A continuous preparation process for water-based acrylic emulsion
Through dual kettle prepolymerization process and continuous dropping technology, the particle size distribution problem in the production of aqueous acrylic emulsions is solved, and the preparation of small-particle size products and the improvement of scrubbing resistance are achieved, which meets the needs of building coatings and has significant industrial applications. value.
Patent Information
- Application Number
- CN202310001901.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-03
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-01-03
AI Technical Summary
The continuous process of existing aqueous acrylic emulsions has a long residence time, resulting in a wider molecular weight distribution and larger particle size distribution, making it difficult to produce small-particle products, and cannot meet the requirements of building coatings, especially high scrubbing resistance. Wall lotion demand.
Using the dual-kettle prepolymerization process, the emulsifier is added continuously as the core, and the nucleation effect of the stabilized emulsifier is used to prepare a small-particle aqueous acrylic emulsion, and the steady state and equilibrium are quickly established through the dual-kettle process to achieve continuous production. .
It realizes the preparation of small-particle water-based acrylic emulsion, has excellent scrubbing resistance, has significant industrial application significance, reduces device costs, and meets application needs in the field of building coatings.
Smart Images

Figure BDA0004034260340000191 
Figure BDA0004034260340000201
Abstract
Description
Technical Field
[0001] The invention relates to a continuous process, in particular to a continuous preparation process of an aqueous acrylic emulsion. Background Art
[0002] Water-based acrylic emulsion uses water as a solvent to replace organic solvents, thereby achieving environmental protection and low VOC effects, reducing the possibility of causing fire and environmental pollution. At present, the industrial production process for preparing acrylic emulsion is mainly based on intermittent and semi-batch production processes. The intermittent process is to first add water, emulsifier, monomer, and initiator to the reactor, heat it to the required temperature to start the polymerization reaction, and finally reach the required reaction conversion rate to cool down and filter to obtain the final emulsion. The semi-batch production process refers to first putting the dispersion medium water and emulsifier, part of the monomer initiator and other components into the reactor, and after polymerization to a certain extent, the remaining monomers, initiators, etc. are continuously added to the polymerization kettle at a certain time interval for polymerization until the target conversion rate is reached.
[0003] Considering the large demand for architectural coating emulsions, which accounts for more than 50% of the total market of water-based acrylic emulsions, continuous process production is most suitable from the perspective of production efficiency. However, it is well known to those skilled in the art that the continuous production process has a long material residence time, which leads to a wide distribution of molecular weight and a large distribution of particle size of latex particles. Therefore, it is difficult to produce small particle size products using a continuous process, and it cannot meet the use demand of architectural coating emulsions, especially architectural interior wall emulsions with strict requirements on scrub resistance.
[0004] Patent CN114163563A realizes the full-process continuous production of water-based acrylic emulsion through continuous pre-emulsification, continuous kettle polymerization and continuous tubular post-treatment. However, it uses at least three reactors to establish the balance of input and output, and the production line is long, which is not conducive to saving equipment costs and production processes. In addition, this solution uses finished seed emulsion with a particle size of 60-120nm as a seed, and it can be expected that a large particle size product of 200-300nm will be prepared. When used in architectural coatings, it cannot meet the high requirements for the scrub resistance of the emulsion. Summary of the invention
[0005] In order to solve the above technical problems, the present invention proposes a continuous preparation process of water-based acrylic emulsion. In the continuous polymerization stage of the emulsion, the process uses the continuously added emulsifier as the core, and prepares the primer through a special double-kettle prepolymerization process. Through the nucleation effect of the primer stabilizing the emulsifier, not only can a small-particle water-based acrylic emulsion be prepared, but also a steady state and equilibrium can be quickly established, realizing continuous production under the double-kettle process, which has great industrial application significance.
[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0007] A continuous preparation process for an aqueous acrylic emulsion comprises the following steps:
[0008] 1) Prepare the first reactor primer
[0009] In parts by mass, 4-11 parts of emulsifier, 250-310 parts of water, and 1-5 parts of initiator are added to the first reaction kettle, and pre-emulsion a is added dropwise at the reaction temperature to initiate polymerization to obtain a primer solution a;
[0010] The pre-emulsion a comprises: 50-90 parts of hard monomer, 70-120 parts of soft monomer, 5-10 parts of emulsifier, and 50-80 parts of water;
[0011] As a preferred embodiment, the hard monomer is styrene and / or methyl methacrylate;
[0012] Preferably, the soft monomer is isooctyl acrylate and / or butyl acrylate;
[0013] Preferably, the emulsifier is one or more of tridecyl alcohol polyoxyethylene ether sulfate sodium salt, sodium dodecyl sulfate, sodium p-styrene sulfonate, and sodium dodecylbenzene sulfonate;
[0014] Preferably, the initiator is ammonium persulfate and / or sodium persulfate.
[0015] 2) Prepare the second reactor primer
[0016] Step 1) and step 2) are based on the same mass parts; 4-12 parts of emulsifier, 260-310 parts of water, 1-5 parts of initiator, and part of pre-emulsion b are added to the second reaction kettle, and after uniform dispersion, the remaining pre-emulsion b is added dropwise at the reaction temperature to initiate polymerization to obtain a primer b;
[0017] The pre-emulsion b comprises: 310-400 parts of hard monomer, 270-360 parts of soft monomer, 12-36 parts of functional monomer, 10-15 parts of emulsifier, and 200-260 parts of water;
[0018] Preferably, the functional monomer is one or more of acrylic acid, methacrylic acid, and vinyl trimethoxysilane. The selection range of the emulsifier, initiator, hard monomer, and soft monomer is the same as above.
