A method for preparing feed additive sodium chloride from sodium sulfate type brine

By using lime flue gas purification and nanofiltration membrane separation technology, the problems of impurity removal and particle size in sodium chloride feed additives have been solved, enabling the preparation of high-purity and highly uniform sodium chloride products, thereby improving product quality and corporate efficiency.

CN116177777BActive Publication Date: 2024-11-15CHINASALT JINTAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211562208.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-07
Publication Date
2024-11-15
Estimated Expiration
2042-12-07

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively remove impurities from sodium chloride feed additives, resulting in low product purity, uneven particle size, and a tendency to clump, which negatively impacts animal health and production performance.

Method used

By combining membrane technology with crystal growth, Ca2+, Mg2+, and trace amounts of Pb and Cd in well brine are removed through lime flue gas purification and nanofiltration membrane separation. This increases the particle size, reduces dust pollution, and produces a product that meets the standards for "Sodium Chloride Feed Additives".

Benefits of technology

It improves product purity and particle size uniformity, reduces dust pollution, meets the requirements for feed formulation uniformity, reduces the generation of lumpy salt, and enhances product quality and enterprise competitiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116177777B_ABST
    Figure CN116177777B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of brine purification, and in particular to a method for preparing sodium chloride, a feed additive, from sodium sulfate brine. In the present invention, the brine extracted from the mine is purified to remove impurities such as calcium and magnesium ions, and the refined brine after impurities removal is filtered through a nanofiltration membrane, and the nanofiltration permeate is evaporated, thickened, centrifuged, and dried to obtain feed salt. The average particle size of the salt is increased from 330 to 360 μm to 545 to 555 μm, which effectively reduces the powder particles and the probability of agglomeration; at the same time, the feed additive sodium chloride under this particle size is refined salt as a product, which can be divided into wet salt and dry salt. The wet salt or dry salt under the particle size of the present invention can effectively ensure that the phenomenon of floating or sinking due to different densities between the two can be reduced during feed preparation, and the uniform distribution of salt can be ensured, and the anti-caking property is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of brine purification, and in particular to a method for preparing sodium chloride, a feed additive, from sodium sulfate brine. Background Art

[0002] In animal nutrition, sodium and chlorine are two elements necessary to maintain healthy growth and normal production performance of animals. However, the content of sodium and chlorine in most feed raw materials (especially plant feed raw materials) is low, so they need to be supplemented. Adding sodium chloride to the feed product formula is the main way to meet the needs of animals for sodium and chlorine. The main component of table salt is sodium chloride (NaCl), so table salt becomes the simplest, cheapest and most effective substance to supplement sodium chloride.

[0003] Sodium chloride is the main chemical component of table salt and an important chemical raw material. In animals, chloride ions and sodium ions are mainly present in body fluids and soft tissues, maintaining osmotic pressure, regulating acid-base balance, and controlling water metabolism. They are mineral elements necessary for the normal growth and development of animals. They can promote the synthesis of organic matter such as fat and protein in the metabolic process, keep digestive juice alkaline in the intestines, activate amylase, and keep gastric juice acidic, which has a bactericidal effect.

[0004] Feed additive sodium chloride products are single ingredients. Except for a certain amount of anti-caking agent (potassium ferrocyanide), they do not contain trace element additives such as iodine, and should not have other artificial additives. At the same time, in order to ensure uniform feed mixing and prevent animals from sodium chloride poisoning or insufficient intake, there are certain requirements for the particle size of feed additive sodium chloride: uniform particles, normal edible salt particle size small particles require 0.15-0.85mm ≥ 75% (edible salt GB / T5461-2016), and the particle size of feed salt (passing 0.71mm test sieve) requires ≥ 85% (feed additive sodium chloride GB / T23880-2009). Uneven particles are easy to cause uneven mixing of powder particles and feeds of other particle sizes when mixing feed salt.

