A nano-titanium dioxide doped Sn-Ag-Cu-X quaternary solder and preparation method thereof
By adding nano titanium dioxide and wettability improver to Sn-Ag-Cu solder, the problem of poor wettability and mechanical properties of lead-free solder is solved, and the high wettability and shear strength of the solder are improved. The stability and reliability of the solder joints are ensured.
Patent Information
- Application Number
- CN202310163949.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-24
AI Technical Summary
Sn-Ag-Cu lead-free solder has poor wetting properties and mechanical properties, and the addition of doping amounts such as Ga, Nd and In is limited, which can easily lead to uneven distribution of gallium-rich, neodymium-rich or indium-rich phases, affecting the solder. performance.
Add nanometer titanium dioxide (TiO2) and wettability improver X (Nd, Ga or In) to Sn-Ag-Cu solder to improve the wettability and mechanical properties of the solder. The crystalline state and mixed crystal structure of nanometer TiO2 prevent The growth of the β-Sn phase and the growth of IMC reduce the formation of gallium-rich, neodymium-rich or indium-rich phases and improve the shear strength of the solder joints.
It significantly improves the wettability of solder and the shear strength of solder joints, weakens the negative effects caused by excessive addition of Ga, Nd or In, and improves the mechanical properties and reliability of solder joints.
Smart Images

Figure BDA0004095225080000071 
Figure BDA0004095225080000081 
Figure BDA0004095225080000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of tin-silver-copper alloy solder, and more specifically, to a nano-titanium dioxide-doped Sn-Ag-Cu-X quaternary solder and a preparation method thereof. Background Art
[0002] The solders used in large quantities for microelectronic packaging and assembly are mainly Sn-Pb solders. However, when electronic products and equipment are discarded as general industrial waste and domestic garbage, the lead in the solder will dissolve and enter the groundwater, causing great harm to the environment and human health. Therefore, in recent years, many countries, including my country, have formulated or are formulating laws and regulations to restrict the use of lead-containing substances. Therefore, replacing traditional Sn-Pb lead-containing solders with lead-free solders has become an irreversible trend in the global microelectronics manufacturing field, and actively looking for new non-toxic and harmless solders has also become an important task in the current electronics industry.
[0003] Based on the requirements of environmental friendliness, Sn-Ag-Cu lead-free solder is popular among people. Compared with Sn-Pb solder, the mechanical properties of Sn-Ag-Cu lead-free solder are better, but its process performance is not good. Therefore, the relevant properties of Sn-Ag-Cu lead-free solder are usually improved by adding rare earth elements and non-rare earth elements. The added rare earth elements include Nd, Ce, Y, La, Er and Pr, and the non-rare earth elements include Ga, Ti, Bi, Fe and In. However, due to the large differences in the properties of different rare earth elements and non-rare earth elements, it is not possible to add any one or more of them at random to have a positive effect on the performance of Sn-Ag-Cu lead-free solder. For example, the addition of 3.5% Bi can change the microstructure of Sn-Ag-Cu lead-free solder to a certain extent, but it will also promote the appearance of more large-sized β-Sn dendrites, which will have an adverse effect on the mechanical properties and reliability of the solder; for another example, the addition of appropriate amounts of Nd and Pr can improve the comprehensive performance of Sn-Ag-Cu lead-free solder, but excessive addition of Nd and Pr will cause more rare earth phases to appear in the structure, which will reduce the performance of Sn-Ag-Cu lead-free solder.
[0004] The doping of Ga, Nd and In can further improve the fluidity and wetting properties of Sn-Ag-Cu lead-free solder; however, the amount of addition should not be too high, otherwise it will have an adverse effect on the wetting properties and mechanical properties of Sn-Ag-Cu lead-free solder. Therefore, it is necessary to propose a method to further improve the performance of Sn-Ag-Cu lead-free solder doped with Ga, Nd and In. Summary of the invention
[0005] In order to improve the poor wetting and mechanical properties of Ga, Nd and In doped Sn-Ag-Cu lead-free solder, the present application provides a nano-titanium dioxide doped Sn-Ag-Cu-X quaternary solder and a preparation method thereof.
[0006] In the first aspect, the present application provides a nano-titanium dioxide doped Sn-Ag-Cu-X quaternary solder, which adopts the following technical solution:
[0007] A nano-titanium dioxide doped Sn-Ag-Cu-X quaternary solder, the components and mass percentages of which are: 0.1-0.3% nano-TiO2, 0.3-0.7% Ag, 0.5-0.9% Cu, 0.4-0.6% wettability improver X, and the balance is Sn; the nano-TiO2 is in a crystalline state and is a mixed crystal; the wettability improver X is selected from any one of Nd, Ga and In.