[0019] 3) Dual-reactor continuous polymerization
[0020] To the first reactor containing the primer liquid a, monomer liquid I, 40-70 parts of emulsifier I, 1-5 parts of initiator I and 110-180 parts of water are continuously added dropwise by mass, and continuous polymerization is carried out at the reaction temperature; at the same time, the emulsion at the bottom of the reactor is transferred to the second reactor at the total flow rate of the raw materials, and equilibrium is established and continuous operation is carried out;
[0021] Simultaneously, monomer liquid II, 3-10 parts of emulsifier II, and 0.5-2 parts of initiator II are continuously added dropwise to the second reaction kettle containing the primer liquid b, and continuous polymerization is performed at the reaction temperature. At the same time, the emulsion at the bottom of the kettle is transferred to the post-treatment kettle at the total flow rate of the raw materials, and equilibrium is established and continuous operation is performed;
[0022] The monomer solution I comprises: 30-50 parts of hard monomer, 40-80 parts of soft monomer, 3-9 parts of emulsifier, and 20-50 parts of water;
[0023] The monomer liquid II comprises: 90-140 parts of hard monomer, 50-120 parts of soft monomer, and 5-10 parts of functional monomer;
[0024] The selection ranges of the emulsifier, initiator, hard monomer, soft monomer and functional monomer in the two reactors of this step are the same as those mentioned above. However, in order to ensure the stability of the continuous reaction operation, the emulsifier in the pre-emulsion b added to the second reactor preferably contains a certain content of sodium p-styrene sulfonate with a double bond functional group, wherein the content of sodium p-styrene sulfonate can be 30-50% of the total amount of the emulsifier; at the same time, the emulsifier II in the dropwise addition liquid preferably contains a certain content of sodium p-styrene sulfonate with a double bond functional group, wherein the content of sodium p-styrene sulfonate can be more than 5% of the total amount of the emulsifier II;
[0025] 4) Post-processing
[0026] When the emulsion is transferred to the post-treatment kettle, the emulsion is cooled, an oxidant, a reducing agent, a neutralizing agent and other optional auxiliary agents are added simultaneously, and the material is discharged after filtration to obtain a water-based acrylic emulsion.
[0027] As a preferred embodiment, in step 1), the reaction temperature is 80-90°C;
[0028] Preferably, in step 1), the pre-emulsion a is added dropwise for 0.5-1 h.
[0029] As a preferred embodiment, in step 2), the reaction temperature is 80-90°C;
[0030] Preferably, the mass of the pre-emulsion b first added to the second reaction kettle in step 2) accounts for 2-4% of the total mass thereof. Preferably, the dropwise addition time of the remaining pre-emulsion b is 2-3 h.
[0031] As a preferred embodiment, in step 3), the emulsifier I and initiator I added dropwise continuously are preferably prepared into solutions with mass concentrations of 50-70% and 5-50%, respectively.
[0032] Preferably, in step 3), the emulsifier II and initiator II added dropwise continuously are preferably prepared into solutions with mass concentrations of 35-60% and 3-25%, respectively.
[0033] As a preferred embodiment, in step 3), the reaction temperature in the first reactor and the second reactor is 85-90°C;
[0034] Preferably, in step 3), the reaction residence time in the first reactor is 70-90 min, and the reaction residence time in the second reactor is 115-145 min.
[0035] As a preferred embodiment, in step 4), the flow ratio of the oxidant to the emulsion is (0.9-1):100; the oxidant is preferably one or more of tert-butyl hydroperoxide, ammonium persulfate, and sodium persulfate;
[0036] Preferably, in step 4), the flow ratio of the reducing agent to the emulsion is (0.8-1):100; the reducing agent is preferably one or more of sodium bisulfite, ascorbic acid, and sodium pyrosulfite;
[0037] Preferably, in step 4), the neutralizing agent is added in an amount such that the pH of the emulsion after neutralization is 7.5-8.5; the neutralizing agent is preferably one or both of sodium hydroxide and potassium hydroxide.
[0038] In addition, the optional other auxiliary agents may be film-forming aids, defoaming agents, preservatives, etc., wherein the flow ratio of the film-forming aid to the emulsion is (2-3):100; the film-forming aid is preferably Eastman OE-300;
[0039] Preferably, the flow ratio of the defoamer to the emulsion is (0.04-0.1):100; the defoamer is preferably Evonik Degussa Tego-825 and / or Tego-1488;
[0040] Preferably, the flow ratio of the preservative to the emulsion is (0.2-0.5):100; the preservative is preferably an isothiazolinone MIT preservative.
[0041] As a preferred embodiment, in step 4), the post-treatment reactor is a tubular reactor, preferably a plurality of tubular reactors connected in series. Preferably, the temperature in the plurality of tubular reactors can be gradually reduced to 70-75°C, 45-50°C, 35-40°C, etc.
[0042] The invention discloses an application of the water-based acrylic emulsion prepared by the process as described above in architectural coatings.
[0043] The present invention adopts a double-kettle polymerization process, which can not only realize rapid continuous and stable operation and has a significant advantage in device cost, but also produces an emulsion with small particle size and excellent scrub resistance, and can be widely used in the field of architectural coatings. DETAILED DESCRIPTION
[0044] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.
[0045] Unless otherwise specified, the sources of raw materials in the following examples and comparative examples of the present invention were obtained from commercial channels.
[0046] The test methods mainly involved in the specific implementation of the present invention are as follows:
[0047] Particle size: Malvern ZS90 particle size analyzer was used, using polystyrene latex model, water as dispersion medium, and general purpose analysis method.
[0048] Scrub resistance of interior wall paint: Apply two coats of latex paint on the sample with a wire rod of 120 microns and 80 microns, respectively, and then place it under constant temperature of 25℃ for one week. Place the sample in the scrub resistance tester, let the brush hang naturally, add 2ml of scrubbing medium (2.5g / L sodium n-dodecylbenzene sulfonate solution) to the test area of the sample, start the instrument to scrub the coating back and forth, and at the same time add the scrubbing medium at a speed of 0.04ml / s to keep the scrubbing surface moist. When the substrate is exposed in the middle 100mm area of the sample, record the number of times the sample is washed and compare the number of times with the latex paint standard prepared by Rohm and Haas DC-420: when the number of evaluation sample times / the number of standard sample times ≥1, it is recorded as Class A; when the number of evaluation sample times / the number of standard sample times is between 0.9-1, it is recorded as Class B; when the number of evaluation sample times / the number of standard sample times is between 0.8-0.9, it is recorded as Class C; when the number of evaluation sample times / the number of standard sample times ≤0.8, it is recorded as Class D.
[0049] Latex paint contrast ratio test: On a cardboard with half black and half white background, use a 100μm wet film preparation device to evenly apply the tested paint, and maintain it for at least 24 hours in an environment with a temperature of (23±2)℃ and a humidity of 50±5%. Use a reflectometer to measure the reflectivity of at least four positions on the paint film, and calculate the average reflectivity RB (on the blackboard) and RW (on the whiteboard) respectively. Calculate the contrast ratio value: contrast ratio = RB / RW, and take the average value after three tests. Parallel test and comparison of values with the latex paint standard prepared by Rohm and Haas DC-420: When the difference between the contrast ratio value of the evaluation sample and the standard sample value is within ±1%, it is recorded as Class A, when the difference between the contrast ratio value of the evaluation sample and the standard sample value is within ±2%, it is recorded as Class B, and when the difference between the contrast ratio value of the evaluation sample and the standard sample value is within ±3%, it is recorded as Class C.