[0005] Due to the special requirements of sodium chloride, a feed additive, in terms of sodium nitrite, particle size, anti-caking agent, and trace element additives such as iodine, it is unreasonable to directly replace its preparation technology with the standards of edible salt, livestock salt, pickling salt or industrial salt. The sales channels of existing products are relatively chaotic and the quality is very unstable. In order to improve its quality and ensure its functionality, it is very necessary to research and develop products that meet the standards of "Sodium Chloride, a Feed Additive" (GB / T 23880-2009). Summary of the invention

[0006] In order to solve the problems in the background technology, the present invention provides a method for preparing sodium chloride, a feed additive, from sodium sulfate brine.

[0007] The present invention adopts a method of coupling membrane technology with crystal cultivation to solve the effect of sodium sulfate or calcium sulfate brine associated with the raw material brine of sodium chloride, a feed additive, on the purity of the product. The high nitrate water produced by nanofiltration is made into gypsum calcium sulfate; at the same time, the particle size is increased, the pollution of small salt crystal dust to the environment is reduced, the product utilization rate is improved, the generation of lump salt is reduced, and the uniformity requirement of feed configuration is met; various indicators of the product meet and are better than the national standard "Sodium Chloride, a Feed Additive".

[0008] The implementation and promotion of this project will standardize the production of sodium chloride, a feed additive, improve product quality, prevent animal sodium chloride poisoning or insufficient intake, and solve the problem of animal health and production performance affected by sodium chloride quality problems. Through technological innovation and structural optimization, with sodium chloride as the feed additive as the target, improving product quality and adjusting product structure will help enhance corporate competitiveness and improve the overall benefits of the salt industry.

[0009] The technical solution adopted by the present invention is:

[0010] A method for preparing sodium chloride, a feed additive, from sodium sulfate brine, comprising the following steps:

[0011] Well brine (raw brine) is purified by lime flue gas to remove Ca in the raw brine 2+ Mg 2+ , and trace amounts of Pb and Cd; then separated by nanofiltration membrane, the low nitrate water after the membrane is divided into two streams, one of which is used to adjust the humidity of wet salt, and the other is sent to the evaporation tank for evaporation and crystallization, the crystallized salt slurry enters the thickening and crystal-growing unit to make the grains grow and uniform in size, and then centrifuged and dehydrated, and then the humidity is adjusted by another stream of low nitrate water to obtain the feed additive sodium chloride wet salt, the moisture content of the wet salt is 2.6-3.2%; or directly dried after centrifugal dehydration, and mixed with anti-caking agent potassium ferrocyanide to obtain the feed additive sodium chloride dry salt;

[0012] The main components of well brine are: sodium chloride: 290-300g / L, sodium sulfate: 10-25g / L, calcium ion: 0.5-1.0g / L, magnesium ion ≤0.05g / L;

[0013] The thickening and crystal growth unit includes:

[0014] A thickener, wherein a material inlet and a first salt slurry inlet are respectively provided at the top of the thickener, the first salt slurry inlet is connected to a spray device, a first salt slurry outlet is provided in the middle of the thickener, and a material outlet is provided at the bottom of the thickener;

[0015] The crystal growing pool is provided with a second salt slurry inlet, a clear liquid outlet is provided at the top of the crystal growing pool, a clear liquid inlet is provided at the bottom, and a second salt slurry outlet is provided in the middle; the first salt slurry outlet is connected to the second salt slurry inlet through a pipeline, and a cooler is provided on the pipeline to cool the salt slurry output by the thickener, and the cooled salt slurry is sent to the crystal growing pool for crystallization; the clear liquid outlet is connected to the clear liquid inlet, and the second salt slurry outlet is connected to the spraying device;

[0016] Utilizing the principle of low-temperature salt precipitation, the salt slurry after evaporation and crystallization enters the thickener through the first salt slurry inlet. The salt slurry in the thickener is cooled by the cooler and then transported to the crystal growing pool for crystal cultivation at 5-15°C for 2-3 hours to allow the salt particle size to grow. During the process, the supernatant in the crystal growing pool is pumped to the bottom of the crystal growing pool to slowly disturb the salt slurry at the bottom of the crystal growing pool to avoid agglomeration. After the crystal cultivation is completed, the salt slurry is pumped from the second salt slurry outlet and sprayed onto the thickener. The temperature of the thickener is controlled at 38-43°C to further regulate the salt particle size.