[0008] In the present application, Sn is added from tin ingot as a raw material, Ag is added from metallic silver, Cu is added from electrolytic copper as a raw material, Ga is added from metallic gallium as a raw material, Nd is added from metallic neodymium as a raw material, and In is added from metallic indium as a raw material.
[0009] Ga, Nd and In doping can further improve the fluidity of Sn-Ag-Cu lead-free solder and improve its wetting performance; however, the addition amount of these elements is limited. Generally, when they are added to 0.3-0.5wt% (especially when the addition amount is 0.5wt%), they will have a negative impact on the wettability of Sn-Ag-Cu lead-free solder, which is mainly caused by the uneven distribution of gallium-rich, neodymium-rich or indium-rich phases. In other words, although Ga, Nd and In doping can improve the wettability of Sn-Ag-Cu lead-free solder, the degree of improvement in wettability is also limited.
[0010] Add any one of Nd, Ga and In to the Sn-Ag-Cu solder to improve the wettability of the solder; but it should be noted here that the amount of Nd, Ga or In added is 0.4-0.6wt%, which is more than the amount added in related studies. Nano-TiO2 is added together with Nd, Ga or In. On the one hand, nano-TiO2 itself has the effect of improving the wettability of the solder. On the other hand, the addition of nano-TiO2 can overcome the negative impact on the wettability of the solder caused by excessive addition of Nd, Ga or In to a certain extent. Nano-TiO2 is in a crystalline state. Its crystalline state can first form nucleation particles when the β-Sn phase solidifies to prevent the β-Sn phase from growing into large dendrites. Based on the advantage of the nano-particle size of TiO2, it can effectively refine the microstructure of the solder joint and refine the IMC (interfacial compound), thereby achieving the purpose of improving the wettability of the solder and the mechanical properties of the solder joint. Similarly, when Nd, Ga or In is in phase formation, crystalline nano-TiO2 will also affect its phase formation, making it difficult to quickly form gallium-rich, neodymium-rich or indium-rich phases, thereby reducing the formation of gallium-rich, neodymium-rich or indium-rich phases, thereby reducing the negative impact caused by more Nd, Ga or In. In addition, the co-addition of wettability improver X and crystalline nano-TiO2 makes the gallium-rich, neodymium-rich or indium-rich phases relatively small, while Nd, Ga or In is relatively dispersed at the solder joint interface, which can significantly inhibit the growth rate of IMC at the solder joint during the aging process, thereby further improving the mechanical properties of the solder joint.
[0011] TiO2 crystals can be divided into rutile TiO2 crystals, anatase TiO2 crystals and brookite TiO2 crystals; among them, rutile TiO2 crystals and anatase TiO2 crystals belong to the tetragonal system, while brookite TiO2 crystals belong to the orthorhombic system. When nano-TiO2 is in a crystalline state and a mixed crystal, the direction of the nano-TiO2 crystal is more disordered, which will provide different directions for the phase growth at the solder joint interface, that is, the phase growth direction of Nd, Ga or In is disordered, making it more difficult to achieve a large number of continuous gallium-rich, neodymium-rich or indium-rich phases, and at the same time, it can further inhibit the growth rate of IMC, so that the mechanical properties of the solder joint are further improved.
[0012] Optionally, the mass percentage of the nano-TiO2 is 0.16-0.24%.
[0013] Optionally, the nano-TiO2 crystals are mixed crystals composed of at least one of rutile TiO2 crystals and anatase TiO2 crystals and brookite TiO2 crystals.
[0014] By adopting the above technical solution, the disorder of the nano-TiO2 crystal direction is further improved, thereby further suppressing the growth rate of IMC, so that the mechanical properties of the solder joint are further improved.
[0015] Optionally, the nano-TiO2 crystals are mixed crystals composed of rutile TiO2 crystals and brookite TiO2 crystals, and the mass ratio of the rutile TiO2 crystals to the brookite TiO2 crystals is 1:(0.2-0.4).
[0016] Anatase TiO2 crystals and brookite TiO2 crystals have poor thermal stability. Anatase TiO2 crystals begin to slowly transform into rutile TiO2 crystals at 610°C and completely transform into rutile TiO2 crystals at 915°C, while brookite TiO2 crystals completely transform into rutile TiO2 crystals at 650°C. By adopting the above technical solution, the thermal stability of nano-TiO2 crystals during welding and aging time is improved while ensuring crystal orientation disorder, thereby ensuring the reliability of solder joints.