[0050] Calcium ion stability test: After filtering the emulsion with an 80-mesh filter, add 30 mL of the emulsion to a beaker, then add 6 mL of a 2% CaCl2 solution by mass, stir evenly by hand, and place in a 50 mL stoppered measuring cylinder. After 48 hours, filter the emulsion with a 325-mesh filter. The residue content = the residue content of the sieve residue / (the mass of the emulsion + the mass of CaCl2). If the residue content is ≤1000ppm, it is recorded as Class A; if the residue content is between 1000ppm and 2000ppm, it is recorded as Class B; if the residue content is ≥2000ppm, it is recorded as Class C.
[0051] [Example 1]
[0052] A continuous preparation process for an aqueous acrylic emulsion comprises the following steps:
[0053] 1) Prepare the first reactor primer
[0054] Prepare pre-emulsion a, including: 70g styrene, 92.6g butyl acrylate, 7g sodium dodecylbenzene sulfonate, 60g water;
[0055] Add 280g of deionized water and 7g of sodium dodecyl sulfate to the first reaction kettle with a volume of 3L, and heat to 88°C. Then add 12.5g of sodium persulfate solution (concentration 20%) as an initiator, disperse for 3 minutes, and then drop pre-emulsion a to initiate polymerization. The pre-emulsion is added within 30 minutes to obtain primer a.
[0056] 2) Prepare the second reactor primer
[0057] Prepare pre-emulsion b, including: 340g styrene, 310.6g isooctyl acrylate, 25g acrylic acid, 4g sodium p-styrene sulfonate, 6g sodium dodecylbenzene sulfonate, 230g water;
[0058] Add 8g of sodium dodecyl sulfate and 270g of water to a second reaction kettle with a volume of 5L, and heat to 88°C. Then add 24.3g of pre-emulsion b and 12.5g of sodium persulfate solution (concentration 20%) as an initiator, disperse for 15min, and then drip the remaining pre-emulsion b to initiate polymerization. After 3h, drip all the pre-emulsion b to obtain primer b;
[0059] 3) Dual-reactor continuous polymerization
[0060] Monomer liquid I contains styrene at a flow rate of 46.7 g / h, butyl acrylate at a flow rate of 61.7 g / h, sodium dodecylbenzene sulfonate at a flow rate of 4.7 g / h, and water at a flow rate of 40 g / h;
[0061] Monomer liquid II contains styrene at a flow rate of 124.2 g / h, isooctyl acrylate at a flow rate of 87.9 g / h, acrylic acid at a flow rate of 6.5 g / h, and vinyltrimethoxysilane at a flow rate of 0.87 g / h;
[0062] The pre-emulsion in the first and second reactors was controlled to drip at the same time, and then the monomer liquid I with a total flow rate of 153.1 g / h, 92 g / h of sodium dodecyl sulfate solution (concentration 56.5%, solid mass 52 g), 8.3 g / h of sodium persulfate solution (concentration 20%, solid mass 1.66 g) and 173 g / h of water were dripped into the first reactor, and the emulsion at the bottom of the reactor was transferred to the second reactor at a total flow rate of 426.4 g / h; and the monomer liquid I was added to the second reactor at a total flow rate of 153.1 g / h. The monomer liquid II with a total flow rate of 219.47 g / h, the emulsifier solution with a mass ratio of sodium styrene sulfonate to sodium dodecylbenzene sulfonate of 1:12.6, the total concentration of the emulsifier of 45.5%, and the solid mass of 4.6 g, and the sodium persulfate solution with a concentration of 8.3% and a solid mass of 0.86 g were added dropwise to the reactor, and at the same time, the emulsion at the bottom of the reactor was transferred to the post-treatment reactor with a total flow rate of 666 g / h of raw materials, and a balance was established and continuous operation was carried out;
[0063] 4) Post-processing
[0064] The emulsion is first transferred to tubular reactor I at a total flow rate of 666 g / h, the temperature range in the reactor is controlled to be 70-75°C, and tert-butyl hydroperoxide solution (concentration 15.3%, solid mass 0.95 g) and ascorbic acid solution (concentration 8.3%, solid mass 0.47 g) are added dropwise at a flow rate of 6.2 g / h; the emulsion is transferred to tubular reactor II, the temperature range in the reactor is controlled to be 45-50°C, and sodium hydroxide solution (concentration 5.7%) is added dropwise at a flow rate of 46.5 g / h; the emulsion is transferred to tubular reactor III, the temperature range in the reactor is controlled to be 35-40°C, and OE-300 film-forming aid, Tego825 defoamer, MIT solution (concentration 30%, solid mass 1.86 g) are added dropwise at a flow rate of 14.9 g / h, 0.32 g / h, and 6.2 g / h. After the emulsion is filtered through a filter, it is transferred to a product storage tank.
[0065] [Example 2]
[0066] A continuous preparation process for an aqueous acrylic emulsion comprises the following steps:
[0067] 1) Prepare the first reactor primer
[0068] Prepare pre-emulsion a, including: 90g styrene, 72.6g butyl acrylate, 9g tridecyl alcohol polyoxyethylene ether sulfate sodium salt, 60g water;
[0069] Add 260g of deionized water and 9g of sodium dodecyl sulfate to the first reaction kettle with a volume of 3L, and heat to 88°C. Then add 15g of sodium persulfate solution (concentration 20%) as an initiator, disperse for 3 minutes, and then drop the pre-emulsion a to initiate polymerization. The pre-emulsion a is added within 30 minutes to obtain the primer a.