[0017] Furthermore, a well-shaped distributor connected to the clear liquid inlet is provided at the bottom of the crystal growing pool, and the clear liquid is distributed in the salt slurry through the well-shaped distributor, and the clear liquid flow rate is 0.2-0.5m / s.

[0018] Furthermore, the nanofiltration concentrate (high nitrate water) is transferred to brine purification to obtain calcium sulfate dihydrate, which is washed, filtered, dehydrated and dried to obtain a gypsum product with the required crystal form. The mother liquor (or filtrate) produced by the preparation of gypsum is returned to the brine purification system and recycled after decalcification.

[0019] Furthermore, the sulfate in the nanofiltration concentrate is prepared into dihydrate gypsum by adding calcium chloride solution, and the dihydrate gypsum is dehydrated and dried to prepare α powder and β powder of hemihydrate gypsum, wherein the ratio of α powder to β powder is 1:2, see reaction equations (1) and (2).

[0020] Na2SO4+CaCl2+2H2O→CaSO4·2H2O↓+2NaCl (1)

[0021] CaSO4·2H2O (heating) → CaSO4·1 / 2H2O+3 / 2 H2O↑ (2)

[0022] Normal sodium sulfate brine produces a lot of salt and nitrate co-production, and is rarely made into gypsum because the salt content in gypsum affects the quality. Salt and nitrate separation is made by direct evaporation of the sodium sulfate product, and the process is simpler.

[0023] The dry basis purity of the gypsum prepared by the invention is ≥98kg / 100kg, and the sodium chloride content is ≤50mg / kg.

[0024] Furthermore, the method for controlling the moisture content of wet salt includes: the moisture content of wet salt after centrifugal dehydration is 2.4-2.6% (mass), and the moisture content of wet salt is reduced by adjusting the pulley speed and pushing frequency of the centrifuge. The speed of the centrifuge pulley is increased by 10-15%, and the pushing frequency is reduced by 15-20%, and the moisture content can be reduced to 2.0%. In order to increase the moisture content of wet salt from 2.5% to 2.6-3.2%, solid clean spraying can be performed. Specifically, the centrifuge is equipped with a spraying device, and nanofiltration low nitrate water is continuously sprayed onto the solid cake, and the addition amount is 0.13-0.95% of the total solid mass of the centrifuge.

[0025] Furthermore, nanofiltration belongs to saturated salt water nanofiltration. The sodium sulfate content of high nitrate water produced by nanofiltration is 60-65g / L, the sodium hydroxide is 0.15-0.35g / L, and the sodium sulfate content of low nitrate water is ≤1.0g / L. Nanofiltration can separate divalent or high-valent ions, and intercept lead, cadmium, magnesium, calcium and other ions into high nitrate water, making the purity of low nitrate water higher, playing a role of secondary interception.

[0026] In the further lime flue gas brine purification process, calcium, magnesium and trace amounts of lead and cadmium are removed in the form of salt mud. The main contents of the salt mud are: calcium carbonate 60.2-70.2%, water 20.5-22.4%, calcium sulfate 10.1-11.3%, sodium chloride 2.5-3.6%, magnesium hydroxide 1.0-1.5%, lead salt (lead carbonate, lead hydroxide) 0.005-0.015%, chromium carbonate 0.004-0.011%, and the rest are inevitable impurities; pH is 10-12. The refined brine sent to the nanofiltration requires water insoluble matter ≤2mg / L, calcium and magnesium ions ≤5mg / L, temperature ≤45℃, pH: 9.0-11.0, mainly to prevent scaling and high-temperature membrane material decomposition. Because the pH value of the refined brine obtained by the lime flue gas process is not too high, 9.0-10.0, it can be directly fed into the nanofiltration membrane without acid adjustment.

[0027] Furthermore, in the process of adding calcium chloride to make gypsum, the concentration of calcium chloride is 300-350 g / L, calcium chloride: high nitrate water = 1:5-1:7 (volume ratio), and the sodium sulfate content in the solution after the reaction is reduced from 60-65 g / L to 6-7 g / L.