[0017] Optionally, the particle size of the nano-TiO2 is 5-50nm.
[0018] Micro-nano-sized particles have extremely high surface activity, so they are more likely to adhere to the surroundings of other components of the solder and to the microscopic defects after the solder is atomized during welding, so as to better exert their effects. By adopting the above technical solution, nano-TiO2 in the above particle size range can be well dispersed in the solder and play a role.
[0019] Optionally, the wettability improving agent X is Ga.
[0020] Ga can simultaneously have the advantages of making the solder melting point appropriate, improving the solder's oxidation resistance, improving the solder's wettability, and improving the solder's mechanical properties.
[0021] Optionally, the mass percentage of Ga is 0.52-0.59%.
[0022] By adopting the above technical solution, the above amount of nano-TiO2 and Ga interact with each other, which can significantly improve the wettability of the solder and the mechanical properties of the solder joint.
[0023] In a second aspect, the present application provides a method for preparing the above-mentioned nano-titanium dioxide-doped Sn-Ag-Cu-X quaternary solder, using the following technical solution:
[0024] A method for preparing the above-mentioned nano-titanium dioxide doped Sn-Ag-Cu-X quaternary solder, the preparation method comprising the following steps: mixing nano-TiO2, Ag, Cu and wettability improver X according to the formula amount to obtain the solder.
[0025] By adopting the above technical solution, ball milling is performed to ensure that the above raw materials are fully mixed.
[0026] In summary, this application has the following beneficial effects:
[0027] 1. The present application adds any one of Nd, Ga and In to Sn-Ag-Cu solder, and adds it together with crystalline nano-TiO2 to significantly improve the solder wettability and the shear strength of the solder joint. The crystalline state of nano-TiO2 can form nucleation particles when the β-Sn phase solidifies to prevent the β-Sn phase from growing into large dendrites, and refine the microstructure of the solder joint based on the characteristics of the nano-scale particle size of TiO2, so that the IMC (interfacial compound) is refined, thereby achieving the purpose of improving the solder wettability and the shear strength of the solder joint. In addition, crystalline nano-TiO2 slows down the formation of gallium-rich, neodymium-rich or indium-rich phases, thereby reducing the negative effects caused by the addition of more Nd, Ga or In. The purpose of setting nano-TiO2 as a mixed crystal is to make the direction of nano-TiO2 crystal more disordered, which will provide different directions for the phase growth at the solder joint interface. That is to say, the phase growth direction of Nd, Ga or In is disordered, making it more difficult to achieve a large number of continuous gallium-rich, neodymium-rich or indium-rich phases. At the same time, it can also further inhibit the growth rate of IMC, so that the mechanical properties of the solder joint are further improved.
[0028] 2. In the present application, the particle size of nano-TiO2 is further selected to be 5-50 nm. Because its micro-nano-sized particles have extremely high surface activity, it is easier to adhere to the surroundings of other components of the solder and to the microscopic defects after the solder is atomized during welding, so that it can better interact with the wettability improver X and exert its effect. DETAILED DESCRIPTION
[0029] The present application is further described in detail below with reference to the embodiments.
[0030] Unless otherwise specified, the raw materials used in this application are all commercially available, including tin ingots with a purity of 99.99wt%, metallic silver with a purity of 99.95wt%, electrolytic copper (cathode copper) with a purity of 99.95wt%, metallic gallium with a purity of 99.95wt%, metallic neodymium with a purity of 99.5wt%, and metallic indium with a purity of 99.5wt%.
[0031] Example
[0032] Example 1
[0033] A nano-titanium dioxide doped Sn-Ag-Cu-Ga quaternary solder, the components and mass percentages of which are: 0.1% nano-TiO2, 0.3% Ag, 0.5% Cu, 0.4% Ga, and the balance is Sn. The nano-TiO2 is in a crystalline state, and is a mixed crystal obtained by mixing rutile TiO2 crystals and brookite TiO2 crystals in a mass ratio of 1:0.2, and the particle sizes of the rutile TiO2 crystals and the brookite TiO2 crystals are both 30-50nm.
[0034] Tin ingot, metallic silver, electrolytic copper (cathode copper), metallic gallium and nano-TiO2 are weighed in the above mass percentages and then ball-milled and mixed to obtain a nano-titanium dioxide-doped Sn-Ag-Cu-Ga quaternary solder.