[0070] 2) Prepare the second reactor primer
[0071] Prepare pre-emulsion b, including: 340g methyl methacrylate, 310.6g butyl acrylate, 15g acrylic acid, 3g sodium p-styrene sulfonate, 7g tridecyl alcohol polyoxyethylene ether sulfate sodium salt, 230g water;
[0072] Add 11g sodium dodecyl sulfate and 280g water to a second reaction kettle with a volume of 5L, and heat to 88°C. Then add 24.3g pre-emulsion b and 7.5g sodium persulfate solution (concentration 20%) as an initiator, disperse for 15min, and then drip the remaining pre-emulsion b to initiate polymerization. After 3h, drip all the pre-emulsion b to obtain primer b;
[0073] 3) Dual-reactor continuous polymerization
[0074] Monomer liquid I contains styrene at a flow rate of 35 g / h, butyl acrylate at a flow rate of 46.3 g / h, sodium dodecylbenzene sulfonate at a flow rate of 3.5 g / h, and water at a flow rate of 30 g / h;
[0075] Monomer liquid II contains methyl methacrylate at a flow rate of 95.2 g / h, butyl acrylate at a flow rate of 67.4 g / h, acrylic acid at a flow rate of 5 g / h, and vinyltrimethoxysilane at a flow rate of 0.83 g / h;
[0076] Control the pre-emulsion in the first reactor and the second reactor to drip at the same time, then drip into the first reactor a monomer liquid I with a total flow rate of 114.8 g / h, a sodium salt solution of tridecyl alcohol polyoxyethylene ether sulfate (concentration 56.5%) of 115 g / h, a sodium persulfate solution (concentration 20%) of 6.3 g / h and water of 111 g / h, and transfer the bottom emulsion to the second reactor at a total raw material flow rate of 347.1 g / h; synchronously drip into the second reactor a monomer liquid II with a total flow rate of 168.43 g / h, an emulsifier solution (the mass ratio of sodium p-styrene sulfonate and sodium salt of tridecyl alcohol polyoxyethylene ether sulfate is 1:12.7, and the total emulsifier concentration is 45.5%), and a sodium persulfate solution of 8 g / h (concentration 8.3%), and transfer the bottom emulsion to the post-treatment reactor at a total raw material flow rate of 530.8 g / h, establish equilibrium and operate continuously;
[0077] 4) Post-processing
[0078] The emulsion was first transferred to tubular reactor I at a total flow rate of 530.8 g / h, the temperature in the reactor was controlled to be 70-75°C, and 4.9 g / h of tert-butyl hydroperoxide solution (concentration 15.3%) and 4.5 g / h of ascorbic acid solution (concentration 8.3%) were added dropwise; the emulsion was transferred to tubular reactor II, the temperature in the reactor was controlled to be 45-50°C, and 38 g / h of potassium hydroxide solution (concentration 5.7%) were added dropwise; the emulsion was transferred to tubular reactor III, the temperature in the reactor was controlled to be 35-40°C, and 11.7 g / h of OE-300 film-forming aid, 0.25 g / h of Tego825 defoamer, and 4.9 g / h of MIT solution (concentration 30%) were added dropwise. After the emulsion was filtered through a filter, it was transferred to a product storage tank.
[0079] [Example 3]
[0080] A continuous preparation process for an aqueous acrylic emulsion comprises the following steps:
[0081] 1) Prepare the first reactor primer
[0082] Prepare pre-emulsion a, including: 70g styrene, 92.6g butyl acrylate, 6g tridecyl alcohol polyoxyethylene ether sulfate sodium salt, 62g water;
[0083] Add 280g of deionized water and 7g of sodium dodecylbenzene sulfonate to the first reaction kettle with a volume of 3L, and heat to 88°C. Then add 12.5g of ammonium persulfate solution (concentration 20%) as an initiator, disperse for 3min, and then drop pre-emulsion a to initiate polymerization. The pre-emulsion is added within 30min to obtain primer a.
[0084] 2) Prepare the second reactor primer
[0085] Prepare pre-emulsion b, including: 310g styrene, 340.6g butyl acrylate, 15g acrylic acid, 6g sodium p-styrene sulfonate, 7g sodium dodecylbenzene sulfonate, 230g water;
[0086] Add 8g of sodium dodecylbenzene sulfonate and 280g of water to a second reaction kettle with a volume of 5L, and heat to 88°C. Then add 24.3g of pre-emulsion b and 12.5g of ammonium persulfate solution (concentration 20%) as an initiator, disperse for 15min, and then drip the remaining pre-emulsion b to initiate polymerization. After 3h, dripping is completed to obtain primer b;
[0087] 3) Dual-reactor continuous polymerization
[0088] Monomer liquid I contains styrene at a flow rate of 40 g / h, isooctyl acrylate at a flow rate of 68.4 g / h, sodium tridecyl alcohol polyoxyethylene ether sulfate at a flow rate of 7 g / h, and water at a flow rate of 40 g / h;
[0089] Monomer liquid II contains styrene at a flow rate of 124.2 g / h, isooctyl acrylate at a flow rate of 87.9 g / h, methacrylic acid at a flow rate of 8 g / h, and vinyltrimethoxysilane at a flow rate of 1 g / h;
[0090] Control the pre-emulsion in the first reactor and the second reactor to drip at the same time, then drip into the first reactor a monomer liquid I with a total flow rate of 155.4 g / h, a sodium dodecyl sulfate solution of 79.6 g / h (concentration 56.5%), a sodium persulfate solution of 8.3 g / h (concentration 20%) and water of 173 g / h, and transfer the bottom emulsion to the second reactor at a total raw material flow rate of 416.3 g / h; synchronously drip into the second reactor a monomer liquid II with a total flow rate of 221.1 g / h, an emulsifier solution of 10.2 g / h (the mass ratio of sodium p-styrene sulfonate to sodium dodecylbenzene sulfonate is 1:12.6, and the total emulsifier concentration is 45.5%), and an ammonium persulfate solution of 10.4 g / h (concentration 8.3%), and transfer the bottom emulsion to the post-treatment reactor at a total raw material flow rate of 657.3 g / h, establish equilibrium and operate continuously;
[0091] 4) Post-processing
[0092] The emulsion was first transferred to tubular reactor I at a total flow rate of 657.3 g / h, the temperature in the reactor was controlled to be 70-75°C, and 6.0 g / h of tert-butyl hydroperoxide solution (concentration 15.3%) and 5.6 g / h of ascorbic acid solution (concentration 8.3%) were added dropwise; the emulsion was transferred to tubular reactor II, the temperature in the reactor was controlled to be 45-50°C, and 45.9 g / h of sodium hydroxide solution (concentration 5.7%) were added dropwise; the emulsion was transferred to tubular reactor III, the temperature in the reactor was controlled to be 35-40°C, and 14.5 g / h of OE-300 film-forming aid, 0.31 g / h of Tego1488 defoamer, and 6.1 g / h of MIT solution (concentration 30%) were added dropwise. After the emulsion was filtered through a filter, it was transferred to a product storage tank.
