0052] (HOOCR 11 )x NH (3x) Formula (E);
[0053] Where R 11 is an alkylene group having 1 to 4 carbon atoms and a branched alkylene group having 3 to 4 carbon atoms, preferably one of methylene, ethylene, n-propylene and n-butylene; x is 1, 2 or 3. When x is greater than 1, multiple R 11 Same or different;
[0054] More preferably, the nitrogen-containing ligand is selected from one or more of ethylamine, ethylenediamine, ethanolamine and ethylenediaminetetraacetic acid.
[0055] Optionally, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200° C.;
[0056] Optionally, the conditions for the calcination treatment include: a calcination temperature of 400 to 900° C. and a calcination time of 1 to 16 hours; preferably, the calcination temperature is 400 to 800° C. and the calcination time is 2 to 8 hours.
[0057] Through the above technical scheme, the present disclosure provides a method for preparing methyl methacrylate by oxidation. The method uses oxygen as an oxidant to carry out a heterogeneous oxidation reaction, and uses a metal-containing multi-level porous molecular sieve as a catalyst to prepare methyl methacrylate by an oxidation reaction of methacrolein. The molecular sieve of the catalyst has a large specific surface area, pore volume and macromolecular substrate reaction activity, and the metal nanoparticles have a high dispersion in the molecular sieve, so that a high conversion rate of methacrolein and a high selectivity of methyl methacrylate can be obtained under relatively mild conditions.
[0058] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings:
[0060] Figure 1 The SEM spectrum of the product obtained in Preparation Example 1 is shown in FIG.
[0061] Figure 2 The XRD spectrum of the product obtained in Preparation Example 1 is shown in FIG.
[0062] Figure 3The FTIR spectrum of the product obtained in Preparation Example 1 is shown in FIG. DETAILED DESCRIPTION
[0063] The specific embodiments of the present disclosure are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present disclosure, and are not used to limit the present disclosure.
[0064] The present disclosure provides a method for preparing methyl methacrylate by oxidation, the method comprising the following steps:
[0065] Under oxygen conditions, methacrolein is contacted with a catalyst to carry out an oxidative esterification reaction;
[0066] The catalyst is a composite catalytic material, which includes an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve, wherein the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0067] The inventors of the present disclosure unexpectedly discovered that using a composite catalytic material of metal nanoparticles and molecular sieves as a catalyst to carry out an oxidation reaction of methacrolein under the action of the catalyst can effectively increase the oxidation reaction rate, shorten the reaction time, and achieve a high conversion rate of methacrolein and a high selectivity of methyl methacrylate under relatively mild conditions.
[0068] In a preferred embodiment, the composite catalytic material has the following FT-IR characteristics:
[0069] The wave number in the FT-IR spectrum of the composite catalytic material is 960 cm -1 The peak intensity of the highest peak at is recorded as I1, and the wave number is 800 cm -1 The peak intensity of the highest peak in the range is recorded as I2.
[0070] I0 defined by the following formula (1) is any value between 0.5 and 1.3;
[0071] I0=I1 / I2 Formula (1);
[0072] The molecular sieve of the composite catalyst material has a large specific surface area, pore volume and macromolecular substrate reaction activity; the molecular sieve of the composite catalyst material has a multi-level pore structure, and the metal oxide nanoparticles have uniform particle sizes and are evenly dispersed in the mesoporous channels of the multi-level pore molecular sieve; the composite catalyst material has high catalytic activity in the oxidative esterification reaction process of methacrolein.
[0073] The inventors of the present disclosure surprisingly found in a large number of experimental studies that when a metal precursor, a nitrogen-containing ligand and a silanization agent are introduced into the molecular sieve synthesis process, after the reaction mixture is subjected to hydrothermal crystallization, washing and calcination, the obtained composite catalytic material including all-silicon molecular sieve and metal M oxide nanoparticles not only has a large specific surface area and pore volume performance, but also the metal oxide nanoparticles have uniform particle size and are uniformly dispersed in the molecular sieve crystals (for example, in the molecular sieve mesoporous channels), and may also exist on the surface of the molecular sieve channels. The composite catalytic material has good catalytic activity in the reaction of methyl methacrylate preparation by oxidation of methacrolein; and the inventors also found that the obtained composite catalytic material has a wavelength of 960 cm in the infrared spectrum test. -1 The highest peak intensity (I1) in the range is 800cm -1 The ratio of the highest peak intensity (I2) in the range of 960 cm to 1000 cm is related to the catalytic performance of the composite catalytic material. In particular, when I0 (I0 = I1 / I2) satisfies 0.5 to 1.3, the composite catalytic material has good catalytic activity in the oxidative esterification reaction of methacrolein, and can obtain a higher methacrolein conversion rate and methyl methacrylate selectivity, and its catalytic activity is further improved. It should be understood that in the present disclosure, "960 cm -1 "Infrared spectrum 960cm -1 Within a certain range nearby, such as 955-965cm -1 , "800cm -1 "Infrared spectrum 800cm -1 Within a certain range nearby, such as 795-805cm -1 .