[0028] Compared with the prior art, the average particle size of the feed additive sodium chloride prepared by the present invention increases from 330-360 μm to 545-555 μm, effectively reducing powder particles and reducing the chance of caking; at the same time, the feed additive sodium chloride with this particle size is refined salt as a product, which can be divided into wet salt and dry salt. The wet salt or dry salt with the particle size of the present invention can effectively ensure that the phenomenon of floating or sinking when mixing due to different densities of the two can be reduced during feed preparation, ensure the uniform distribution of salt, and have good anti-caking properties. Among them, the wet salt, without adding the anti-caking agent potassium ferrocyanide, has a storage time of more than 20 days; if the moisture content of the wet salt is 2.0-2.5%, the storage time exceeds 7 days. The dry salt with the particle size of the present invention has a strong anti-caking ability and can effectively reduce the use of anti-caking agents.

[0029] Compared with the prior art, the present invention has the following excellent effects:

[0030] (1) The present invention utilizes lime flue gas brine purification combined with nanofiltration membrane to effectively remove impurities such as calcium, magnesium, lead, and cadmium in well brine, thereby increasing the purity of the product from 95.50% to 99.80%.

[0031] (2) Recover the nanofiltration high-nitrate water and prepare gypsum α powder or β powder by adding calcium chloride solution, so as to effectively recover the sulfate resources in the sodium sulfate brine.

[0032] (3) The salt particle size is effectively increased by thickening and crystal-forming units, and the average salt particle size increases from 330-360 μm to 545-555 μm, effectively reducing powder particles, reducing the chance of agglomeration, and ensuring uniform distribution in the feed.

[0033] (4) Feed additive sodium chloride products are classified into dry and wet types according to standard moisture requirements, which can effectively meet the needs of different customers. For short-distance users, the need for anti-caking agent potassium ferrocyanide to prevent caking can be achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is a process flow chart of an embodiment.

[0035] The reference numerals in the figure are: 1. thickener, 2. cooler, 3. crystal growing pool, 4. well-shaped distributor, 5. spraying device. DETAILED DESCRIPTION

[0036] The present invention will be further described below in conjunction with embodiments, but is not limited thereto.

[0037] Example

[0038] A method for preparing sodium chloride, a feed additive, from sodium sulfate brine, comprising the following steps:

[0039] (1) Well brine (raw brine) is transported from the mine to the brine purification process in the factory through the brine pipeline. The lime flue gas brine purification reaction is used to remove Ca in the raw brine. 2+ Mg 2+ , and trace amounts of Pb and Cd; the refined brine after the reaction is pumped into the nanofiltration membrane for separation, and the low nitrate water after the membrane is divided into two streams, one of which enters the centrifuge for wet salt humidity adjustment, and the other is pumped into the evaporation section for evaporation and crystallization. The crystallized salt slurry enters the thickening and crystal growth unit for thickening (to make the grains grow and have a uniform particle size), and then centrifuges for dehydration, and then adjusts the humidity with another stream of low nitrate water to obtain the feed additive sodium chloride wet salt, with a moisture content of 2.6-3.2%; or it is directly dried after centrifugal dehydration, and after adding the anti-caking agent potassium ferrocyanide and mixing, it enters the packaging section to obtain the feed additive sodium chloride dry salt.

[0040] The thickening and crystal growth unit includes:

[0041] A thickener 1, wherein a material inlet and a first salt slurry inlet are respectively provided at the top of the thickener 1, the first salt slurry inlet is connected to a spray device 5, a first salt slurry outlet is provided in the middle of the thickener 1, and a material outlet is provided at the bottom of the thickener 1;

[0042] A crystal growing pool 3 is provided with a second salt slurry inlet, a clear liquid outlet is provided at the top of the crystal growing pool 3, a clear liquid inlet is provided at the bottom, and a second salt slurry outlet is provided in the middle; the first salt slurry outlet is connected with the second salt slurry inlet through a pipeline, and a cooler 2 is provided on the pipeline for cooling the salt slurry output by the thickener 1, and the cooled salt slurry is sent to the crystal growing pool 3 for crystallization; the clear liquid outlet is connected with the clear liquid inlet, and the second salt slurry outlet is connected with the spraying device 5; a tic-tac-toe distributor 4 connected with the clear liquid inlet is also provided at the bottom of the crystal growing pool 3.