[0093] [Example 4]
[0094] A continuous preparation process for an aqueous acrylic emulsion comprises the following steps:
[0095] 1) Prepare the first reactor primer
[0096] Prepare pre-emulsion a, including: 55g styrene, 107.6g butyl acrylate, 5.5g sodium lauryl sulfate, 60g water;
[0097] Add 270g of deionized water and 7g of sodium dodecyl sulfate to the first reaction kettle with a volume of 3L, and heat to 88°C. Then add 20g of ammonium persulfate solution (concentration 20%) as an initiator, disperse for 3 minutes, and then drop pre-emulsion a to initiate polymerization. The pre-emulsion is added within 30 minutes to obtain primer a.
[0098] 2) Prepare the second reactor primer
[0099] Prepare pre-emulsion b, including: 370g styrene, 280.6g isooctyl acrylate, 25g methacrylic acid, 6g sodium p-styrene sulfonate, 8g sodium dodecylbenzene sulfonate, 240g water;
[0100] Add 7g of sodium dodecyl sulfate and 270g of water to a second reaction kettle with a volume of 5L, and heat to 88°C. Then add 24.3g of pre-emulsion b and 12.5g of ammonium persulfate solution (concentration 20%) as an initiator, disperse for 15min, and then drip the remaining pre-emulsion b to initiate polymerization. After 3h, dripping is completed to obtain primer b;
[0101] 3) Dual-reactor continuous polymerization
[0102] Monomer liquid I contains methyl methacrylate at a flow rate of 46.7 g / h, butyl acrylate at a flow rate of 61.7 g / h, sodium lauryl sulfate at a flow rate of 4.7 g / h, and water at a flow rate of 40 g / h;
[0103] Monomer liquid II contains methyl methacrylate at a flow rate of 104.2 g / h, butyl acrylate at a flow rate of 107.9 g / h, methacrylic acid at a flow rate of 6.5 g / h, and vinyltrimethoxysilane at a flow rate of 0.87 g / h;
[0104] Control the pre-emulsion in the first reactor and the second reactor to drip at the same time, then drip into the first reactor a monomer liquid I with a total flow rate of 153.1 g / h, a sodium dodecylbenzene sulfonate solution (concentration 56.5%) of 88.5 g / h, an ammonium persulfate solution (concentration 20%) and 173 g / h of water, and transfer the bottom emulsion to the second reactor at a total raw material flow rate of 422.9 g / h; synchronously drip into the second reactor a monomer liquid II with a total flow rate of 219.5 g / h, an emulsifier solution (the mass ratio of sodium styrene sulfonate to sodium dodecyl sulfate is 1:11.8, and the total emulsifier concentration is 42.0%), and an ammonium persulfate solution (concentration 8.3%) of 12.0 g / h, and transfer the bottom emulsion to the post-treatment reactor at a total raw material flow rate of 663.9 g / h, establish equilibrium and operate continuously;
[0105] 4) Post-processing
[0106] The emulsion was first transferred to tubular reactor I at a total flow rate of 663.9 g / h, the temperature in the reactor was controlled at 70-75°C, and 6.1 g / h of tert-butyl hydroperoxide solution (concentration 15.3%) and 5.6 g / h of sodium bisulfite solution (concentration 8.3%) were added dropwise; the emulsion was transferred to tubular reactor II, the temperature in the reactor was controlled at 45-50°C, and 46.1 g / h of sodium hydroxide solution (concentration 5.7%) were added dropwise; the emulsion was transferred to tubular reactor III, the temperature in the reactor was controlled at 35-40°C, and 14.6 g / h of OE-300 film-forming aid, 0.31 g / h of Tego1488 defoamer, and 6.1 g / h of MIT solution (concentration 30%) were added dropwise. After the emulsion was filtered through a filter, it was transferred to a product storage tank.
[0107] [Example 5]
[0108] A continuous preparation process for an aqueous acrylic emulsion comprises the following steps:
[0109] 1) Prepare the first reactor primer
[0110] Prepare pre-emulsion a, including: 90g methyl methacrylate, 72.6g butyl acrylate, 8g tridecyl alcohol polyoxyethylene ether sulfate sodium salt, 50g water;
[0111] Add 250g of deionized water and 7g of sodium dodecyl sulfate to the first reaction kettle with a volume of 3L, and heat to 88°C. Then add 12.5g of ammonium persulfate solution (concentration 20%) as an initiator, disperse for 3min, and then drop pre-emulsion a to initiate polymerization. The pre-emulsion is added within 30min to obtain primer a.
[0112] 2) Prepare the second reactor primer
[0113] Prepare pre-emulsion b, including: 340g methyl methacrylate, 310.6g isooctyl acrylate, 30g acrylic acid, 3g sodium p-styrene sulfonate, 7g tridecyl alcohol polyoxyethylene ether sulfate sodium salt, 220g water;
[0114] Add 6g of sodium dodecyl sulfate and 280g of water to a second reaction kettle with a volume of 5L, and heat to 88°C. Then add 24.3g of pre-emulsion b and 7.5g of sodium persulfate solution (concentration 20%) as an initiator, disperse for 15 minutes, and then drip the remaining pre-emulsion b to initiate polymerization. After 3 hours, drip all the pre-emulsion b to obtain a primer b.
[0115] 3) Dual-reactor continuous polymerization
[0116] Monomer liquid I contains methyl methacrylate at a flow rate of 40 g / h, isooctyl acrylate at a flow rate of 41.3 g / h, sodium lauryl sulfate at a flow rate of 5 g / h, and water at a flow rate of 32 g / h;
[0117] Monomer liquid II contains methyl methacrylate at a flow rate of 95.2 g / h, isooctyl acrylate at a flow rate of 67.4 g / h, acrylic acid at a flow rate of 5 g / h, and vinyltrimethoxysilane at a flow rate of 0.83 g / h;
[0118] Control the pre-emulsion in the first reactor and the second reactor to drip at the same time, then drip into the first reactor a monomer liquid I with a total flow rate of 118.3 g / h, a sodium dodecyl sulfate solution of 115 g / h (concentration 56.5%), an ammonium persulfate solution of 9.5 g / h (concentration 40%) and water of 111 g / h, and transfer the bottom emulsion to the second reactor at a total raw material flow rate of 353.8 g / h; synchronously drip into the second reactor a monomer liquid II with a total flow rate of 168.43 g / h, an emulsifier solution of 8.6 g / h (the mass ratio of sodium p-styrene sulfonate and sodium tridecyl alcohol polyoxyethylene ether sulfate is 1:14.3, and the total emulsifier concentration is 50%), and an ammonium persulfate solution of 8 g / h (concentration 8.3%), and transfer the bottom emulsion to the post-treatment reactor at a total raw material flow rate of 530.2 g / h, establish equilibrium and operate continuously;
[0119] 4) Post-processing
[0120] The emulsion was first transferred to tubular reactor I at a total flow rate of 530.2 g / h, the temperature in the reactor was controlled to be 70-75°C, and 4.9 g / h of tert-butyl hydroperoxide solution (concentration 15.3%) and 4.5 g / h of sodium pyrosulfite solution (concentration 8.3%) were added dropwise; the emulsion was transferred to tubular reactor II, the temperature in the reactor was controlled to be 45-50°C, and 38 g / h of potassium hydroxide solution (concentration 5.7%) were added dropwise; the emulsion was transferred to tubular reactor III, the temperature in the reactor was controlled to be 35-40°C, and 11.7 g / h of OE-300 film-forming aid, 0.25 g / h of Tego825 defoamer, and 4.9 g / h of MIT solution (concentration 30%) were added dropwise. After the emulsion was filtered through a filter, it was transferred to a product storage tank.