[0074] In a preferred embodiment, the value of I0 is any value between 0.6 and 1.3, and the composite catalytic material has higher catalytic activity when I0 is within this range.
[0075] In one embodiment, the method further comprises: mixing the methacrolein and methanol and contacting the mixture with the catalyst;
[0076] In a preferred embodiment, the molar ratio of methacrolein to methanol is 1:(50-200), preferably 1:(60-100).
[0077] In one embodiment, the conditions of the oxidative esterification reaction include: reaction temperature of 40-100° C., preferably 50-100° C.; reaction time of 1 to 48 hours, preferably 1 to 24 hours; oxygen pressure of 0.1 to 0.5 MPa, preferably 0.1 to 0.3 MPa;
[0078] The weight ratio of the catalyst to the methacrolein is 1:(1-20); preferably 1:(1-10);
[0079] In one embodiment, the reactor for the oxidation reaction includes any one of a tank reactor, a fixed bed reactor, a moving bed reactor, a suspended bed reactor and a slurry bed reactor.
[0080] In one embodiment, the all-silicon molecular sieve in the composite catalytic material is one or more of MFI structure molecular sieve (such as S-1), MEL structure molecular sieve (such as S-2), BEA structure molecular sieve (such as Beta), MWW structure molecular sieve (such as MCM-22), two-dimensional hexagonal structure molecular sieve (such as MCM-41, SBA-15), MOR structure molecular sieve (such as MOR), TUN structure molecular sieve (such as TUN) and silicon molecular sieves of other structures (such as ZSM-48, MCM-48); preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve; further preferably, it is one or more selected from MFI structure molecular sieve, MEL structure molecular sieve and BEA structure molecular sieve, such as the silicon molecular sieve is one of S-1, S-2 and Beta; further preferably, it is an MFI structure molecular sieve, such as S-1.
[0081] In one embodiment, the metal M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold.
[0082] In one embodiment, the composite catalytic material includes silicon element, metal element M and oxygen element, and the molar ratio of the metal element M to the silicon element is (0.001-0.18):1, preferably (0.001-0.15):1.
[0083] In one embodiment, the BET specific surface area of the composite catalytic material is 400 to 800 m 2 / g, the total pore volume is 0.3-0.65mL / g, the micropore volume is 0.1-0.19mL / g, the mesopore volume is 0.2-0.48mL / g, and the average particle size of the metal nanoparticles in the composite catalytic material is 0.5-9nm. The composite catalytic material in the present disclosure also has a multi-level pore structure, which is conducive to catalyzing reaction substrates of different sizes.
[0084] In one embodiment, the catalyst is prepared by a preparation method comprising the following steps:
[0085] S1, mixing a template, a silicon source, water, a metal M precursor, a nitrogen-containing ligand and a silanization agent to obtain a reaction mixture;
[0086] S2. performing hydrothermal crystallization and calcination on the reaction mixture.
[0087] The present invention introduces a metal precursor, a nitrogen-containing ligand and a silanization agent into the raw materials for the crystallization synthesis of the molecular sieve, which can simultaneously achieve the effects of highly dispersing metal oxide nanoparticles in the molecular sieve crystals and expanding the pores of the molecular sieve support layer, thereby preparing a multi-level porous molecular sieve composite catalytic material with highly dispersed metal oxide nanoparticles.
[0088] In the present disclosure, on the one hand, the metal ions in the reaction mixture are complexed with the nitrogen-containing ligands to achieve the effect of dispersing and stabilizing the metal; at the same time, at least one coordination group of the silanization agent can also be complexed with the metal ions to achieve the effect of fixing and dispersing the metal, so that the metal oxide nanoparticles in the molecular sieve pores obtained after hydrothermal crystallization and calcination have high dispersion; on the other hand, the alkyl chain of the silanization agent also ensures the realization of the molecular sieve support layer expansion effect of the synthesized composite catalyst material. Thus, a multi-level porous all-silicon molecular sieve composite catalyst material with highly dispersed metal nanoparticles is finally prepared.
[0089] In one embodiment, in step S1, the molar ratio of SiO2: template: water: metal M element: silanization agent in the reaction mixture is 1: (0.001-1): (5-100): (0.001-0.18): (0.025-0.4), preferably 1: (0.001-0.5): (5-50): (0.001-0.15): (0.025-0.3); the molar ratio of nitrogen-containing ligand to metal element M is (0.2-2): 1. Specifically, the water used in step S1 can be water commonly used in the synthesis of molecular sieves, and in order to avoid the introduction of heteroatoms, it is preferably deionized water.