[0043] Using the principle of low-temperature salt precipitation, the salt slurry after evaporation and crystallization enters the thickener 1 through the first salt slurry inlet. The salt slurry of the thickener 1 is cooled by the cooler 2 and then transferred to the crystal cultivation pool 3. After cooling and reducing the temperature in the crystal cultivation pool 3, the salt particle size grows instantly and stays in the crystal cultivation pool 3 for 2 to 3 hours. During the process, the supernatant in the crystal cultivation pool 3 is pumped to the bottom of the crystal cultivation pool 3 and distributed in the salt slurry through the well-shaped distributor 4. The clear liquid flow rate is 0.2-0.5m / s, which slowly disturbs the salt slurry at the bottom of the crystal cultivation pool so that the bottom does not agglomerate due to long-term standing and controls the growth of grains. After the crystal cultivation is completed, the salt slurry is drawn from the second salt slurry outlet and sprayed to the thickener 1. When entering the thickener 1, a circular spray system is used. The salt slurry is sprayed evenly in the space above the liquid level of the thickener 1 after spray cooling, so that the salt slurry continues to cool and crystallize at this stage, and the salt particle size is further adjusted. Finally, the sodium chloride with uniform particles that meet the particle size requirements is discharged from the material outlet. The specific temperature and grain size distribution are shown in Table 1.

[0044] Table 1

[0045]

[0046] (2) The high-nitrate water produced by nanofiltration is transferred to brine purification to obtain calcium sulfate dihydrate, which is then washed, filtered, dehydrated, and dried to obtain gypsum products (α powder or β powder) of different crystal forms. The mother liquor (or filtrate) produced by the preparation of gypsum is returned to the brine purification system and recycled after decalcification.

[0047] (3) The sulfate in the nanofiltration concentrate is added with calcium chloride solution to produce dihydrate gypsum, which is then dehydrated and dried to produce α powder and β powder of hemihydrate gypsum, which are used as building materials. The ratio of α powder to β powder is 1:2, as shown in reaction equations (1) and (2).

[0048] Na2SO4+CaCl2+2H2O→CaSO4·2H2O↓+2NaCl (1)

[0049] CaSO4·2H2O (heating) → CaSO4·1 / 2H2O+3 / 2 H2O↑ (2)

[0050] Normal sodium sulfate brine produces more salt and nitrate, and rarely makes gypsum, because the salt content in gypsum affects the quality, and the process of separating sodium sulfate products with salt and nitrate and directly evaporating is simpler. The by-product sulfate in the brine can be used to make gypsum in the purification section or to directly produce sodium sulfate in the evaporation process. Most of them use the latter, sodium sulfate products.

[0051] Feed additive sodium chloride is produced in the form of refined salt, which can be divided into wet salt and dry salt. The wet salt with a moisture content of 2.6-3.2% under the particle size of the present invention can effectively reduce the degree of wet salt anti-caking. Without adding anti-caking agent potassium ferrocyanide, the storage time exceeds 20 days; if the wet salt moisture content is 2.0-2.5%, the storage time is more than 7 days. It is recommended that the moisture content of wet salt be controlled at 2.6-3.2%. When the humidity is required to be less than 2.0%, it cannot be directly centrifuged and dehydrated due to the limitation of the centrifuge dehydration equipment itself; it is recommended to obtain dry salt for sale after drying.