[0121] [Comparative Example 1]
[0122] A continuous preparation process for an aqueous acrylic emulsion comprises the following steps:
[0123] 1) Prepare the first reactor primer
[0124] Prepare pre-emulsion a, including: 70g styrene, 92.6g butyl acrylate, 7g sodium dodecylbenzene sulfonate, 60g water;
[0125] Add 280g of deionized water and 7g of sodium dodecyl sulfate to the first reaction kettle with a volume of 3L, and heat to 88°C. Then add 12.5g of sodium persulfate solution (concentration 20%) as an initiator, disperse for 3 minutes, and then drop pre-emulsion a to initiate polymerization. The pre-emulsion is added within 30 minutes to obtain primer a.
[0126] 2) Prepare the second reactor primer
[0127] Prepare pre-emulsion b, including: 340g styrene, 310.6g isooctyl acrylate, 25g acrylic acid, 4g sodium p-styrene sulfonate, 6g sodium dodecylbenzene sulfonate, 230g water;
[0128] Add 8g of sodium dodecyl sulfate and 270g of water to a second reaction kettle with a volume of 5L, and heat to 88°C. Then add 24.3g of pre-emulsion b and 12.5g of sodium persulfate solution (concentration 20%) as an initiator, disperse for 15min, and then drip the remaining pre-emulsion b to initiate polymerization. After 3h, drip all the pre-emulsion b to obtain primer b;
[0129] 3) Dual-reactor continuous polymerization
[0130] Monomer liquid I contains styrene at a flow rate of 46.7 g / h, butyl acrylate at a flow rate of 61.7 g / h, sodium dodecylbenzene sulfonate at a flow rate of 4.7 g / h, and water at a flow rate of 40 g / h;
[0131] Monomer liquid II contains styrene at a flow rate of 124.2 g / h, isooctyl acrylate at a flow rate of 87.9 g / h, acrylic acid at a flow rate of 6.5 g / h, and vinyltrimethoxysilane at a flow rate of 0.87 g / h;
[0132] The pre-emulsion in the first and second reactors was controlled to drip at the same time, and then 153.1 g / h of monomer solution I and 92 g / h of finished seed emulsion Archsol were added to the first reactor. 8087 (Wanhua Chemical, particle size 50nm), 8.3g / h of sodium persulfate solution (concentration 20%, solid mass 1.66g) and 123g / h of water, and at the same time, the bottom emulsion is transferred to the second reactor at a total raw material flow rate of 376.4g / h; synchronously, a total flow rate of 219.47g / h of monomer liquid II, 9.5g / h of emulsifier solution (the mass ratio of sodium p-styrene sulfonate and sodium dodecylbenzene sulfonate is 1:12.6, the total emulsifier concentration is 45.5%, the solid mass is 4.3g), and 10.4g / h of sodium persulfate solution (concentration 8.3%, solid mass 0.86g) are added dropwise to the second reactor, and at the same time, the bottom emulsion is transferred to the post-treatment reactor at a total raw material flow rate of 615.8g / h, and equilibrium is established and continuous operation is carried out;
[0133] 4) Post-processing
[0134] The emulsion was first transferred to tubular reactor I at a total flow rate of 615.8 g / h, the temperature range in the reactor was controlled to be 70-75°C, and 5.7 g / h of tert-butyl hydroperoxide solution (concentration 15.3%, solid mass 0.87 g) and 5.2 g / h of ascorbic acid solution (concentration 8.3%, solid mass 0.43 g) were added dropwise; the emulsion was transferred to tubular reactor II, the temperature range in the reactor was controlled to be 45-50°C, and 44 g / h of sodium hydroxide solution (concentration 5.7%) were added dropwise; the emulsion was transferred to tubular reactor III, the temperature range in the reactor was controlled to be 35-40°C, and 13.5 g / h of OE-300 film-forming aid, 0.29 g / h of Tego825 defoamer, and 5.7 g / h of MIT solution (concentration 30%, solid mass 1.71 g) were added dropwise. After the emulsion was filtered through a filter, it was transferred to a product storage tank.
[0135] [Comparative Example 2]
[0136] 1) Prepare the first reactor primer
[0137] Add 522 g of deionized water and 7 g of sodium dodecyl sulfate into the first reaction kettle with a volume of 3 L, and heat to 88° C. to obtain a primer solution a;
[0138] 2) Prepare the second reactor primer
[0139] Add 1198 g of deionized water and 8 g of sodium dodecyl sulfate to a second reaction kettle with a volume of 5 L, and heat to 88° C. to obtain a primer solution b;
[0140] 3) Dual-reactor continuous polymerization
[0141] Monomer liquid I contains styrene at a flow rate of 46.7 g / h, butyl acrylate at a flow rate of 61.7 g / h, sodium dodecylbenzene sulfonate at a flow rate of 4.7 g / h, and water at a flow rate of 40 g / h;
[0142] Monomer liquid II contains styrene at a flow rate of 124.2 g / h, isooctyl acrylate at a flow rate of 87.9 g / h, acrylic acid at a flow rate of 6.5 g / h, and vinyltrimethoxysilane at a flow rate of 0.87 g / h;
[0143] Control the pre-emulsion in the first reactor and the second reactor to drip at the same time, then drip into the first reactor a monomer liquid I with a total flow rate of 153.1 g / h, a sodium dodecyl sulfate solution of 92 g / h (concentration 56.5%), a sodium persulfate solution of 8.3 g / h (concentration 20%) and water of 173 g / h, and transfer the bottom emulsion to the second reactor at a total raw material flow rate of 426.4 g / h; synchronously drip into the second reactor a monomer liquid II with a total flow rate of 219.47 g / h, an emulsifier solution of 9.5 g / h (the mass ratio of sodium styrene sulfonate to sodium dodecylbenzene sulfonate is 1:12.6, and the total emulsifier concentration is 45.5%), and a sodium persulfate solution of 10.4 g / h (concentration 8.3%), and transfer the bottom emulsion to the post-treatment reactor at a total raw material flow rate of 666 g / h, establish equilibrium and operate continuously;
[0144] 4) Post-processing
[0145] The emulsion was first transferred to tubular reactor I at a total flow rate of 666 g / h, the temperature in the reactor was controlled to be 70-75°C, and 6.2 g / h of tert-butyl hydroperoxide solution (concentration 15.3%) and 5.7 g / h of ascorbic acid solution (concentration 8.3%) were added dropwise; the emulsion was transferred to tubular reactor II, the temperature in the reactor was controlled to be 45-50°C, and 46.5 g / h of sodium hydroxide solution (concentration 5.7%) were added dropwise; the emulsion was transferred to tubular reactor III, the temperature in the reactor was controlled to be 35-40°C, and 14.9 g / h of OE-300 film-forming aid, 0.32 g / h of Tego825 defoamer, and 6.2 g / h of MIT solution (concentration 30%) were added dropwise. After the emulsion was filtered through a filter, it was transferred to a product storage tank.