[0090] In a preferred embodiment, step S1 comprises:
[0091] a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution;
[0092] b. adding a nitrogen-containing ligand to an aqueous solution of a metal M precursor, and mixing the mixture to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material;
[0093] c. Adding a silanization agent to the second mixed material, and mixing to obtain the reaction mixture; preferably, the mixing conditions in step c include: stirring at 20 to 80° C. for 0.5 to 2 hours.
[0094] In one embodiment, in step S1, the silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol; preferably, it is selected from at least one of organic silicone grease, solid silica gel and white carbon black; the general formula of the organic silicone grease is the structure shown in the following formula (A):
[0095]
[0096] Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, wherein the alkyl group is a branched or straight chain alkyl group; preferably, R a , R b , R c , R d Each is independently selected from a straight chain alkyl group having 1 to 4 carbon atoms or a branched chain alkyl group having 3 to 4 carbon atoms. a , R b , R c , R d Each is independently methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl. a , R b , R c , R d Each is independently methyl or ethyl.
[0097] In a preferred embodiment, the organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
[0098] According to the present disclosure, in step S1, the template is an organic base, preferably at least one selected from quaternary ammonium base, aliphatic amine and aliphatic alcohol amine. The quaternary ammonium base may be an organic quaternary ammonium base; the aliphatic amine may be a compound formed by replacing at least one hydrogen in NH3 with an aliphatic hydrocarbon group (such as an alkyl group); the aliphatic alcohol amine may be a compound formed by replacing at least one hydrogen in various NH3 with an aliphatic group (such as an alkyl group) containing a hydroxyl group.
[0099] Further preferably, the template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B):
[0100] R1, R2, R3 and R4 are independently selected from alkyl groups having 1 to 4 carbon atoms, preferably straight-chain alkyl groups having 1 to 4 carbon atoms and branched-chain alkyl groups having 3 to 4 carbon atoms, more preferably R1, R2, R3 and R4 are independently selected from at least one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
[0101] The template agent is preferably at least one of tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide (including various isomers of tetrapropylammonium hydroxide, such as tetra-n-propylammonium hydroxide and tetraisopropylammonium hydroxide) and tetrabutylammonium hydroxide (including various isomers of tetrabutylammonium hydroxide, such as tetra-n-butylammonium hydroxide and tetraisobutylammonium hydroxide).
[0102] In a preferred embodiment, the molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or
[0103] The molecular sieve of the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or
[0104] The molecular sieve of the composite catalytic material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide. The present disclosure can prepare molecular sieves of different structures by selecting different template agents.
[0105] In one embodiment, in step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is further performed to obtain a hydrolyzed solution of the silicon;
[0106] The conditions for the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0 to 95° C. for 2 to 10 hours; preferably stirring and hydrolyzing at 50 to 95° C. for 2 to 8 hours.
[0107] Preferably, the hydrolysis-alcohol removal treatment is performed so that the mass content of alcohol produced by hydrolysis of the obtained organic silicone grease in the hydrolysis solution of silicon is less than 10 ppm.
[0108] According to the present disclosure, the optional range of types of the metal precursor is relatively wide, and any substance containing the metal (such as a compound containing a metal element and / or a metal single substance) can achieve the purpose of the present disclosure.
[0109] In one embodiment, in step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the organic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M; preferably, the metal M precursor is a water-soluble inorganic salt of metal M;
[0110] Preferably, the metal M precursor is an aqueous solution of a metal M precursor, and the molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
[0111] In one embodiment, in step S1, the general formula of the silanization reagent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group, and the amine group are each independently 1 to 18 carbon atoms, preferably 1 to 12; the number of carbon atoms of the aromatic group can be 6 to 18, preferably 6 to 12.
[0112] Preferably, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, 1,7-dichlorooctylmethyltetrasiloxane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane; further preferably, it is at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
[0113] In one embodiment, in step S1, the nitrogen-containing ligand is an alkylamine compound containing only amino groups or an amine compound containing other coordination groups, and the other coordination groups include one or more of hydroxyl, carboxyl, carbonyl, and thiol. In the present disclosure, the "alkylamine compound containing only amino groups" means that the alkylamine compound contains only amino groups, which is a nitrogen-containing group, and does not contain other types of nitrogen-containing groups, but the number of amino groups contained can be one or more.