[0052] Whether the feed additive sodium chloride is lumpy, the average value of solidification degree (Kgf / cm 2 ), the degree of consolidation = the force when the salt is broken / the bottom area of ​​the salt block cylinder. The degree of agglomeration of wet salt at various moisture contents can be determined based on the degree of consolidation. The heat-sealed salt bags were placed upright, and the salt bags were opened 15 days, 30 days, 45 days, and 60 days after the sampling date to conduct experiments. The harder agglomerated salt blocks were made into cylindrical salt blocks with a bottom diameter of 5 to 8.5 cm and a height of 5 cm. Then, the salt blocks were pressed with the palm of the hand on the electronic scale. The reading displayed on the electronic scale when the salt blocks were broken was recorded, and then the degree of consolidation of the salt blocks was calculated. When the degree of consolidation is ≤0.050Kgf / cm 2The salt agglomeration is not obvious, and there is no large agglomeration, which is the storage standard. The experiment shows that the moisture content of the sodium chloride wet salt prepared in this embodiment is controlled at 2.6-3.2%, and the degree of consolidation is 0.054Kgf / cm after storage for 30 days. 2 ; The degree of consolidation of dry salt after 100 days of storage is 0.062Kgf / cm 2 .

[0053] The method for controlling the moisture content of wet salt in this embodiment is as follows: the moisture content of wet salt is reduced by adjusting the pulley speed and pushing frequency of the centrifuge. The pulley speed of the centrifuge is increased by 10-15%, and the pushing frequency is reduced by 15-20%. The moisture content can be reduced from 2.5% to 2.0%. In order to increase the moisture content of wet salt from 2.5% to 2.6-3.2%, solid clean spraying can be performed. When spraying is required, the centrifuge is equipped with a spraying device 5, and the liquid (nanofiltration low nitrate water) is continuously sprayed onto the solid cake. The addition amount is 0.13-0.95% of the total solid mass of the centrifuge.

[0054] Step (2) nanofiltration belongs to saturated brine nanofiltration. The sodium sulfate content of high nitrate water produced by nanofiltration is 60-65g / L, the sodium hydroxide is 0.15-0.35g / L, and the sodium sulfate content of low nitrate water is ≤1.0g / L. Normal nanofiltration membranes require nanofiltration of unsaturated brine (sodium chloride ≤250g / L). In order to meet the direct nanofiltration of raw brine, this project adopts saturated brine nanofiltration without adding pure water for dilution; at the same time, nanofiltration can separate divalent or high-valent ions. Here, lead, cadmium, magnesium, calcium and other ions can be intercepted in high nitrate water, making the purity of low nitrate water higher, playing a role of secondary interception.

[0055] In the lime flue gas brine purification process in step (1), calcium, magnesium and trace amounts of lead and cadmium are removed in the form of salt mud. The main contents of the salt mud are: calcium carbonate 60.2-70.2%, water 20.5-22.4%, calcium sulfate 10.1-11.3%, sodium chloride 2.5-3.6%, magnesium hydroxide 1.0-1.5%, lead salt (lead carbonate, lead hydroxide) 0.005-0.015%, chromium carbonate 0.004-0.011%, and the rest are inevitable impurities; pH is 10-12. The requirements for the refined brine sent to the nanofiltration are: water insoluble matter ≤2mg / L, calcium and magnesium ions ≤5mg / L, temperature ≤45°C, pH: 9.0-11.0, mainly to prevent membrane scaling and high-temperature membrane material decomposition. Because the pH value of the refined brine obtained by the lime flue gas process is not too high, 9.0-10.0, it can be directly fed into the nanofiltration membrane without acid adjustment.

[0056] In the process of adding calcium chloride to prepare gypsum in step (1), the concentration of calcium chloride is 300-350 g / L, and the ratio of calcium chloride to high nitrate water is 1:5-1:7 (volume ratio). After the reaction, the sodium sulfate content in the solution decreases from 60-65 g / L to 6-7 g / L.

[0057] The components of the prepared feed additive sodium chloride dry salt and wet salt are shown in Table 2. The average particle size of the salt increases from 330-360 μm to 545-555 μm, which effectively reduces the powder particles and reduces the chance of agglomeration.