[0146] [Comparative Example 3]
[0147] 1) Prepare the first reactor primer
[0148] Prepare pre-emulsion a, including: 70g styrene, 92.6g butyl acrylate, 7g sodium dodecylbenzene sulfonate, 60g water;
[0149] Add 280g of deionized water and 7g of sodium dodecyl sulfate to the first reaction kettle with a volume of 3L, and heat to 88°C. Then add 12.5g of sodium persulfate solution (concentration 20%) as an initiator, disperse for 3 minutes, and then drop pre-emulsion a to initiate polymerization. The pre-emulsion is added within 30 minutes to obtain primer a.
[0150] 2) Prepare the second reactor primer
[0151] Add 1198 g of deionized water and 8 g of sodium dodecyl sulfate to a second reaction kettle with a volume of 5 L, and heat to 88° C. to obtain a primer solution b;
[0152] 3) Dual-reactor continuous polymerization
[0153] Monomer liquid I contains styrene at a flow rate of 46.7 g / h, butyl acrylate at a flow rate of 61.7 g / h, sodium dodecylbenzene sulfonate at a flow rate of 4.7 g / h, and water at a flow rate of 40 g / h;
[0154] Monomer liquid II contains styrene at a flow rate of 124.2 g / h, isooctyl acrylate at a flow rate of 87.9 g / h, acrylic acid at a flow rate of 6.5 g / h, and vinyltrimethoxysilane at a flow rate of 0.87 g / h;
[0155] Control the pre-emulsion in the first reactor and the second reactor to drip at the same time, then drip into the first reactor a monomer liquid I with a total flow rate of 153.1 g / h, a sodium dodecyl sulfate solution of 92 g / h (concentration 56.5%), a sodium persulfate solution of 8.3 g / h (concentration 20%) and water of 173 g / h, and transfer the bottom emulsion to the second reactor at a total raw material flow rate of 426.4 g / h; synchronously drip into the second reactor a monomer liquid II with a total flow rate of 219.47 g / h, an emulsifier solution of 9.5 g / h (the mass ratio of sodium styrene sulfonate to sodium dodecylbenzene sulfonate is 1:12.6, and the total emulsifier concentration is 45.5%), and a sodium persulfate solution of 10.4 g / h (concentration 8.3%), and transfer the bottom emulsion to the post-treatment reactor at a total raw material flow rate of 666 g / h, establish equilibrium and operate continuously;
[0156] 4) Post-processing
[0157] The emulsion was first transferred to tubular reactor I at a total flow rate of 666 g / h, the temperature in the reactor was controlled to be 70-75°C, and 6.2 g / h of tert-butyl hydroperoxide solution (concentration 15.3%) and 5.7 g / h of ascorbic acid solution (concentration 8.3%) were added dropwise; the emulsion was transferred to tubular reactor II, the temperature in the reactor was controlled to be 45-50°C, and 46.5 g / h of sodium hydroxide solution (concentration 5.7%) were added dropwise; the emulsion was transferred to tubular reactor III, the temperature in the reactor was controlled to be 35-40°C, and 14.9 g / h of OE-300 film-forming aid, 0.32 g / h of Tego825 defoamer, and 6.2 g / h of MIT solution (concentration 30%) were added dropwise. After the emulsion was filtered through a filter, it was transferred to a product storage tank.
[0158] During the 30-hour operation of the preparation process in each embodiment and comparative example, the particle size of the aqueous acrylic emulsion obtained in each time period was sampled and analyzed, so as to monitor the period when the system reaches a steady state, and the results are shown in Table 1. In addition, the aqueous acrylic emulsion obtained after the preparation process in each embodiment and comparative example was stably operated for 30 hours was used to prepare interior wall coatings according to the formula in Table 2, and the coating properties were tested, and the results are shown in Table 3.
[0159] Table 1. Particle size of water-based acrylic emulsion
[0160] Particle size nm 1h 3h 6h 9h 12h 15h 18h 21h 24h 30h Example 1 108 116 122 122 123 122 123 121 120 121 Example 2 102 114 120 121 122 120 120 121 120 121 Example 3 107 116 122 123 123 122 123 120 121 119 Example 4 104 113 120 123 123 122 123 121 120 121 Example 5 104 114 120 121 122 120 120 122 123 123 Comparative Example 1 89 118 132 155 180 189 201 205 206 205 Comparative Example 2 95 101 107 112 118 122 127 132 137 142 Comparative Example 3 112 122 131 141 150 156 160 165 169 172
[0161] Table 2, interior wall paint latex paint formula
[0162]
[0163]
[0164] Table 3. Performance test results
[0165] Scrub resistance Contrast ratio Calcium ion stability Example 1 A A A Example 2 A A A Example 3 A A A Example 4 A A A Example 5 A A A Comparative Example 1 C A A Comparative Example 2 C B A Comparative Example 3 B B A
[0166] It can be seen from the data in Table 1 that the sample prepared by the embodiment of this patent can quickly establish equilibrium in 3-6 hours, and the prepared emulsion has a small particle size and excellent scrub resistance.
[0167] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.