[0114] Preferably, the nitrogen-containing ligand is one or more of an alkylamine compound containing only an amino group having a structure shown in the following formula (C), an alcoholamine compound having a structure shown in the following formula (D), and an aminocarboxylic acid compound having a structure shown in the following formula (E):
[0115] R9(NH2) n Formula (C); wherein n is 1 or 2; when n is 1, R9 is an alkyl group having 1 to 6 carbon atoms, preferably a linear alkyl group having 1 to 6 carbon atoms and a branched alkyl group having 3 to 6 carbon atoms, and more preferably one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, isopentyl, tert-pentyl and n-hexyl; when n is 2, R9 is an alkylene group having 1 to 6 carbon atoms, preferably a linear alkylene group having 1 to 6 carbon atoms and a branched alkylene group having 3 to 6 carbon atoms, and more preferably one of methylene, ethylene, n-propylene, n-butylene, n-pentylene and n-hexylene;
[0116] (HOR 10 ) m NH (3m) Formula (D); wherein R 10 is an alkylene group having 1 to 4 carbon atoms and a branched alkylene group having 3 to 4 carbon atoms, preferably one of methylene, ethylene, n-propylene and n-butylene; m is 1, 2 or 3. When m is greater than 1, multiple R 10 Same or different;
[0117] (HOOCR 11 ) x NH (3x) Formula (E); wherein R 11 is an alkylene group having 1 to 4 carbon atoms and a branched alkylene group having 3 to 4 carbon atoms, preferably one of methylene, ethylene, n-propylene and n-butylene; x is 1, 2 or 3. When x is greater than 1, multiple R 11 Same or different;
[0118] More preferably, the nitrogen-containing ligand is selected from one or more of ethylamine, ethylenediamine, ethanolamine and ethylenediaminetetraacetic acid.
[0119] In one embodiment, in step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200°C; preferably, the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C.
[0120] In one embodiment, in step S2, the conditions of the calcination treatment include: a calcination temperature of 400-900° C., and a calcination time of 1-16 hours; preferably, the calcination temperature is 400-800° C., and the calcination time is 2-8 hours.
[0121] The present disclosure is further described in detail below through examples.
[0122] In the present disclosure, the X-ray diffraction (XRD) crystal phase diagram of the sample is measured on a Siemens D5005 X-ray diffractometer, the radiation source is Kα (Cu), and the test range 2θ is 0.5° to 70°.
[0123] The SEM images of the samples were obtained on a Hitachi S4800 high-resolution cold field emission scanning electron microscope.
[0124] The Fourier transform infrared (FT-IR) spectra of the samples were measured on a Nicolet 8210 Fourier transform infrared spectrometer in the range of 400 to 4000 cm -1 .
[0125] The total specific surface area and total pore volume of the sample were measured on a Micromeritics ASAP245 static nitrogen adsorption instrument according to the ASTM D4222-98 standard method. The adsorption isotherm and desorption isotherm of low-temperature nitrogen adsorption of the sample were measured according to the ASTM D4222-98 standard method.
[0126] Preparation Example 1
[0127] (1) 1.6 g of a 25.05 wt % tetrapropylammonium hydroxide (TPAOH) aqueous solution, 20.8 g of tetraethyl silicate and 52.8 g of water were added to a 500 mL beaker in sequence, placed on a magnetic stirrer with heating and stirring functions to mix evenly, and stirred at 50° C. for 2 hours, and the evaporated water was replenished regularly to obtain a colorless and transparent silica gel solution;
[0128] (2) 0.036 g of sodium chloroaurate and 0.18 g of water were mixed, 0.05 mmol of β-mercaptoethylamine was added, and the aqueous solution was mixed with the hydrolyzed silicon solution obtained in step (1);
[0129] (3) adding 0.64 g of 3-mercaptopropyltrimethoxysilane (3-TSPE) to the mixture of step (2) and stirring for 0.5 hour;
[0130] (4) The mixture obtained in step (3) was transferred to a stainless steel closed reactor, and crystallized at a constant temperature of 175° C. for 24 hours to obtain a sample, and the obtained sample was filtered, washed, dried at 110° C. for 6 hours, and then calcined in a muffle furnace at 550° C. for 6 hours to obtain a metal nanoparticle and molecular sieve composite catalytic material product, and the obtained product was recorded as CAT-1;
[0131] The average particle size, BET specific surface area, total pore volume, micropore volume and mesopore volume of CAT-1 are listed in Table 2. The SEM image of CAT-1 is shown in Figure 1 The XRD spectrum of CAT-1 is shown in Figure 2 As shown in Figure 2, XRD analysis shows that it has an MFI structure; the TEM image of CAT-1 is shown in Figure 2. Figure 3 As shown; the infrared spectrum of CAT-1 is as shown Figure 3 As shown in the infrared spectrum of this sample, 960 cm -1 The peak intensity of the highest peak at 800 cm (absorbance 5.1%) is -1 The ratio I0 of the peak intensity of the highest peak (absorbance is 7.5%) is 0.68. Figure 1 It can be seen that the products prepared in this example have regular shapes and uniform sizes; Figure 3 Medium 960cm -1 The characteristic peaks nearby indicate that there is interaction between Au and the silicon skeleton.