[0035] Example 2
[0036] A nano-titanium dioxide doped Sn-Ag-Cu-Ga quaternary solder, the components and mass percentages of which are: 0.3% nano-TiO2, 0.7% Ag, 0.9% Cu, 0.6% Ga, and the balance is Sn. The nano-TiO2 is in a crystalline state, and is a mixed crystal obtained by mixing anatase TiO2 crystal and brookite TiO2 crystal in a mass ratio of 1:0.4, and the particle sizes of the anatase TiO2 crystal and the brookite TiO2 crystal are both 5-50nm.
[0037] The preparation method of the Sn-Ag-Cu-Ga quaternary solder doped with nano-titanium dioxide is the same as that in Example 1.
[0038] Example 3
[0039] A nano-titanium dioxide doped Sn-Ag-Cu-Ga quaternary solder, the components and mass percentages of which are: 0.18% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.54% Ga, and the balance is Sn. The nano-TiO2 is in a crystalline state, and is a mixed crystal obtained by mixing rutile TiO2 crystals and brookite TiO2 crystals in a mass ratio of 1:0.3, and the particle sizes of the rutile TiO2 crystals and the brookite TiO2 crystals are both 5-30nm.
[0040] The preparation method of the Sn-Ag-Cu-Ga quaternary solder doped with nano-titanium dioxide is the same as that in Example 1.
[0041] Example 4
[0042] The difference between this embodiment and embodiment 3 is that the amount of nano-TiO2 added is different, and the specific components and mass percentages are: 0.16% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.54% Ga, and the balance is Sn. The rest is the same as embodiment 3.
[0043] Example 5
[0044] The difference between this embodiment and embodiment 3 is that the amount of nano-TiO2 added is different, and the specific components and mass percentages are: 0.24% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.54% Ga, and the balance is Sn. The rest is the same as embodiment 3.
[0045] Example 6
[0046] The difference between this embodiment and embodiment 3 is that the addition ratio of rutile TiO2 crystals and brookite TiO2 crystals is different, specifically: rutile TiO2 crystals and brookite TiO2 crystals are mixed in a mass ratio of 1:0.1 to obtain a mixed crystal. The rest is the same as embodiment 3.
[0047] Example 7
[0048] The difference between this embodiment and embodiment 3 is that the addition ratio of rutile TiO2 crystals and brookite TiO2 crystals is different, specifically: rutile TiO2 crystals and brookite TiO2 crystals are mixed in a mass ratio of 1:0.5 to obtain a mixed crystal. The rest is the same as embodiment 3.
[0049] Example 8
[0050] The difference between this embodiment and embodiment 3 is that the particle size ranges of rutile TiO2 crystals and brookite TiO2 crystals are different, specifically: the particle sizes of rutile TiO2 crystals and brookite TiO2 crystals are both 60-100 nm. Others are the same as embodiment 3.
[0051] Example 9
[0052] The difference between this embodiment and embodiment 3 is that the specific selection of wettability improver X is different, and its composition and mass percentage are specifically: 0.18% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.54% In, and the balance is Sn. The rest is the same as embodiment 3.
[0053] Example 10
[0054] The difference between this embodiment and embodiment 3 is that the specific selection of wettability improver X is different, and its composition and mass percentage are specifically: 0.18% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.54% Nd, and the balance is Sn. The rest is the same as embodiment 3.
[0055] Embodiment 11
[0056] The difference between this embodiment and embodiment 3 is that the amount of Ga added is different, and the specific composition and mass percentage are: 0.18% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.52% Ga, and the balance is Sn. The rest is the same as embodiment 3.
[0057] Example 12
[0058] The difference between this embodiment and embodiment 3 is that the amount of Ga added is different, and the specific composition and mass percentage are: 0.18% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.59% Ga, and the balance is Sn. The rest is the same as embodiment 3.
[0059] Embodiment 13
[0060] The difference between this embodiment and embodiment 3 is that the amount of Ga added is different, and the specific composition and mass percentage are: 0.18% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.45% Ga, and the balance is Sn. The rest is the same as embodiment 3.
[0061] Comparative Example
[0062] Comparative Example 1
[0063] The difference between this comparative example and Example 3 is that the specific selection of wettability improver X is different, and its composition and mass percentage are specifically: 0.18% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.54% Ni, and the balance is Sn. The rest is the same as Example 3.