[0058] Table 2

[0059]

[0060]

[0061] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing sodium chloride, a feed additive, from sodium sulfate brine, characterized in that: The process includes the following steps: the well brine is purified by lime flue gas to remove Ca in the original brine. 2+ Mg 2+ , and trace amounts of Pb and Cd; then the nanofiltration membrane is used for separation, and the low nitrate water after the membrane is divided into two streams, one of which is used to adjust the humidity of the wet salt, and the other is sent to the evaporation tank for evaporation and crystallization. The crystallized salt slurry enters the thickening and crystal-growing unit to make the grains grow and have a uniform particle size, and then centrifugal dehydration, and then the humidity is adjusted with another stream of low nitrate water to obtain the feed additive sodium chloride wet salt, the moisture content of the wet salt is 2.6~3.2%; or it can be directly dried after centrifugal dehydration, and after adding the anti-caking agent potassium ferrocyanide and mixing, the feed additive sodium chloride dry salt is obtained; Well brine contains sodium chloride: 290~300g / L, sodium sulfate: 10-25g / L, calcium ion: 0.5~1.0g / L, magnesium ion ≤0.05g / L; The thickening and crystal growth unit includes: A thickener (1), wherein a material inlet and a first salt slurry inlet are respectively provided at the top of the thickener (1), the first salt slurry inlet is connected to the spray device (5), a first salt slurry outlet is provided at the middle of the thickener (1), and a material outlet is provided at the bottom of the thickener (1); A crystal growing pool (3), the crystal growing pool (3) is provided with a second salt slurry inlet, a clear liquid outlet is provided at the top of the crystal growing pool (3), a clear liquid inlet is provided at the bottom, and a second salt slurry outlet is provided in the middle; the first salt slurry outlet is connected to the second salt slurry inlet via a pipeline, the pipeline is provided with a cooler (2) for cooling the salt slurry output from the thickener (1), and the cooled salt slurry is sent to the crystal growing pool (3) for crystallization; the clear liquid outlet is connected to the clear liquid inlet, and the second salt slurry outlet is connected to the spray device (5); By utilizing the principle of low-temperature salt precipitation, the salt slurry after evaporation and crystallization enters the thickener (1) through the first salt slurry inlet, and the salt slurry in the thickener (1) is cooled by the cooler (2) and then transferred to the crystal growing pool (3), where the crystals are grown at 5-15°C for 2-3 hours, and the salt particle size is grown. During the process, the supernatant in the crystal growing pool (3) is pumped to the bottom of the crystal growing pool (3), and the salt slurry at the bottom of the crystal growing pool (3) is slowly disturbed. After the crystal growing is completed, the salt slurry is pumped from the second salt slurry outlet and sprayed to the thickener (1), and the temperature of the thickener (1) is controlled at 38-43°C. After the crystals grow and have a uniform particle size, the crystals are discharged from the material outlet, and the average particle size of the discharged crystals is 545-555μm.

2. The method for preparing feed additive sodium chloride from sodium sulfate type brine according to claim 1, characterized in that: A well-shaped distributor (4) connected to the clear liquid inlet is provided at the bottom of the crystal cultivation pool (3). The clear liquid is distributed in the salt slurry through the well-shaped distributor (4). The clear liquid flow rate is 0.2-0.5 m / s.

3. The method for preparing feed additive sodium chloride from sodium sulfate type brine according to claim 1, characterized in that: The nanofiltration concentrate is transferred to brine purification to obtain calcium sulfate dihydrate, which is then washed, filtered, dehydrated and dried to obtain a gypsum product of the desired crystal form. The filtrate produced by preparing the gypsum is returned to the brine purification system and recycled after decalcification.

4. The method for preparing feed additive sodium chloride from sodium sulfate type brine according to claim 3, characterized in that: The sulfate in the nanofiltration concentrate is made into dihydrate gypsum by adding calcium chloride solution, and the dihydrate gypsum is dehydrated and dried to make α powder and β powder of hemihydrate gypsum, wherein the ratio of α powder to β powder is 1:2; In the process of adding calcium chloride solution to make gypsum, the concentration of calcium chloride solution is 300-350g / L, the volume ratio of calcium chloride solution to nanofiltration concentrate is 1:5~1:7, and the sodium sulfate content in the solution drops from 60~65g / L to 6~7g / L after the reaction.