[0132] Preparation Examples 2 to 9
[0133] The corresponding products CAT-2 to CAT-9 were prepared according to the method of Preparation Example 1. The ratios, synthesis conditions and results are shown in Table 1. Other conditions and operations refer to Example 1. The SEM images are similar to those of Figure 1 Similar; XRD analysis shows that it has MFI structure, and the XRD spectrum is similar to Figure 2 Similar; its TEM image is Figure 3 Similar; its FT-IR spectrum is Figure 3 similar.
[0134] Preparation Example 10
[0135] The cobalt-containing multi-level porous β molecular sieve was prepared by referring to the method of Example 1, but changing the ratio and template agent. The template agent used was tetraethylammonium hydroxide (TEAOH). The obtained product was recorded as CAT-10. The ratio, synthesis conditions and results are shown in Table 1.
[0136] Preparation Example 11
[0137] The cobalt-containing multi-level porous MEL molecular sieve was prepared by referring to the method of Example 1, changing the ratio and template agent, and using tetrabutylammonium hydroxide (TBAOH) as the template agent. The obtained product was recorded as CAT-11. The ratio, synthesis conditions and results are shown in Table 1.
[0138] Preparation Example 12
[0139] The corresponding product was prepared according to the method of Example 1, and its ratio, synthesis conditions and results are listed in Table 1. Other conditions and operations refer to those of Preparation Example 1, and the obtained product is recorded as CAT-12. Among them, the hydrothermal crystallization temperature is 120°C, the time is 8 days, the calcination temperature is 850°C, and the calcination time is 10 hours.
[0140] Preparation Comparative Example 1
[0141] The product was prepared according to the method of Preparation Example 1, except that no silanization agent was added. The obtained product was recorded as DCAT-1.
[0142] Preparation Comparative Example 2
[0143] 0.036g of sodium chloroaurate and 0.18g of water were stirred evenly to obtain a gold aqueous solution. Then 10.2g of alumina carrier was added, stirred for 4h, the solvent was evaporated, the solid was collected and dried at 110°C for 6h, and then calcined at 550°C in a muffle furnace for 6h. The obtained product was recorded as DCAT-2.
[0144] Preparation Comparative Example 3
[0145] 0.036g of sodium chloroaurate and 0.18g of water were stirred evenly to obtain a gold aqueous solution, and then 6g of all-silicon MFI molecular sieve carrier was added, stirred for 4h, the solvent was evaporated, the solid was collected and dried at 110°C for 6 hours, and then calcined at 550°C in a muffle furnace for 6 hours. The obtained product was recorded as DCAT-3. The preparation process of all-silicon MFI molecular sieve is referred to Preparation Example 1, which is different from Preparation Example 1 in that sodium chloroaurate and β-mercaptoethylamine are not introduced in the molecular sieve synthesis process, and the rest of the process is the same as Preparation Example 1.
[0146] The BET specific surface area, total pore volume, micropore volume and mesopore volume of the products obtained in the above examples and comparative examples, and the average particle size of the metal nanoparticles of the composite catalytic material are listed in Table 2 below.
[0147] Table 1
[0148]
[0149]
[0150] In Table 1, the cobalt nitrate used is cobalt nitrate hexahydrate; TPAOH is tetrapropylammonium hydroxide, TPABr is tetrapropylammonium bromide, TBAOH is tetrabutylammonium hydroxide, TEAOH is tetraethylammonium hydroxide; PHAPTMS is N-phenyl-3-aminopropyltrimethoxysilane, APTES is 3-aminopropyltriethoxysilane, KH792 is silane coupling agent kh792 (bisamino functional group silane); 3-TSPE is 3-mercaptopropyltrimethoxysilane;. The reagents used in the present disclosure can be obtained through conventional purchasing channels.
[0151] Table 2
[0152]
[0153] Among them, pores with a diameter less than 2nm are micropores, and pores with a diameter between 2 and 50nm are mesopores.
[0154] According to Table 2, compared with Comparative Example 1 (without adding silanization agent), the products obtained by adding silanization agent during the preparation process of Examples 1 to 12 of the present disclosure have higher mesopore volume, indicating that the method provided by the present disclosure can effectively expand the pores of the molecular sieve.
[0155] Compared with DCAT-2 and DCAT-3, the composite catalytic materials CAT-1 to CAT-12 provided in the present disclosure can simultaneously have a large mesopore volume, a large specific surface area and a smaller metal nanoparticle size, indicating that the metal nanoparticles in the composite catalytic materials obtained in the present disclosure have a lower degree of aggregation and a higher degree of dispersion.