[0064] Comparative Example 2
[0065] The difference between this comparative example and Example 3 is that the amount of nano-TiO2 added is different, and its components and mass percentages are specifically: 0.05% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.54% Ga, and the balance is Sn. The rest is the same as Example 3.
[0066] Comparative Example 3
[0067] The difference between this comparative example and Example 3 is that the amount of nano-TiO2 added is different, and the specific components and mass percentages are: 0.35% nano-TiO2, 0.42% Ag, 0.64% Cu, 0.54% Ga, and the balance is Sn. The rest is the same as Example 3.
[0068] Comparative Example 4
[0069] The difference between this comparative example and Example 3 is that the raw material does not contain nano-TiO2 and the addition amount of other raw materials is different, and the composition and mass percentage are specifically: 0.50% Ag, 0.70% Cu and 0.49% Ga, and the balance is Sn. The rest is the same as Example 3.
[0070] Comparative Example 5
[0071] The difference between this comparative example and Example 3 is that the raw material does not contain Ga and the amount of nano-TiO2 added is different, and its components and mass percentages are specifically: 0.35% nano-TiO2, 0.42% Ag and 0.64% Cu, and the balance is Sn. The rest is the same as Example 3.
[0072] Performance testing
[0073] 1. Wettability determination
[0074] The wettability test was carried out in accordance with the relevant provisions of the standard JIS Z3198-4:2003 "Test Methods for Lead-free Solder - Part 4: Wettability Test Method Based on Wetting Balance and Contact Angle Method". Specifically, the solder sample to be tested was placed in a solder bath and heated to completely melt and then kept warm (the holding temperatures were 245°C and 265°C respectively); the oxygen-free copper sheet was immersed in the flux (water-soluble flux was selected) for 5 seconds and then taken out, and the oxide film on the surface was scraped off; the copper sheet was brought into contact with the melted and kept warm solder and the copper sheet was inserted into the solder at a speed of 4mm / s and a depth of 2mm. After reaching the target depth, it was kept for 10 seconds, and then the copper sheet and the solder were separated, and the wetting time and wetting force were calculated respectively. The results are shown in Table 1.
[0075] Table 1 Wetting force and wetting time of solder obtained by different implementation schemes
[0076]
[0077] It can be seen from the data results in Table 1 that when the holding temperatures are 245°C and 265°C respectively, compared with the implementation scheme of the comparative example, the solder in the implementation scheme of the present application has a shorter wetting time and a greater wetting force, which indicates that the solder wetting performance obtained in the present application is more excellent.
[0078] By comparing the data results of Examples 3-5 and Comparative Examples 2-3, it can be seen that the amount of nano-TiO2 added will affect the wettability of the solder. The amount of nano-TiO2 added is recommended to be in the range of 0.1-0.3wt%, and further in the range of 0.16-0.24wt% (Examples 3-5). At this addition ratio, a solder with relatively excellent wettability will be obtained; if the amount of nano-TiO2 added exceeds the basic requirement of 0.1-0.3wt%, the wettability of the solder will be significantly poor.
[0079] In addition, the data results of Examples 3, 6-8 show that the addition ratio and particle size range of rutile TiO2 crystals and brook TiO2 crystals will also affect the wettability of the solder. The different addition ratios of rutile TiO2 crystals and brook TiO2 crystals will affect the distribution and distribution of different crystal forms of TiO2 crystals, that is, the crystal orientation distribution is different, which will affect the growth distribution of the Ga-rich phase, thereby affecting the wettability. The surface performance of larger particles of nano-TiO2 (Example 8) is poor, which makes the distribution uniformity of the raw materials in the solder poor, and then leads to poor wettability of the solder.
[0080] By comparing Examples 3, 9-10 and Comparative Example 1, it can be seen that the selection of wettability improver X is also very important. Different wettability improvers X have great differences in the compatibility of the solder system. Among the raw materials Ga, In, Nd and Ni, Ga has a higher compatibility with the solder system and can significantly improve the solder wettability, while Ni has the worst performance in improving the solder wettability.
[0081] By comparing the data results of Example 3 and Examples 11-13, it can be seen that even if Ga is selected as the wettability improver X, there are certain requirements for its addition amount. The addition amount of Ga is higher than the conventional maximum addition amount of 0.5wt% (Comparative Example 4), but the addition amount of Ga is still recommended to be in the range of 0.4-0.6wt%, and further in the range of 0.52-0.59wt% (Examples 11-12). With this addition ratio, a solder with excellent wettability will be obtained; exceeding this range will still have a negative impact on the wettability of the solder.