Claims
1. A continuous preparation process for an aqueous acrylic emulsion, characterized in that: The following steps are involved: 1) Prepare the first reactor primer In parts by mass, 4-11 parts of emulsifier, 250-310 parts of water, and 1-5 parts of initiator are added to the first reaction kettle, and pre-emulsion a is added dropwise at the reaction temperature to initiate polymerization to obtain a primer solution a; The pre-emulsion a comprises: 50-90 parts of hard monomer, 70-120 parts of soft monomer, 5-10 parts of emulsifier, and 50-80 parts of water; 2) Prepare the second reactor primer Step 1) and step 2) are based on the same mass parts; 4-12 parts of emulsifier, 260-310 parts of water, 1-5 parts of initiator, and part of pre-emulsion b are added to the second reaction kettle, and after uniform dispersion, the remaining pre-emulsion b is added dropwise at the reaction temperature to initiate polymerization to obtain a primer b; The pre-emulsion b comprises: 310-400 parts of hard monomer, 270-360 parts of soft monomer, 12-36 parts of functional monomer, 10-15 parts of emulsifier, and 200-260 parts of water; 3) Dual-reactor continuous polymerization To the first reactor containing the primer liquid a, monomer liquid I, 40-70 parts of emulsifier I, 1-5 parts of initiator I and 110-180 parts of water are continuously added dropwise by mass, and continuous polymerization is carried out at the reaction temperature; at the same time, the emulsion at the bottom of the reactor is transferred to the second reactor at the total flow rate of the raw materials, and equilibrium is established and continuous operation is carried out; Simultaneously, monomer liquid II, 3-10 parts of emulsifier II, and 0.5-2 parts of initiator II are continuously added dropwise to the second reaction kettle containing the primer liquid b, and continuous polymerization is performed at the reaction temperature. At the same time, the emulsion at the bottom of the kettle is transferred to the post-treatment kettle at the total flow rate of the raw materials, and equilibrium is established and continuous operation is performed; The monomer solution I comprises: 30-50 parts of hard monomer, 40-80 parts of soft monomer, 3-9 parts of emulsifier, and 20-50 parts of water; The monomer liquid II comprises: 90-140 parts of hard monomer, 50-120 parts of soft monomer, and 5-10 parts of functional monomer; 4) Post-processing When the emulsion is transferred to the post-treatment kettle, the emulsion is cooled, an oxidant, a reducing agent, a neutralizing agent and other optional auxiliary agents are added simultaneously, and the material is discharged after filtration to obtain a water-based acrylic emulsion.
2. The continuous preparation process of aqueous acrylic emulsion according to claim 1, characterized in that: In step 1), the reaction temperature is 80-90°C.
3. The continuous preparation process of the aqueous acrylic emulsion according to claim 2, characterized in that: In step 1), the pre-emulsion a is added dropwise for 0.5-1 h.
4. The continuous preparation process of aqueous acrylic emulsion according to claim 1, characterized in that: In step 2), the reaction temperature is 80-90°C.
5. The continuous preparation process of the aqueous acrylic emulsion according to claim 4, characterized in that: The mass of the pre-emulsion b first added to the second reaction kettle in step 2) accounts for 2-4% of its total mass.
6. The continuous preparation process of the aqueous acrylic emulsion according to claim 4, characterized in that: The remaining pre-emulsion b in step 2) is added dropwise for 2-3 hours.
7. The continuous preparation process of the aqueous acrylic emulsion according to any one of claims 1 to 6, characterized in that: In step 3), the reaction temperature in the first reactor and the second reactor is 80-90°C.
8. The continuous preparation process of aqueous acrylic emulsion according to claim 7, characterized in that: In step 3), the reaction residence time in the first reactor is 70-90 min, and the reaction residence time in the second reactor is 115-145 min.
9. The continuous preparation process of the aqueous acrylic emulsion according to any one of claims 1 to 6, characterized in that: In step 4), the flow ratio of the oxidant to the emulsion is (0.9-1):
100.
10. The continuous preparation process of water-based acrylic emulsion according to claim 9, characterized in that: The oxidant is one or more of tert-butyl hydroperoxide, ammonium persulfate, and sodium persulfate.
11. The continuous preparation process of water-based acrylic emulsion according to claim 9, characterized in that: In step 4), the flow ratio of the reducing agent to the emulsion is (0.8-1):
100.
12. The continuous preparation process of water-based acrylic emulsion according to claim 11, characterized in that: The reducing agent is one or more of sodium bisulfite, ascorbic acid, and sodium pyrosulfite.
13. The continuous preparation process of water-based acrylic emulsion according to claim 9, characterized in that: Step 4), the neutralizing agent is added in an amount such that the pH of the emulsion after neutralization is 7.5-8.
5.
14. The continuous preparation process of water-based acrylic emulsion according to claim 13, characterized in that: The neutralizing agent is one or both of sodium hydroxide and potassium hydroxide.
15. The continuous preparation process of water-based acrylic emulsion according to claim 9, characterized in that: In step 4), the post-treatment reactor is a tubular reactor.
16. The continuous preparation process of water-based acrylic emulsion according to claim 15, characterized in that: In step 4), the post-treatment reactor is a plurality of tubular reactors connected in series.
17. The continuous preparation process of the aqueous acrylic emulsion according to any one of claims 1 to 6, characterized in that: The hard monomer is styrene and / or methyl methacrylate.
18. The continuous preparation process of water-based acrylic emulsion according to claim 17, characterized in that: The soft monomer is isooctyl acrylate and / or butyl acrylate.
19. The continuous preparation process of water-based acrylic emulsion according to claim 17, characterized in that: The functional monomer is one or more of acrylic acid, methacrylic acid and vinyltrimethoxysilane.
20. The continuous preparation process of aqueous acrylic emulsion according to claim 17, characterized in that: The emulsifier is one or more of tridecyl alcohol polyoxyethylene ether sulfate sodium salt, sodium dodecyl sulfate, sodium p-styrene sulfonate, and sodium dodecylbenzene sulfonate.
21. The continuous preparation process of aqueous acrylic emulsion according to claim 20, characterized in that: The initiator is ammonium persulfate and / or sodium persulfate.
22. Use of the aqueous acrylic emulsion prepared by the process according to any one of claims 1 to 21 in architectural coatings.
Citation Information
Patent Citations
Continuous production process and system of water-based acrylic resin emulsion
CN114163563A
Preparation method of acrylate copolymerization emulsion for high-adhesion heavy anti-corrosion coating
CN105218725A
Preparation method of acrylate emulsion for novel wood lacquer coating
CN110669181A
Process for Continuous Emulsion Polymerization
US20130102702A1