[0156] Reaction Example 1
[0157] This is used to illustrate the reaction effect of the oxidative esterification of methacrolein provided by the present invention.
[0158] The samples prepared in the above-mentioned preparation examples and comparative examples were used to catalyze the oxidative dehydrogenation of methacrolein. Methacrolein was mixed with a methanol solvent (the molar ratio of methacrolein to methanol was controlled to be 1:62.5), and then contacted with 30 mg of the catalyst in a slurry bed reactor (the specific weight ratio of methacrolein to catalyst is shown in Table 3). The contact temperature was 60° C., the contact time was 2 h, and the oxygen pressure was 0.1 MPa. The results are shown in Table 3 below.
[0159] Methacrolein conversion rate (%) = number of moles of methacrolein participating in the reaction / number of moles of methacrolein added×100%.
[0160] Methyl methacrylate selectivity (%) = number of moles of methyl methacrylate / number of moles of methacrolein participating in the reaction×100%.
[0161] The molar number of methacrolein participating in the reaction = the molar number of methacrolein fed - the molar number of methacrolein remaining in the obtained reaction mixture.
[0162] Table 3
[0163]
[0164]
[0165] It can be seen from the results in Table 3 that, compared with Comparative Examples 1-3, the composite catalytic materials I0 prepared in Examples 1 to 12 of the present disclosure are in the range of 0.5 to 1.3, and the composite catalytic materials have higher catalytic activity. Under relatively mild reaction conditions (60° C.), more than 80% ketone conversion rate and more than 80% lactone selectivity can be obtained in 24 hours.
[0166] Comparing Preparation Examples 1 to 11 with Preparation Example 12, the composite catalytic material I0 prepared in Preparation Examples 1 to 11 is in the range of 0.6 to 1.3, and Examples 1 to 11 have better catalytic effects, and have higher ketone conversion rates and lactone selectivities.
[0167] Reaction Examples 2 to 3
[0168] Referring to the reaction method and conditions of Reaction Example 1, the composite catalytic material CAT-4 obtained in Preparation Example 4 was used, and methacrolein was used as a raw material to test the reaction effects under different oxidation reaction conditions. The specific reaction conditions and reaction results are listed in Table 4 below.
[0169] Table 4
[0170]
[0171] Comparing Reaction Example 2 with Reaction Example 3, it can be seen that when the reaction is carried out at 60° C. (satisfying the range of 50-100° C.) in Reaction Example 2, the oxidation reaction effect is better, and the methacrolein conversion rate and methyl methacrylate selectivity are higher.
[0172] The preferred embodiments of the present disclosure are described in detail above; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.
[0173] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.
[0174] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.
Claims
1. A method for preparing methyl methacrylate by oxidation, characterized in that: The method comprises the following steps: Under oxygen conditions, methacrolein is contacted with a catalyst to carry out an oxidative esterification reaction; The catalyst is a composite catalytic material, which includes an all-silicon molecular sieve and a metal element M dispersed in the crystal of the all-silicon molecular sieve, wherein the metal element M is selected from one or more of manganese, iron, cobalt, nickel, palladium, platinum, copper and gold; The composite catalytic material has the following FT-IR characteristics: The wave number in the FT-IR spectrum of the composite catalytic material is 960 cm -1 The peak intensity is recorded as I1, and the wave number is 800 cm -1 The peak intensity is recorded as I2, I0 defined by the following formula (1) is any value between 0.5 and 1.3; I0= I1 / I2 (1); The composite catalytic material is prepared by a method comprising the following steps: S1, mixing a template, a silicon source, water, a metal M precursor, a nitrogen-containing ligand and a silanization agent to obtain a reaction mixture; S2, subjecting the reaction mixture to hydrothermal crystallization and calcination treatments; The general formula of the silanization agent is R5Si(R6)(R7)R8, wherein R5, R6, R7, and R8 are each independently a halogen, an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group, and at least one of R5, R6, R7, and R8 is an alkyl group, an alkoxy group, an aromatic group, a thiol group, or an amine group; the number of carbon atoms of the alkyl group, the alkoxy group, the thiol group, and the amine group are each independently 1 to 18, and the number of carbon atoms of the aromatic group is 6 to 18; The nitrogen-containing ligand is an alkylamine compound containing only an amino group or an amine compound containing other coordination groups, and the other coordination groups include one or more of hydroxyl, carboxyl, carbonyl, and thiol.
2. The method according to claim 1, characterized in that The value of I0 is any value between 0.6 and 1.
3.
3. The method according to claim 1, characterized in that The method further comprises: mixing the methacrolein and methanol and contacting the mixture with the catalyst; The molar ratio of methacrolein to methanol is 1:(50-200).