[0082] Comparing the data results of Example 3 and Comparative Example 5, it can be seen that when only nano-TiO2 is added to the solder without Ga, it is difficult to achieve the purpose of significantly improving the wettability of the solder.
[0083] 2. Determination of mechanical properties of micro solder joints
[0084] The mechanical properties of micro solder joints were tested with reference to the relevant provisions of the standard JIS Z3198-4:2003 "Test Methods for Lead-free Solder - Part 7: Shear Test Methods for Chip Component Solder Joints". Specifically, the solders with different components and proportions were pressed into thin sheets of about 2 mm, the surface oxides were scraped off and the solders were cut into granular solders of the same size for standby use; the chip resistors were soldered to the PCB board using an electric soldering iron, and the solder used was the prepared standby solder mentioned above, the soldering temperature was 370°C, the circuit board was wiped and dried after soldering, and then the shear strength test was performed. The solders obtained with different implementation plans were tested, and the specific results are shown in Table 2.
[0085] Table 2 Shear strength of solder joints obtained by different implementation schemes
[0086]
[0087]
[0088] From the data results of Table 2, it can be seen that the shear strength of the solder joint of the present application is significantly higher than the solder joint strength of the solder obtained by the comparative example. The data results of Examples 3 and 8 show that the particle size of nano-TiO2 has a certain influence on the shear strength of the solder joint, and the selection of nano-TiO2 with a smaller particle size can improve the shear strength of the solder joint. The data results of Example 3, Examples 9-10 and Comparative Example 1 show that the selection of different wetting improvers X has a greater influence on the shear strength of the solder joint: different wetting improvers X have different compatibility with other components in the system, and among the raw materials Ga, In, Nd and Ni, Ga has a higher compatibility with the solder system and can significantly improve the shear strength of the solder joint.
[0089] Example 3 and Examples 11-13 show that, although more Ga can be added in the present application, the amount of Ga added is also recommended to be within the range of 0.4-0.6wt%, otherwise it will still have a negative impact on the shear strength of the solder joint. In addition, compared with Example 2-3, Example 3 shows that in this solution, the amount of nano-TiO2 added also has an impact on the shear strength of the solder joint, wherein the amount of 0.1-0.3wt% added can ensure the shear strength of the solder joint. The implementation schemes of Example 3 and Comparative Examples 4-5 verify the contribution of nano-TiO2 and Ga added together to the shear strength of the solder joint in this solution. These two raw materials can interact and jointly affect the interaction of each element of the solder and the PBC board during welding, ensuring the shear strength of the solder joint and making it difficult to fall off.
[0090] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A nano-titanium dioxide doped Sn-Ag-Cu-X quaternary solder, It is characterized in that Its components and mass percentage are: 0.1-0.3% nano-TiO 2 , 0.3-0.7% Ag, 0.5-0.9% Cu, 0.4-0.6% wettability improver X, and the balance is Sn; the nano-TiO 2 It is in a crystalline state and a mixed crystal; the wettability improver X is selected from any one of Nd, Ga and In; The nano-TiO 2 The crystal is rutile TiO 2 Crystalline and brookite TiO 2 The mixed crystal composed of crystalline form, the rutile TiO 2 Crystalline and brookite TiO 2 The mass ratio of crystalline form crystals is 1:(0.2-0.4).
2. The Sn-Ag-Cu-X quaternary solder doped with nano-titanium dioxide according to claim 1, It is characterized in that The mass percentage of the nano-TiO2 is 0.16-0.24%.
3. The Sn-Ag-Cu-X quaternary solder doped with nano-titanium dioxide according to claim 1, It is characterized in that The nano-TiO 2 The particle size is 5-50nm.
4. The Sn-Ag-Cu-X quaternary solder doped with nano-titanium dioxide according to claim 1, It is characterized in that The wettability improving agent X is Ga.
5. The Sn-Ag-Cu-X quaternary solder doped with nano-titanium dioxide according to claim 3, It is characterized in that The mass percentage of Ga is 0.52-0.59%.
6. A method for preparing the Sn-Ag-Cu-X quaternary solder doped with nano-titanium dioxide according to any one of claims 1 to 5, It is characterized in that The preparation method comprises the following steps: 2 , Ag, Cu and wettability improver X are mixed according to the formula amount.
Citation Information
Patent Citations
Low-silver lead-free solder alloy and preparation method and device thereof
CN102029479A