4. The method according to claim 3, characterized in that The molar ratio of methacrolein to methanol is 1:(60-100).
5. The method according to claim 1, characterized in that The conditions of the oxidative esterification reaction include: reaction temperature of 40-100°C; time of 1-48h; oxygen pressure of 0.1-0.5MPa; The weight ratio of the catalyst to the methacrolein is 1:(1-20).
6. The method according to claim 5, characterized in that The conditions of the oxidative esterification reaction include: reaction temperature of 50-100° C.; reaction time of 1-24 h; oxygen pressure of 0.1-0.3 MPa; The weight ratio of the catalyst to the methacrolein is 1:(1-10).
7. The method according to claim 1, characterized in that The reactor for the oxidation reaction includes any one of a tank reactor, a fixed bed reactor, a moving bed reactor, a suspended bed reactor and a slurry bed reactor.
8. The method according to claim 1, characterized in that The all-silicon molecular sieve in the composite catalytic material is at least one of an MFI structure molecular sieve, a MEL structure molecular sieve, a BEA structure molecular sieve, an MWW structure molecular sieve, a two-dimensional hexagonal structure molecular sieve, a MOR structure molecular sieve and a TUN structure molecular sieve.
9. The method according to claim 8, characterized in that The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the MFI structure molecular sieve, MEL structure molecular sieve, BEA structure molecular sieve, MCM structure molecular sieve and SBA structure molecular sieve.
10. The method according to claim 9, characterized in that The all-silicon molecular sieve in the composite catalytic material is selected from one or more of the MFI structure molecular sieve, the MEL structure molecular sieve and the BEA structure molecular sieve.
11. The method according to claim 1, characterized in that: In the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.18):
1.
12. The method according to claim 11, characterized in that In the composite catalytic material, the molar ratio of the metal element M to the silicon element is (0.001-0.15):
1.
13. The method according to claim 1, characterized in that The BET specific surface area of the composite catalytic material is 400-800 m 2 / g, the total pore volume is 0.3~0.65mL / g, the micropore volume is 0.1~0.19mL / g, the mesopore volume is 0.2~0.48mL / g, and the metal element M in the composite catalytic material exists in the form of metal nanoparticles, and the average particle size of the metal nanoparticles is 0.5~9nm.
14. The method according to claim 1, characterized in that In step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent calculated as SiO2 is 1: (0.001~1): (5~100): (0.001~0.18): (0.025~0.4); the molar ratio of nitrogen-containing ligand to metal element M is (0.2~2):
1.
15. The method according to claim 14, characterized in that In step S1, the molar ratio of silicon source: template: water: metal M element: silanization agent calculated as SiO2 is 1: (0.001-0.5): (5-50): (0.001-0.15): (0.025-0.3).
16. The method according to claim 1, characterized in that Step S1 includes: a. mixing a template, a silicon source and water to obtain a silicon hydrolysis solution; b. adding a nitrogen-containing ligand to an aqueous solution of a metal M precursor, and mixing the mixture to obtain a first mixed material; and mixing the first mixed material with the hydrolyzed silicon solution to obtain a second mixed material; c. Adding a silanization agent into the second mixed material and mixing them to obtain the reaction mixture.
17. The method according to claim 16, characterized in that The mixing conditions in step c include: stirring at 20-80° C. for 0.5-2 hours.
18. The method according to claim 1, characterized in that The silicon source is selected from at least one of organic silicone grease, solid silica gel, white carbon black and silica sol.
19. The method according to claim 18, characterized in that The silicon source is selected from at least one of organic silicone grease, solid silica gel and white carbon black.
20. The method according to claim 19, characterized in that The silicon source is organic silicone grease, and the general formula of the organic silicone grease is the structure shown in the following formula (A): (A); Where R a , R b , R c , R d Each is independently selected from an alkyl group having 1 to 6 carbon atoms, and the alkyl group is a branched or straight chain alkyl group.
21. The method according to claim 20, characterized in that In formula (A), R a , R b , R c , R d Each is independently selected from a straight-chain alkyl group having 1 to 4 carbon atoms or a branched-chain alkyl group having 3 to 4 carbon atoms.
22. The method according to claim 21, characterized in that In formula (A), R a , R b , R c , R d Each is independently selected from methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl or tert-butyl.
23. The method according to claim 22, characterized in that The organic silicone grease is selected from one or more of tetramethyl silicate, tetraethyl silicate, tetrabutyl silicate and dimethyl diethyl silicone grease.
24. The method according to claim 1, characterized in that In step S1, the template agent is an organic base.
25. The method according to claim 24, characterized in that The template agent is selected from at least one of quaternary ammonium base, aliphatic amine and aliphatic alcohol amine.
26. The method according to claim 25, characterized in that The template is selected from at least one quaternary ammonium base having a structure represented by the following formula (B): (B); R1, R2, R3 and R4 are independently selected from an alkyl group having 1 to 4 carbon atoms.
27. The method according to claim 26, characterized in that In formula (B), R1, R2, R3 and R4 are independently selected from a linear alkyl group having 1 to 4 carbon atoms and a branched alkyl group having 3 to 4 carbon atoms.
28. The method according to claim 27, characterized in that In formula (B), R1, R2, R3 and R4 are independently selected from at least one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl and tert-butyl.
29. The method according to claim 1, characterized in that The molecular sieve of the composite catalyst material is an MFI type molecular sieve, and the template agent is tetrapropylammonium hydroxide or a mixture of tetrapropylammonium hydroxide and one or more selected from tetrapropylammonium chloride and tetrapropylammonium bromide; or The molecular sieve of the composite catalytic material is a MEL type molecular sieve, and the template agent is tetrabutylammonium hydroxide or a mixture of tetrabutylammonium hydroxide and one or more selected from tetrabutylammonium chloride and tetrabutylammonium bromide; or The molecular sieve of the composite catalytic material is a BEA type molecular sieve, and the template agent is tetraethylammonium hydroxide or a mixture of tetraethylammonium hydroxide and one or more selected from tetraethylammonium chloride and tetraethylammonium bromide.
30. The method according to claim 16, characterized in that In step a, the silicon source is organic silicone grease, and after the template, the organic silicone grease and water are mixed, a hydrolysis and alcohol removal treatment is also performed to obtain a hydrolyzed solution of the silicon; The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 0-95° C. for 2-10 hours.
31. The method according to claim 30, characterized in that The conditions of the hydrolysis and alcohol removal treatment include: stirring and hydrolyzing at 50-95° C. for 2-8 hours.
32. The method according to claim 1, characterized in that In step S1, the metal M precursor is one or more of an inorganic metal compound and an organic metal compound; the inorganic metal compound is a water-soluble inorganic salt of metal M; the water-soluble inorganic salt of metal M is selected from one or more of the chloride, hydrated chloride, sulfate, hydrated sulfate and nitrate of metal M; the organic metal compound is an organic ligand compound of metal M.
33. The method according to claim 32, characterized in that The metal M precursor is a water-soluble inorganic salt of metal M.
34. The method according to claim 16, characterized in that The molar ratio of the metal M element to water in the aqueous solution of the metal M precursor is 1:(50-500).
35. The method according to claim 1, characterized in that In step S1, the silanization agent is selected from one or more of dimethyldichlorosilane, N-phenyl-3-aminopropyltrimethoxysilane, phenyltrimethoxysilane, hexadecyltrimethoxysilane, octyltriethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
36. The method according to claim 35, characterized in that The silanization agent is selected from at least one of N-phenyl-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane and 3-mercaptopropyltrimethoxysilane.
37. The method according to claim 1, characterized in that In step S1, the nitrogen-containing ligand is one or more of an alkylamine compound containing only amino groups having a structure shown in the following formula (C), ethanolamine and ethylenediaminetetraacetic acid; R9(NH2) n Formula (C); Wherein, n is 1 or 2; when n is 1, R9 is an alkyl group having 1 to 6 carbon atoms; when n is 2, R9 is an alkylene group having 1 to 6 carbon atoms.
38. The method according to claim 37, characterized in that In formula (C), when n is 1, R9 is a straight-chain alkyl group having 1 to 6 carbon atoms and a branched-chain alkyl group having 3 to 6 carbon atoms; when n is 2, R9 is a straight-chain alkylene group having 1 to 6 carbon atoms and a branched-chain alkylene group having 3 to 6 carbon atoms.
39. The method according to claim 38, characterized in that In formula (C), when n is 1, R9 is selected from one of methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, isobutyl, tert-butyl, n-pentyl, neopentyl, isopentyl, tert-pentyl and n-hexyl; when n is 2, R9 is selected from one of methylene, ethylene, n-propylene, n-butylene, n-pentylene and n-hexylene.
40. The method according to claim 37, characterized in that The nitrogen-containing ligand is selected from one or more of ethylamine, ethylenediamine, ethanolamine and ethylenediaminetetraacetic acid.
41. The method according to claim 1, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: under autogenous pressure conditions, the hydrothermal crystallization time is 0.5 to 10 days, and the hydrothermal crystallization temperature is 110 to 200° C.; The conditions of the calcination treatment include: a calcination temperature of 400-900° C. and a calcination time of 1-16 hours.
42. The method according to claim 41, characterized in that In step S2, the conditions of the hydrothermal crystallization treatment include: the hydrothermal crystallization time is 0.5 to 5 days, and the hydrothermal crystallization temperature is 150 to 200°C; The conditions of the calcination treatment include: a calcination temperature of 400-800° C. and a calcination time of 2-8 hours.